Metal coating and preparation method and application thereof
By combining the nickel layer and the modified silica/conductive metal composite material layer in the metal plating, the problem of difficult to take into account in the prior art is solved, and the self-cleaning and conductive performance of the metal matrix is improved. Reduced costs.
Patent Information
- Application Number
- CN202411048875.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
It is difficult for existing metal coatings to have excellent electrical conductivity, hydrophobicity and low cost in the automotive field, and are prone to water droplets or wet mud deposition, which affects use.
Using a metal plating layer including a nickel layer and a conductive hydrophobic material layer, the conductive hydrophobic material layer consists of modified silica and conductive metal, and is formed by electroplating. The modified silica is modified by a silicone modifier and combined with conductive The metal salt is electroplated in the plating solution to form a plating layer with high hydrophobicity and electrical conductivity.
It realizes the self-cleaning function of the metal matrix surface, improves the conductivity and hydrophobic properties, reduces costs, and meets the use needs in harsh environments.
Smart Images

Figure CN118979294A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of super-hydrophobic materials, and in particular to a metal coating and a preparation method and application thereof. Background Art
[0002] Metal coatings are used in the automotive field to enhance the corrosion resistance, aesthetics and wear resistance of metal substrate surfaces. Metal coatings used for water level detection need to have both excellent conductivity and good coating cleanliness, which requires the coating to be hydrophobic, have good surface self-cleaning properties and conductivity. Most existing coatings cannot meet these requirements.
[0003] Chinese invention patent CN 115110128 B discloses a method for preparing a highly stable nickel tetradecanoate super-hydrophobic coating on a metal surface, belonging to the field of super-hydrophobic coating. The present invention first uses Watt nickel plating solution to prepare a layer of pure nickel layer on the metal sheet surface; then corrosion treatment is carried out in the anodic corrosion solution made of nickel sulfate, sulfuric acid and deionized water, so as to produce micron-sized holes; finally, electrodeposition is carried out in a solution made of nickel chloride, tetradecanoic acid and anhydrous ethanol, and a nickel tetradecanoate super-hydrophobic coating is obtained. The present invention uses an anodic corrosion method to prepare micron-sized holes, combines nickel tetradecanoate particles with low surface energy, and improves the stability of the super-hydrophobic coating. Although the hydrophobicity and electrical conductivity of this nickel tetradecanoate super-hydrophobic coating (nickel plating and nickel tetradecanoate plating) can meet the use requirements; however, the price of nickel plating after nickel plating is relatively expensive, and the cost is relatively high. Summary of the invention
[0004] The purpose of the present invention is to overcome the problem that water droplets or wet mud are easily deposited on the surface of a metal substrate, causing corrosion and affecting use, and the poor conductivity of the metal substrate surface, as well as the high cost of existing metal coatings, and to provide a metal coating and a preparation method and application thereof. The metal coating provided by the present invention has excellent hydrophobicity and conductivity, thereby automatically cleaning water droplets, mud, dust and other pollutants on the surface of the metal substrate, and realizing the function of rapid response of the metal substrate in practical applications.
[0005] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a metal coating, which includes a nickel layer and a conductive hydrophobic material layer, wherein the conductive hydrophobic material layer contains modified silica and a conductive metal, wherein the modified silica contains silica and a siloxane segment formed on the surface of the silica.
[0006] Preferably, the surface contact angle of the conductive hydrophobic material layer is greater than 100°, preferably 145-150°.
[0007] Preferably, the conductivity of the conductive hydrophobic material layer is (1.45-1.5)×10 -6Ω · cm.
[0008] Preferably, the modified silicon dioxide is obtained by modifying silicon dioxide with a siloxane modifier.
[0009] Preferably, the mass ratio of the siloxane modifier to the silicon dioxide is 1:0.1-15, preferably 1:1-10.
[0010] Preferably, the siloxane modifier is hydrogen-containing silicone oil, preferably one or more of polydimethyl hydrogen-containing silicone oil, ethyl hydrogen-containing silicone oil and phenyl hydrogen-containing silicone oil.
[0011] Preferably, in the conductive hydrophobic material layer, the molar ratio of the modified silicon dioxide to the conductive metal is 1:1-4, preferably 1:1-3.
[0012] Preferably, the conductive metal is one or more of copper, silver, aluminum and gold.
[0013] Preferably, the thickness ratio of the nickel layer to the conductive hydrophobic material layer is 1:0.8-1.
[0014] Preferably, the thickness of the nickel layer is 2um-10um, more preferably 2um-4um.
[0015] Preferably, the thickness of the conductive hydrophobic material layer is 1.6um-10um, more preferably 1.6um-4um.
[0016] A second aspect of the present invention provides a method for preparing a metal coating, the method comprising the following steps:
[0017] (1) forming a nickel layer by electroplating;
[0018] (2) electroplating the nickel layer in an electroplating solution containing modified silicon dioxide and a conductive metal salt, wherein the modified silicon dioxide is modified by a siloxane modifier.
[0019] Preferably, the preparation process of the modified silica is: mixing silica, a siloxane modifier and a catalyst.
[0020] Preferably, the siloxane modifier is hydrogen-containing silicone oil, preferably one or more of polydimethyl hydrogen-containing silicone oil, ethyl hydrogen-containing silicone oil and phenyl hydrogen-containing silicone oil.
