Method for extracting rare earth from ardealite
Through the dissolution and high-temperature oxidation methods of Aspergillus niger mycelia and culture medium, rare earth elements are efficiently recovered from phosphogypsum, solving the problems of high cost of inorganic acid leaching and inapplicability of traditional microorganisms, and achieving efficient and environmentally friendly rare earths Resource utilization.
Patent Information
- Application Number
- CN202411154044.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-19
AI Technical Summary
In the prior art, when recovering rare earth elements from phosphogypsum, the use of inorganic acid leaching method is high and not environmentally friendly, and traditional biometallurgical microorganisms are not suitable for leaching rare earths in phosphogypsum, resulting in low efficiency of rare earth resource utilization.
Aspergillus niger mycelia and culture medium were used to dissolve rare earth elements in phosphogypsum, and rare earth oxides were recovered through high-temperature oxidation to achieve efficient extraction and enrichment of rare earths.
The rare earth extraction rate has reached 81.1%, reducing the harmless treatment cost in phosphogypsum, improving resource utilization efficiency, and reducing the free fluorine ion content, and is suitable for by-product phosphogypsum enterprises.
Smart Images

Figure CN118979163A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for extracting metal elements by means of microorganisms, and further to a method for extracting rare earth elements from phosphogypsum. Background Art
[0002] Rare earth elements exist mainly in the form of minerals in the earth's crust, and a considerable part of them coexist in apatite and phosphorite. The total reserves of phosphate ore in the world are about 100 billion tons, and the rare earth associated with phosphate ore is about 46 million tons, with an average rare earth content of 0.046%. 90% of the world's phosphoric acid is produced by wet process. Every 1 ton of phosphoric acid (in terms of P2O5) produced will produce about 5 tons of phosphogypsum. The most common dihydrate phosphoric acid process causes 70% to 80% of the rare earth elements in phosphate ore to migrate into phosphogypsum, while hemihydrate phosphoric acid causes 95% of the rare earth elements to migrate into phosphogypsum. It is estimated that 250 million tons of phosphate ore are used for phosphoric acid production worldwide each year. If the average rare earth element content in phosphate ore is 0.046%, about 100,000 tons of rare earth elements will eventually enter phosphogypsum. At present, the annual global production of rare earth oxides is only 126,000 tons. The amount of rare earth elements lost from phosphogypsum is huge, so recovering rare earths from phosphogypsum will be a potential solution to the dwindling rare earth resources.
[0003] Recent studies have shown that most of the rare earth elements in phosphogypsum may be rare earth phosphates adsorbed on the gypsum surface as a second phase. This surface binding indicates that rare earth elements should be relatively easy to extract by aqueous chemical reagents compared to the case where rare earth elements are bound to the crystal lattice. At present, the recovery of rare earths from phosphogypsum is mostly studied by leaching phosphogypsum with inorganic acids and filtering to obtain rare earth solutions, and then using concentration, crystallization or chemical precipitation to obtain rare earth concentrates. There are also organic solvents that extract rare earth solutions to separate rare earths. The rare earth extraction rate can reach more than 68.5%. However, the use of inorganic acid leaching has high costs for the subsequent harmless treatment of phosphogypsum, which is not economically viable.
[0004] Biometallurgy has become a hot topic in recent years due to its low cost and eco-friendly environment. At present, biometallurgy technology has been widely used in extracting metals from low-grade and difficult-to-process ores, including copper, gold, nickel, zinc, cobalt, uranium, etc. The copper, gold and uranium produced by biometallurgy account for 15%, 25% and 13% of the world's total production respectively, so it has broad prospects.
[0005] Since there is no sulfide component in phosphogypsum, the traditional thiobacillus microorganisms used in biometallurgy of copper, gold, zinc and other metals are not suitable for leaching rare earths in phosphogypsum. However, Aspergillus niger has gradually attracted attention because of its wide source, good adsorption capacity for rare earth elements, and can be cultivated with biomass such as corn stalks, potato peels, and discarded fruits. Aspergillus niger is widely distributed in grains, plant products and soils around the world. It is an important fermentation industry strain with an optimal growth temperature of 37°C and a minimum relative humidity of 88%. It can cause mildew in grains with high moisture content and other industrial equipment. Due to its fast growth and reproduction, short fermentation time, and no toxic and harmful substances, it is listed as one of the main production bacteria by the US Food and Drug Administration and used in food industry enzymes. According to different culture conditions, Aspergillus niger can produce citric acid and different types of enzymes, dissolve minerals, and utilize the useful elements in them through acidolysis and chelation.