[0021] Preferably, the mass ratio of the siloxane modifier to the silicon dioxide is 1:0.1-15, preferably 1:1-10.
[0022] Preferably, the catalyst is a karstedt catalyst.
[0023] Preferably, the mass ratio of the catalyst to the silicon dioxide is 1:5000-9000.
[0024] Preferably, the mixing conditions include: temperature of 0-100°C and time of 5-12h.
[0025] Preferably, in the electroplating solution of step (2), the molar ratio of the modified silicon dioxide to the conductive metal salt is 1:1-4, preferably 1:1-3.
[0026] Preferably, in the electroplating solution of step (2), the concentration of the conductive metal salt is 5-25 g / 100 mL.
[0027] Preferably, the conductive metal salt is one or more of copper salt, silver salt, aluminum salt and gold salt.
[0028] Preferably, in step (2), the electroplating conditions include: a temperature of 40-60°C, a current density of 4-5A / dm 2 The electroplating time is 1-2 hours, and the pH value of the electroplating solution is 3-5.
[0029] Preferably, in step (1), the concentration of nickel salt in the nickel electroplating solution used to form the nickel layer by electroplating is 300-400 g / L, and the pH value of the nickel electroplating solution is 3-5.
[0030] Preferably, in step (1), the electroplating conditions include: a temperature of 40-60°C, a current density of 4-5A / dm 2 , the plating time is 1-2 hours.
[0031] A third aspect of the present invention provides a metal coating prepared by the method described above.
[0032] A fourth aspect of the present invention provides an application of the metal coating mentioned above in water level detection.
[0033] Compared with the prior art, the present invention has at least the following technical effects:
[0034] (1) The metal coating described in the present invention includes two layers located on the surface of the metal substrate, one layer is a nickel layer, and the other layer is a conductive hydrophobic material layer containing modified silicon dioxide and a conductive metal. The nickel layer can improve the bonding strength between the conductive hydrophobic material layer and the surface of the metal substrate; the modified silicon dioxide has a siloxane segment, which has good hydrophobicity and dispersibility. The presence of the conductive metal can improve the conductive properties of the metal substrate surface. Therefore, the metal coating can solve the problem of water, ice, debris and wet mud adhesion on the metal surface, realize the self-cleaning function of the coating to prevent mud and water adhesion, and meet the requirements for metal conductivity and water resistance and pollution prevention in harsh environments.
[0035] (2) The method of the present invention is simple, and the nickel layer and the conductive hydrophobic material layer can be formed by electroplating. When forming the conductive hydrophobic material layer, it is only necessary to directly electroplate the electroplating solution containing siloxane-modified modified silicon dioxide and a conductive metal salt. The surface contact angle of the metal coating formed by this method is greater than 100°, or even as high as 150°, which can realize the self-cleaning function of the metal coating against pollutants such as water, muddy water, and dust, and can greatly improve the conductive performance of the metal coating.
[0036] (3) The method of the present invention adds modified silicon dioxide when forming a conductive hydrophobic material layer on the nickel layer, thereby reducing the amount of precious metals used and saving costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 It is a schematic diagram of one embodiment of the metal plating layer of the present invention;
[0038] Figure 2 It is a schematic diagram of forming a conductive hydrophobic material layer by electroplating. DETAILED DESCRIPTION
[0039] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.
[0040] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0041] The metal plating layer provided by the present invention comprises a nickel layer and a conductive hydrophobic material layer, wherein the conductive hydrophobic material layer contains modified silicon dioxide and a conductive metal, wherein the modified silicon dioxide contains silicon dioxide and a siloxane segment formed on the surface of the silicon dioxide.
[0042] In the present invention, the surface of the modified silica has both hydrophilic Si-OH groups and hydrophobic siloxane segments. The rigid siloxane segments repel each other, which can increase the steric hindrance between silica particles, effectively inhibit the agglomeration of silica particles, and improve the stability of particles in various environments. Among them, the silica and the siloxane segments are connected by a binary cross-linked structure, and the structure of the siloxane segment is -OSi(CH3) 2 O-, both ends of the siloxane chain segment are connected to the silicon on the silica.
[0043] In the present invention, the modified silica is obtained by modifying silica with a siloxane modifier. In some embodiments, the mass ratio of the siloxane modifier to the silica can be 1:0.1-15. In order to improve the hydrophobic properties of the conductive hydrophobic material layer, in a more preferred embodiment, the mass ratio of the siloxane modifier to the silica is 1:1-10. In a preferred embodiment, the siloxane modifier is a hydrogen-containing silicone oil, more preferably one or more of polydimethyl hydrogen-containing silicone oil, ethyl hydrogen-containing silicone oil and phenyl hydrogen-containing silicone oil. In a more specific embodiment, the preparation process of the modified silica is: mixing silica, a siloxane modifier and a catalyst. Among them, the catalyst is a karstedt catalyst; the mass ratio of the amount of the catalyst to the silica is 1:5000-9000; the mixing conditions include: a temperature of 0°C-100°C and a time of 5-12h.
[0044] In some embodiments, in the modified silica, the mass ratio of the siloxane segment to the silica may be 1: 1-15, preferably 1: 1-10. The mass ratio of the siloxane segment to the silica may be determined according to the feed ratio of the siloxane modifier to the silica during the preparation of the modified silica. In the obtained metal coating, the ratio of the siloxane segment to the silica is equivalent to the feed ratio of the siloxane modifier to the silica.
[0045] The nickel layer and the conductive hydrophobic material layer in the metal plating layer of the present invention can be formed on the surface of the metal substrate in sequence. The material, shape and size of the metal substrate can be selected according to actual needs, so there is no special limitation.
[0046] In the present invention, if Figure 1 As shown, the metal plating layer of the present invention comprises a nickel layer and a conductive hydrophobic material layer sequentially formed on the surface of the metal substrate. The nickel layer can improve the bonding strength between the conductive hydrophobic material layer and the surface of the metal substrate; the conductive hydrophobic material layer has good hydrophobicity and conductivity.
[0047] In some embodiments, the surface contact angle of the conductive hydrophobic material layer is greater than 100°, preferably 145-150°. In the present invention, a contact angle meter is used to measure the surface contact angle of the metal coating to evaluate its hydrophobicity. The surface contact angle refers to the angle between the surface of the metal coating and the tangent line of the droplet when the liquid drops on the surface of the metal coating. The contact angle represents the wettability of the liquid on the metal coating. The closer the contact angle is to 180°, the better the self-cleaning ability of the metal coating.
[0048] When the surface contact angle is greater than 90°, the liquid-solid interfacial tension is greater than the gas-solid interfacial tension, that is, the attraction between the solid and the gas is greater than the attraction between the solid and the liquid. At this time, the water droplets will not stay on the metal surface, and the rolling water droplets will take away the sludge and dust. After adding a conductive hydrophobic material layer to the surface of the metal substrate, the metal plating surface has a nano-rough structure, and the attraction of the gas between the nano-scale convex hulls is greater than the attraction between the nano-scale convex hulls and the air, so that the water will not spread on the surface of the metal substrate, and the hydrophobic function is realized. This phenomenon applies the lotus principle: there are many tiny convex hulls on the surface of the lotus leaf, which are about 10μm on average, and each convex hull is composed of a hair-like structure with a diameter of 200 nanometers, so that the lotus leaf has a nano-type periodic structure. When the water droplets fall, they will fall on the nano-type convex hulls. There is a lot of air between the convex hulls, so the water will not spread out on the surface of the lotus leaf, so it cannot wet the lotus leaf, so that water and pollutants are not easy to adhere to the surface of the lotus leaf, thus showing hydrophobic properties and realizing the self-cleaning function.
[0049] The self-cleaning function means that when a pollutant stays on the surface of the substrate, it will appear suspended in the air at the microscopic level. At the same time, because the surface contact angle is greater than 90°, water droplets will not spread on the metal surface. When the water droplets leave the metal substrate surface, they will take away the pollutants, thus achieving the self-cleaning function.
[0050] In some embodiments, the conductivity of the conductive hydrophobic material layer may be (1.45-1.5)×10 -6 Ω · In the present invention, the conductivity of the prepared metal coating is measured by an eddy current conductivity meter, and the conductivity of the metal substrate can be improved by plating a modified silicon dioxide / copper composite material (conductive hydrophobic material layer) on the surface of the metal substrate after metal nickel plating.
[0051] In some embodiments, the molar ratio of the modified silicon dioxide to the conductive metal may be 1:1-4. In order to make the metal coating have excellent hydrophobicity and conductivity, in a preferred embodiment, the molar ratio of the modified silicon dioxide to the conductive metal is 1:1-3. In the obtained metal coating, the molar ratio of the modified silicon dioxide to the conductive metal can be determined according to the feed ratio, which is equivalent to the feed ratio.
[0052] In the metal plating provided by the present invention, the conductive metal may be various metals well known in the art. In some embodiments, the conductive metal may be one or more of copper, silver, aluminum and gold, preferably copper.
[0053] In the present invention, the thickness of the nickel layer and the conductive hydrophobic material layer will affect the hydrophobicity and conductive properties of the metal plating layer. In some embodiments, the ratio of the thickness of the nickel layer to the conductive hydrophobic material layer can be 1:0.8-1. In some preferred embodiments, the thickness of the nickel layer is 2um-10um, more preferably 2um-4um. In some preferred embodiments, the thickness of the conductive hydrophobic material layer is 1.6um-10um, more preferably 1.6um-4um.
[0054] The metal plating layer provided by the present invention can realize the self-cleaning function of the metal substrate without affecting the conductive performance of the metal substrate, and the conductive hydrophobic material layer and the metal substrate have a high bonding strength.
[0055] The method for preparing a metal coating provided by the present invention comprises the following steps:
[0056] (1) forming a nickel layer by electroplating;
[0057] (2) electroplating the nickel layer in an electroplating solution containing modified silicon dioxide and a conductive metal salt, wherein the modified silicon dioxide is modified by a siloxane modifier.
[0058] In a specific embodiment, the method for preparing the metal coating comprises:
[0059] 1) forming a nickel layer on the surface of a metal substrate by electroplating;
[0060] 2) electroplating the nickel layer in an electroplating solution containing modified silicon dioxide and a conductive metal salt to form a conductive hydrophobic material layer, wherein the modified silicon dioxide is modified by a siloxane modifier.