[0006] There are not many patent applications related to the extraction of rare earths from phosphogypsum in the Chinese patent database, such as CN200710053196.0 "Method for Extracting Rare Earths from Phosphogypsum", 200810068762.X "A Method for Recovering Rare Earths from Phosphogypsum", CN201910831672.X "A Method for Leaching Rare Earth-Containing Phosphogypsum to Recover Rare Earths", etc. However, there are no patent applications for the use of Aspergillus niger culture solution and phosphogypsum liquid-solid mixing, which cannot better realize the resource utilization of phosphogypsum. Summary of the invention
[0007] The present invention aims to provide a method for extracting rare earth elements from phosphogypsum by means of microorganisms, so as to overcome the deficiencies of the prior art and achieve effective recovery of rare earth elements from phosphogypsum.
[0008] The inventor provides a method for extracting rare earth from phosphogypsum, which utilizes organic acids such as citric acid and gluconic acid produced by Aspergillus niger in the metabolic process and unique biological effects to dissolve rare earth elements precipitated and adsorbed in phosphogypsum into leaching solution, and then enriches them in Aspergillus niger mycelium balls through biological metabolism, and recovers rare earth by separating and high-temperature oxidizing Aspergillus niger mycelium balls containing rare earth. The specific method includes the following steps: (1) Phosphogypsum crushing Crushing the phosphogypsum until it passes through a 10-mesh sieve to obtain phosphogypsum powder; (2) Preparation of extraction solution Using the pre-purified Aspergillus niger as the basis, 20% potato juice and 20g / L glucose as the main nutrients to supply Aspergillus niger growth and culture, the main metabolites of the Aspergillus niger culture fluid obtained are citric acid, gluconic acid, oxalic acid, tartaric acid, ketoglutaric acid, etc. The diameter of the Aspergillus niger mycelium balls in the Aspergillus niger culture fluid is controlled to be 0.2mm~10mm. The cultured Aspergillus niger culture fluid is transferred to the leaching tank, and 0.1%~5% potato juice and 1~4g / L glucose are added to obtain the extract used for leaching, which is called the leaching fluid; (3) Extraction of rare earths from phosphogypsum Add phosphogypsum powder to the leaching tank, stir or bubble it to make the leaching solution, mycelium balls and phosphogypsum powder fully mixed, and regularly measure the pH value of the leaching solution and the rare earth content in the phosphogypsum; stop leaching when more than 76% of the rare earth in the phosphogypsum is transferred to the mycelium balls and the leaching solution; filter and separate the mycelium balls with a 20-mesh screen, and then filter and separate the phosphogypsum and the leaching solution with a 300-mesh filter cloth, and return the mycelium balls, filtrate and filter residue washing water to the leaching tank, and then add phosphogypsum powder, 0.1% to 5% potato juice, 1 to 4g / L glucose, and repeat the leaching for 48 hours; if the total rare earth content of the leaching solution is ≥100ppm, stop leaching, filter and separate the mycelium balls, and the mycelium balls are mycelium balls enriched with rare earth elements at this time; the filtrate and filter residue washing water are returned to be used for culturing Aspergillus niger culture medium; (4) Recovery of rare earths from mycelium pellets The mycelium balls enriched with rare earth elements collected in the previous step are dried with hot air and then oxidized into ashes at high temperature to obtain rare earth oxides.
[0009] In step (2) of the above method, the concentration of citric acid in the Aspergillus niger culture solution used to prepare the leaching solution is ≥10 mmol / L; and the nutrient composition is 20% potato juice and 20 g / L glucose.
[0010] In step (3) of the above method, the leaching tank is a container or other device that can contain the leaching solution and phosphogypsum and can achieve stirring or bubbling; the leaching tank adopts appropriate heating and heat preservation measures to keep the temperature of the leaching solution in the range of 29°C±9°C. The mass ratio of the leaching solution to the phosphogypsum is 0.4:1 to 40:1.
[0011] In step (4) of the above method, the high temperature oxidation process is burning or decomposition at a temperature above 400° C. in air or oxygen atmosphere.
[0012] Compared with the prior art, the method of the present invention uses Aspergillus niger mycelium pellets and culture fluid to extract rare earth elements from phosphogypsum, which is more economical and environmentally friendly than using inorganic acid to extract rare earths from phosphogypsum. The phosphogypsum after leaching has lower inorganic acid and free fluoride ion contents, which is more conducive to the resource utilization of phosphogypsum. It is suitable for enterprises with by-product phosphogypsum. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 The process flow chart of the method of the present invention is shown in FIG. DETAILED DESCRIPTION
[0014] Example: 1 t of phosphogypsum (total rare earth content of 0.051% (TRE2O3), pH 3.2 (mix 20 g of phosphogypsum with 20 g of water and let stand, measure the pH of the supernatant), free F - The concentration of citric acid in the mixture was 0.20%, and it was crushed and passed through a 30-mesh sieve; 1t of Aspergillus niger culture solution (wherein the concentration of citric acid was 55 mmol / L), 10kg of potato juice and 2kg of glucose were added to the leaching tank and mixed evenly; then the phosphogypsum powder was added to the leaching tank and stirred and mixed at a rate of 50r / min.