[0061] The method of the present invention first uses electroplating to plate nickel as a base, and then plates a modified silicon dioxide / metal composite material layer (conductive hydrophobic material layer) on the nickel plating layer, which can not only improve the bonding strength between the conductive hydrophobic material layer and the surface of the metal substrate, but also improve the hydrophobicity and conductivity of the metal plating layer.
[0062] In the present invention, the metal substrate can be selected according to actual needs. In a specific embodiment, the metal substrate can be pretreated before use, and the process of pretreating the metal substrate is: after the metal substrate is polished to 2000 mesh, it is rinsed with deionized water and anhydrous ethanol and then blown dry, and then the metal substrate is placed in a degreasing liquid for ultrasonic cleaning for ten minutes, and then rinsed with deionized water and anhydrous ethanol and blown dry.
[0063] In one embodiment, when the nickel layer is formed by electroplating in step (1), the pretreated metal substrate can be placed in a nickel electroplating solution as a cathode, and a pure nickel plate can be used as an anode for electroplating.
[0064] In some embodiments, the concentration of nickel salt in the nickel electroplating solution is 300-400 g / L, and the pH value of the nickel electroplating solution is 3-5. In a more specific embodiment, the nickel plating solution can be a mixed aqueous solution of 300 g / L nickel sulfate, 45 g / L nickel chloride, 35 g / L boric acid and 0.1 g / L sodium dodecyl sulfate.
[0065] In a preferred embodiment, in order to form a nickel layer of a specific thickness, in step (1), the electroplating conditions include: a temperature of 40-60° C., a current density of 4-5 A / dm 2 , the plating time is 1-2 hours.
[0066] In step (2), since silicon dioxide is hydrophilic, the inventors modified it and added it to the electroplating solution for electroplating, so that the formed coating containing modified silicon dioxide has good hydrophobicity and dispersibility.
[0067] In the present invention, the electroplating solution can be prepared by the following steps: firstly preparing nano-silica particles by a sol-gel method, then modifying the nano-silica by a siloxane modifier to prepare modified nano-silica, and then mixing the modified nano-silica with a copper plating solution.
[0068] In one embodiment, the preparation process of the modified silicon dioxide may be: mixing nano silicon dioxide, a siloxane modifier and a catalyst. The nano silicon dioxide may be prepared according to conventional methods in the art, or may be prepared by a new method.
[0069] In the method of the present invention, the siloxane modifier can be a conventional choice in the art. In one embodiment, the siloxane modifier can be a hydrogen-containing silicone oil. In some preferred embodiments, the siloxane modifier is one or more of polydimethyl hydrogen-containing silicone oil, ethyl hydrogen-containing silicone oil and phenyl hydrogen-containing silicone oil.
[0070] In some embodiments, the mass ratio of the siloxane modifier to the silicon dioxide can be 1:0.1-15. In order to further improve the hydrophobicity and conductivity of the prepared metal coating, the mass ratio of the siloxane modifier to the silicon dioxide is 1:1-10, for example, 1:1, 1:12, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10.
[0071] In the method of the present invention, the catalyst used to modify the silicon dioxide can be a conventional choice in the art, for example, it can be a karstedt catalyst. In some embodiments, the mass ratio of the amount of the catalyst to the amount of the silicon dioxide can be 1:5000-9000. In the process of preparing modified silicon dioxide, the mixing conditions include: a temperature of 0°C-100°C and a time of 5-12h.
[0072] In a more specific embodiment, the preparation process of the modified silica is: preparing nano-silica particles by a sol-gel method, then adding a siloxane modifier and a catalyst to the nano-silica particles, magnetically stirring, and then filtering the obtained product, washing it with anhydrous ethanol several times during ultrasonic vibration, and redispersing the nano-particles.
[0073] In the present invention, the copper plating solution can be prepared according to the existing method or according to the new method. In one embodiment, the copper plating solution can be prepared according to the following method: 0.5-3g of brightener and 0.5-3g of wetting agent are added to 100mL of deionized water and stirred until dissolved; then 8-15g of copper sulfate and 5-9g of copper chloride are added to the above solution and stirred at room temperature until dissolved; then 4-7g of sodium sulfate and 6-12g of potassium sulfate are added to the solution, heated to 55-65°C, stirred while heating, and then a buffer is added to adjust the pH value to between 3-5.
[0074] In the present invention, in order to obtain a conductive hydrophobic material layer with a moderate ratio of modified silica to conductive metal, and to ensure that the obtained metal coating has both excellent hydrophobic properties and conductive properties, in the electroplating solution of step (2), the molar ratio of the modified silica to the conductive metal salt can be 1:1-4, preferably 1:1-3.
[0075] In some embodiments, in the electroplating solution of step (2), the concentration of the conductive metal salt may be 5-25 g / 100 mL, for example, 5 g / 100 mL, 10 g / 100 mL, 15 g / 100 mL, 20 g / 100 mL or 25 g / 100 mL.
[0076] In the present invention, the conductive metal salt may be an inorganic salt of a conductive metal commonly used in the art. In some embodiments, the conductive metal salt may be one or more of a copper salt, a silver salt, an aluminum salt, and a gold salt. In a more specific embodiment, the conductive metal salt may be a sulfate and / or chloride salt of a conductive metal.
[0077] In one embodiment, Figure 2As shown, when electroplating is performed in step (2), the anode is pure copper, the cathode is a nickel-plated metal substrate, and the electroplating solution is an electroplating solution containing modified silicon dioxide and a conductive metal salt. In some embodiments, the electroplating conditions in step (2) include: a temperature of 40-60°C, a current density of 4-5A / dm 2 The electroplating time is 1-2 hours, and the pH value of the electroplating solution is 3-5.
[0078] In a more specific embodiment, the electroplating process in step (2) can be carried out under the condition of magnetic stirring, wherein the rate of the magnetic stirring can be 300-500 r / min.
[0079] The present invention also provides a metal coating prepared by the method described above, wherein the metal coating realizes the self-cleaning property of the metal substrate and does not affect the conductive property of the metal substrate.
[0080] The present invention also provides an application of the metal coating described above in water level detection. The metal coating provided by the present invention is widely applicable, especially in the automotive field or the industrial field.
[0081] The metal coating of the present invention is based on nickel electroplating, and a modified silicon dioxide / metal composite material (conductive hydrophobic material layer) is plated in the water level signal sensing area, which can meet the requirements of metal conductivity and water resistance and pollution prevention in harsh environments.
[0082] The present invention will be described in detail below by way of examples, but the protection scope of the present invention is not limited thereto. In the following examples, unless otherwise specified, the raw materials used are all common commercially available products.
[0083] In the following examples:
[0084] The steps of preparing nano-silica particles by the sol-gel method include: mixing silicate, sodium hydroxide and ethanol in a mass ratio of 1:0.5:1, dripping sodium hydroxide and ethanol into ethyl orthosilicate at room temperature for reaction for half an hour, centrifuging the reaction solution and washing with water for 2 hours, repeating 5 times to obtain a silica suspension, and drying it after standing for 2 days.
[0085] Hydrogenated silicone oil is polydimethyl hydrogenated silicone oil, with a hydrogen content of 1.58-1.6% and a viscosity of 20-40 (mm 2 / 25℃).
[0086] Example 1
[0087] S1. Pretreatment of metal substrate: After grinding the metal sheet to 2000 mesh, rinse it with deionized water and anhydrous ethanol and blow it dry. Then, put the metal substrate into the degreasing liquid for ultrasonic cleaning for ten minutes, and then rinse it with deionized water and anhydrous ethanol and blow it dry.
[0088] S2. Electroplated nickel layer on metal substrate:
[0089] S21, preparing a mixed aqueous solution of 300 g / L nickel sulfate, 45 g / L nickel chloride, 35 g / L boric acid and 0.1 g / L sodium dodecyl sulfate as a nickel electroplating solution;
[0090] S22, put the pretreated metal substrate into the nickel electroplating solution as the cathode, the anode is a pure nickel plate, the electroplating temperature is 50 ° C, the current density is 4.5A / dm 2 The electroplating time is 1.5 hours, the pH value of the nickel electroplating solution is 4.5, and a magnetic stirring speed of 400 r / min is applied during the electroplating process to obtain a nickel layer.
[0091] S3, electroplating a conductive hydrophobic material layer on a metal substrate:
[0092] S31, preparing nano-silica particles by a sol-gel method, then adding hydrogen-containing silicone oil (100 g) and a catalyst (0.1 g) to the nano-silica particles, and magnetically stirring at 50° C. for 8 h, wherein the mass ratio of the hydrogen-containing silicone oil to the nano-silica particles is 1:10, and the mass ratio of the catalyst to the amount of the nano-silica is 1:5000, and then filtering the obtained product, washing it with anhydrous ethanol several times during ultrasonic oscillation, and redispersing the nano-particles to obtain modified nano-silica;
[0093] S32, add 1.5g brightener and 2g wetting agent to 100mL deionized water and stir until dissolved; then take 12g copper sulfate and 7g copper chloride and add them to the above solution, stir until dissolved at room temperature; then add 6g sodium sulfate and 9g potassium sulfate to the solution, heat to 60°C, stir while heating, and add buffer (HCl solution) under stirring to adjust the pH value of the solution to 4 to obtain a copper plating solution;
[0094] S33, mixing the modified silicon dioxide with the copper plating solution to obtain a plating solution, wherein the molar ratio of the modified nano silicon dioxide to the copper salt (copper sulfate and copper chloride) is 1:1.2;
[0095] S34, put the nickel-plated metal substrate into the electroplating solution as the cathode, the anode is pure copper, the electroplating temperature is 50°C, the current density is 4.5A / dm 2 The electroplating time was 1.5 hours, the pH value of the electroplating solution was 4.5, and magnetic stirring at 400 r / min was applied during the electroplating process.
[0096] Example 2
[0097] S1. Pretreatment of metal substrate: After grinding the metal sheet to 2000 mesh, rinse it with deionized water and anhydrous ethanol and blow it dry. Then, put the metal substrate into the degreasing liquid for ultrasonic cleaning for ten minutes, and then rinse it with deionized water and anhydrous ethanol and blow it dry.