[0015] After that, samples were taken regularly every day to determine the total rare earth content in the leaching solution and phosphogypsum, and the evaporation of the leaching solution was observed and pure water was added. The pH of the leaching solution was monitored and controlled between 3.1 and 3.9, the dissolved oxygen content was between 7 mg / L and 9 mg / L, and the leaching solution temperature was between 25°C and 28°C. After 2 days of continuous stirring and leaching, it was determined that 85% of the rare earth in the phosphogypsum was transferred to the mycelium balls and the leaching solution. At this time, the total rare earth content in the leaching solution was 51ppm, and the leaching was stopped; 0.9t of leaching solution and mycelium balls were collected and collected, and the phosphogypsum filter cake was rinsed with 0.1t of pure water and returned to the leaching tank; then 10kg of potato juice and 2kg of glucose were added to the leaching tank. After mixing, 1t of phosphogypsum powder was added to continue leaching. Repeat the above operation until the total rare earth content in the leaching solution is 110ppm. A total of 10t of phosphogypsum is leached. The total rare earth content in the oxide ash of the rare earth-enriched mycelium balls after burning is 4136.1g (TRE2O3), and the total rare earth leaching rate reaches 81.1%. The pH of the phosphogypsum after leaching is 4.2 (take 20g of phosphogypsum and mix it with 20g of water, let it stand, and measure the pH of the supernatant); free F - The content was 0.12%, a decrease of 40.0%. The filtrate and the residue washing liquid were returned to inoculate the Aspergillus niger culture liquid.
Claims
1. A method for extracting rare earth from phosphogypsum, characterized in that It utilizes organic acids such as citric acid and gluconic acid produced by the Aspergillus niger culture solution in the metabolic process and unique biological effects to dissolve the rare earths precipitated and adsorbed in the phosphogypsum into the leaching solution, and then enriches the rare earths in the Aspergillus niger mycelium balls through biological metabolism. The rare earths are recovered by separating and oxidizing the Aspergillus niger mycelium balls containing rare earths at high temperature. The specific method includes the following steps: (1) Phosphogypsum crushing Crushing the phosphogypsum until it passes through a 10-mesh sieve to obtain phosphogypsum powder; (2) Extraction solution preparation Using the pre-purified Aspergillus niger as the basis, 20% potato juice and 20g / L glucose as the main nutrients to supply Aspergillus niger growth and culture, the main metabolites of the Aspergillus niger culture fluid obtained are citric acid, gluconic acid, oxalic acid, tartaric acid, ketoglutaric acid, etc. The diameter of the Aspergillus niger mycelium balls in the Aspergillus niger culture fluid is controlled to be 0.2mm~10mm; the cultured Aspergillus niger culture fluid is transferred to the leaching tank, and 0.1%~5% potato juice and 1~4g / L glucose are added, which is the extract used for leaching, called the leaching fluid; (3) Extraction of rare earths from phosphogypsum Add phosphogypsum powder to the leaching tank, stir or bubble it to make the leaching solution, mycelium balls and phosphogypsum powder fully mixed, and regularly measure the pH value of the leaching solution and the rare earth content in the phosphogypsum; stop leaching when more than 76% of the rare earth in the phosphogypsum is transferred to the mycelium balls and the leaching solution; filter and separate the mycelium balls with a 20-mesh screen, and then filter and separate the phosphogypsum and the leaching solution with a 300-mesh filter cloth, and return the mycelium balls, filtrate and filter residue washing water to the leaching tank, and then add phosphogypsum powder, 0.1% to 5% potato juice, 1 to 4g / L glucose, and repeat the leaching for 48 hours; if the total rare earth content of the leaching solution is ≥100 ppm, stop leaching, filter and separate the mycelium balls, and the mycelium balls are mycelium balls enriched with rare earth elements; the filtrate and filter residue washing water are returned to be used for culturing Aspergillus niger culture medium; (4) Recovery of rare earth from mycelium pellets The mycelium balls enriched with rare earth elements collected in the previous step are dried with hot air and then oxidized into ashes at high temperature to obtain rare earth oxides.
2. The method according to claim 1, characterized in that In step (2), the concentration of citric acid in the Aspergillus niger culture solution used to prepare the leaching solution is ≥10 mmol / L; and the nutrient composition is 20% potato juice and 20 g / L glucose.
3. The method according to claim 1, characterized in that In step (3), the leaching tank is a container or other device that can contain the leaching solution and phosphogypsum and can achieve stirring or bubbling; the leaching tank adopts heating and heat preservation measures to keep the temperature of the leaching solution in the range of 29°C±9°C; the mass ratio of the leaching solution to the phosphogypsum is 0.4:1 to 40:
1.
4. The method according to claim 1, characterized in that In step (4), the high temperature oxidation process is burning or decomposition at a temperature above 400° C. in air or oxygen atmosphere.
Citation Information
Cited By
Method for synergistically leaching rare earth elements in process of preparing phosphoric acid by acidolysis of phosphate concentrate
CN121109789A