[0098] S2. Electroplated nickel layer on metal substrate:
[0099] S21, preparing a mixed aqueous solution of 300 g / L nickel sulfate, 45 g / L nickel chloride, 35 g / L boric acid and 0.1 g / L sodium dodecyl sulfate as a nickel electroplating solution;
[0100] S22, put the pretreated metal substrate into the nickel electroplating solution as the cathode, the anode is a pure nickel plate, the electroplating temperature is 50 ° C, the current density is 4.5A / dm 2 The electroplating time is 1.5 hours, the pH value of the nickel electroplating solution is 4.5, and a magnetic stirring speed of 400 r / min is applied during the electroplating process to obtain a nickel layer.
[0101] S3, electroplating a conductive hydrophobic material layer on a metal substrate:
[0102] S31, preparing nano-silica particles by a sol-gel method, then adding hydrogen-containing silicone oil (80 g) and a catalyst (0.08 g) to the nano-silica particles, and magnetically stirring at 80° C. for 8 h, wherein the mass ratio of the hydrogen-containing silicone oil to the nano-silica particles is 1:10, and the mass ratio of the catalyst to the amount of the nano-silica is 1:7000, and then filtering the obtained product, washing it with anhydrous ethanol several times during ultrasonic oscillation, and redispersing the nano-particles to obtain modified nano-silica;
[0103] S32, adding 1.5g of brightener and 2g of wetting agent into 100mL of deionized water and stirring until dissolved; then taking 12g of copper sulfate and 7g of copper chloride and adding them to the above solution, stirring at room temperature until dissolved; then adding 6g of sodium sulfate and 9g of potassium sulfate into the solution, heating to 60°C, stirring while heating, and then adding a buffer (HCl solution) under stirring to adjust the pH value of the solution to 4 to obtain a copper plating electroplating solution;
[0104] S33, mixing the modified silicon dioxide with the copper plating solution to obtain a plating solution, wherein the molar ratio of the modified nano silicon dioxide to the copper salt (copper sulfate and copper chloride) is 1:1;
[0105] S34, put the nickel-plated metal substrate into the electroplating solution as the cathode, the anode is pure copper, the electroplating temperature is 50°C, the current density is 4.5A / dm 2 The electroplating time was 1.5 hours, the pH value of the electroplating solution was 4.5, and magnetic stirring at 400 r / min was applied during the electroplating process.
[0106] Example 3
[0107] S1. Pretreatment of metal substrate: After grinding the metal sheet to 2000 mesh, rinse it with deionized water and anhydrous ethanol and blow it dry. Then, put the metal substrate into the degreasing liquid for ultrasonic cleaning for ten minutes, and then rinse it with deionized water and anhydrous ethanol and blow it dry.
[0108] S2. Electroplated nickel layer on metal substrate:
[0109] S21, preparing a mixed aqueous solution of 300 g / L nickel sulfate, 45 g / L nickel chloride, 35 g / L boric acid and 0.1 g / L sodium dodecyl sulfate as a nickel electroplating solution;
[0110] S22, put the pretreated metal substrate into the nickel electroplating solution as the cathode, the anode is a pure nickel plate, the electroplating temperature is 50 ° C, the current density is 4.5A / dm 2 The electroplating time is 1.5 hours, the pH value of the nickel electroplating solution is 4.5, and a magnetic stirring speed of 400 r / min is applied during the electroplating process to obtain a nickel layer.
[0111] S3, electroplating a conductive hydrophobic material layer on a metal substrate:
[0112] S31, preparing nano-silica particles by a sol-gel method, then adding hydrogen-containing silicone oil (90g) and a catalyst (0.09g) to the nano-silica particles, and magnetically stirring at 30°C for 8h, wherein the mass ratio of the hydrogen-containing silicone oil to the nano-silica particles is 1:10, and the mass ratio of the catalyst to the amount of the nano-silica is 1:7000, then filtering the obtained product, washing it with anhydrous ethanol several times during ultrasonic oscillation, and redispersing the nano-particles to obtain modified nano-silica;
[0113] S32, adding 1.5g of brightener and 2g of wetting agent into 100mL of deionized water and stirring until dissolved; then taking 12g of copper sulfate and 7g of copper chloride and adding them to the above solution, stirring at room temperature until dissolved; then adding 6g of sodium sulfate and 9g of potassium sulfate into the solution, heating to 60°C, stirring while heating, and then adding a buffer (HCl solution) under stirring to adjust the pH value of the solution to 4 to obtain a copper plating electroplating solution;
[0114] S33, mixing the modified silicon dioxide with the copper plating solution to obtain a plating solution, wherein the molar ratio of the modified nano silicon dioxide to the copper salt (copper sulfate and copper chloride) is 1:3;
[0115] S34, put the nickel-plated metal substrate into the electroplating solution as the cathode, the anode is pure copper, the electroplating temperature is 50°C, the current density is 4.5A / dm 2The electroplating time was 1.5 hours, the pH value of the electroplating solution was 4.5, and magnetic stirring at 400 r / min was applied during the electroplating process.
[0116] Comparative Example 1
[0117] The method of Example 1 is followed, except that the nano-silicon dioxide particles are not modified, and the nano-silicon dioxide particles are directly mixed with the copper plating solution to prepare the plating solution.
[0118] The specific operations are:
[0119] S1. Pretreatment of metal substrate: After grinding the metal sheet to 2000 mesh, rinse it with deionized water and anhydrous ethanol and blow it dry. Then, put the metal substrate into the degreasing liquid for ultrasonic cleaning for ten minutes, and then rinse it with deionized water and anhydrous ethanol and blow it dry.
[0120] S2. Electroplated nickel layer on metal substrate:
[0121] S21, preparing a mixed aqueous solution of 300 g / L nickel sulfate, 45 g / L nickel chloride, 35 g / L boric acid and 0.1 g / L sodium dodecyl sulfate as a nickel electroplating solution;
[0122] S22, put the pretreated metal substrate into the nickel electroplating solution as the cathode, the anode is a pure nickel plate, the electroplating temperature is 50 ° C, the current density is 4.5A / dm 2 The electroplating time is 1.5 hours, the pH value of the nickel electroplating solution is 4.5, and a magnetic stirring speed of 400 r / min is applied during the electroplating process to obtain a nickel layer.
[0123] S3, electroplating a conductive hydrophobic material layer on a metal substrate:
[0124] S31, adding 1.5g of brightener and 2g of wetting agent to 100mL of deionized water and stirring until dissolved; then taking 12g of copper sulfate and 7g of copper chloride and adding them to the above solution, stirring at room temperature until dissolved; then adding 6g of sodium sulfate and 9g of potassium sulfate to the solution, heating to 60°C, stirring while heating, and adding a buffer (HCl solution) under stirring to adjust the pH value of the solution to 4, to obtain a copper plating solution;
[0125] S32, mixing the nano-silicon dioxide particles with the copper plating solution to obtain a plating solution, wherein the molar ratio of the nano-silicon dioxide particles to the copper salt (copper sulfate and copper chloride) is 1:1.2;
[0126] S33, put the nickel-plated metal substrate into the electroplating solution as the cathode, the anode is pure copper, the electroplating temperature is 50°C, the current density is 4.5A / dm 2The electroplating time was 1.5 hours, the pH value of the electroplating solution was 4.5, and magnetic stirring at 400 r / min was applied during the electroplating process.
[0127] Comparative Example 2
[0128] The method of Example 1 is followed, except that the nickel electroplating solution and the electroplating solution containing modified silicon dioxide and copper electroplating solution are mixed together for electroplating.
[0129] The specific operations are:
[0130] S1. Pretreatment of metal substrate: After grinding the metal sheet to 2000 mesh, rinse it with deionized water and anhydrous ethanol and blow it dry. Then, put the metal substrate into the degreasing liquid for ultrasonic cleaning for ten minutes, and then rinse it with deionized water and anhydrous ethanol and blow it dry.
[0131] S2. Electroplated nickel layer on metal substrate:
[0132] S21, preparing a mixed aqueous solution of 300 g / L nickel sulfate, 45 g / L nickel chloride, 35 g / L boric acid and 0.1 g / L sodium dodecyl sulfate as a nickel electroplating solution;
[0133] S22, preparing nano-silica particles by a sol-gel method, then adding hydrogen-containing silicone oil (100 g) and a catalyst (0.1 g) to the nano-silica particles, and magnetically stirring at 50° C. for 8 h, wherein the mass ratio of the hydrogen-containing silicone oil to the nano-silica particles is 1:10, and the mass ratio of the amount of the catalyst to the nano-silica can be 1:5000, and then filtering the obtained product, washing it with anhydrous ethanol several times during ultrasonic oscillation, and redispersing the nano-particles to obtain modified nano-silica;
[0134] S23, add 1.5g brightener and 2g wetting agent to 100mL deionized water and stir until dissolved; then take 12g copper sulfate and 7g copper chloride and add them to the above solution, stir until dissolved at room temperature; then add 6g sodium sulfate and 9g potassium sulfate to the solution, heat to 60°C, stir while heating, and add buffer (HCl solution) under stirring to adjust the pH value of the solution to 4 to obtain a copper plating solution;
[0135] S24, mixing a nickel electroplating solution, modified silicon dioxide and the copper electroplating solution to obtain an electroplating solution, wherein the molar ratio of the modified nano silicon dioxide to the copper salt (copper sulfate and copper chloride) is 1:1.2, and the molar ratio of the modified nano silicon dioxide to the nickel salt is 1:1;
[0136] S25, put the pretreated metal substrate into the electroplating solution as the cathode, the anode is a pure nickel plate, the electroplating temperature is 50 ° C, the current density is 4.5A / dm 2The electroplating time is 1.5 hours, the pH value of the nickel electroplating solution is 4.5, and a magnetic stirring speed of 400 r / min is applied during the electroplating process.
[0137] Test Example 1
[0138] The thickness of the nickel layer and the thickness of the conductive hydrophobic material layer in the metal plating layers obtained in the examples and comparative examples were tested and calculated, and the results are shown in Table 1.
[0139] The instrument is an X-ray film thickness measuring instrument. The measuring process is as follows: first place the film sample to be measured on the sample table, and then start the instrument for measurement.
[0140] Table 1
[0141]
[0142] Test Example 2
[0143] The surface contact angles of the metal coatings obtained in the examples and comparative examples were tested using a contact angle meter. The results are shown in Table 2.
[0144] The electrical conductivity of the metal coatings obtained in the embodiment and the comparative example was tested using an eddy current conductivity meter, and the results are shown in Table 2.
[0145] The bonding strength between the metal coatings obtained in the embodiments and comparative examples and the metal substrate was tested by end face observation method. The results are shown in Table 2.
[0146] Table 2
[0147] Example No. Surface contact angle Conductivity Bonding strength Example 1 150 <![CDATA[1.53x10 -6 Oh.cm]]> powerful Example 2 146 <![CDATA[1.5x10 -6 Oh.cm]]> powerful Example 3 148 <![CDATA[1.5x10 -6 Oh.cm]]> powerful Comparative Example 1 90 <![CDATA[1.52x10 -6 Oh.cm]]> powerful Comparative Example 2 95 <![CDATA[1.53x10 -6 Oh.cm]]> weak
[0148] It can be seen from Table 2 that the surface contact angle of the metal coating prepared by the method described in the present invention is significantly greater than that of the comparative example, and the hydrophobicity is significantly improved; and the conductive property is good and the bonding strength is high.
[0149] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A metal coating, characterized in that: The metal plating layer comprises a nickel layer and a conductive hydrophobic material layer, wherein the conductive hydrophobic material layer contains modified silicon dioxide and a conductive metal, wherein the modified silicon dioxide contains silicon dioxide and a siloxane segment formed on the surface of the silicon dioxide.
2. The metal coating according to claim 1, characterized in that: The surface contact angle of the conductive hydrophobic material layer is greater than 100°, preferably 145-150°.
3. The metal coating according to claim 1 or 2, characterized in that: The conductivity of the conductive hydrophobic material layer is (1.45-1.5)×10 -6 Ω · cm.
4. The metal coating according to any one of claims 1 to 3, characterized in that: The modified silicon dioxide is obtained by modifying silicon dioxide with a siloxane modifier; Preferably, the mass ratio of the siloxane modifier to the silicon dioxide is 1:0.1-15, preferably 1:1-10; Preferably, the siloxane modifier is hydrogen-containing silicone oil, preferably one or more of polydimethyl hydrogen-containing silicone oil, ethyl hydrogen-containing silicone oil and phenyl hydrogen-containing silicone oil.
5. The metal coating according to any one of claims 1 to 4, characterized in that: In the conductive hydrophobic material layer, the molar ratio of the modified silicon dioxide to the conductive metal is 1:1-4, preferably 1:1-3.
6. The metal coating according to any one of claims 1 to 5, characterized in that: The conductive metal is one or more of copper, silver, aluminum and gold.
7. The metal coating according to any one of claims 1 to 6, characterized in that: The thickness ratio of the nickel layer to the conductive hydrophobic material layer is 1:0.8-1; Preferably, the thickness of the nickel layer is 2um-10um, more preferably 2um-4um; Preferably, the thickness of the conductive hydrophobic material layer is 1.6um-10um, more preferably 1.6um-4um.
8. A method for preparing a metal coating, characterized in that: The method comprises the following steps: (1) forming a nickel layer by electroplating; (2) electroplating the nickel layer in an electroplating solution containing modified silicon dioxide and a conductive metal salt, wherein the modified silicon dioxide is modified by a siloxane modifier.
9. The method according to claim 8, characterized in that The preparation process of the modified silicon dioxide is as follows: silicon dioxide, a siloxane modifier and a catalyst are mixed.
10. The method according to claim 8 or 9, characterized in that: The siloxane modifier is hydrogen-containing silicone oil, preferably one or more of polydimethyl hydrogen-containing silicone oil, ethyl hydrogen-containing silicone oil and phenyl hydrogen-containing silicone oil; Preferably, the mass ratio of the siloxane modifier to the silicon dioxide is 1:0.1-15, preferably 1:1-10; Preferably, the catalyst is a karstedt catalyst; Preferably, the mass ratio of the catalyst to the silicon dioxide is 1:5000-9000; Preferably, the mixing conditions include: temperature of 0°C-100°C and time of 5-12h.
11. The method according to any one of claims 8 to 10, characterized in that: In the electroplating solution of step (2), the molar ratio of the modified silicon dioxide to the conductive metal salt is 1:1-4, preferably 1:1-3; Preferably, in the electroplating solution of step (2), the concentration of the conductive metal salt is 5-25 g / 100 mL; Preferably, the conductive metal salt is one or more of copper salt, silver salt, aluminum salt and gold salt.
12. The method according to any one of claims 8 to 11, characterized in that: In step (2), the electroplating conditions include: a temperature of 40-60°C, a current density of 4-5A / dm 2 The electroplating time is 1-2 hours, and the pH value of the electroplating solution is 3-5.
13. The method according to any one of claims 8 to 12, characterized in that: In step (1), the nickel layer is formed by electroplating in a nickel plating solution having a nickel salt concentration of 300-400 g / L and a pH value of 3-5; Preferably, in step (1), the electroplating conditions include: a temperature of 40-60°C, a current density of 4-5A / dm 2 , the plating time is 1-2 hours.
14. The metal coating prepared by the method according to any one of claims 8 to 13.
15. Use of the metal coating according to any one of claims 1 to 7 or the metal coating according to claim 14 in water level detection.
Citation Information
Cited By
Chemical copper plating nano modifier for SLP type support plate aMSAP process and preparation method thereof
CN120366754A