Battery cell tab defect detection method and device and storage medium

By evaluating and comparing the electrical performance parameters of the battery cell and using parameters such as leakage current to establish a defect evaluation model, the problem of complex detection of battery cell ear defects in the existing technology is solved, and more accurate and efficient The inspection improves the production quality of battery manufacturing.

CN118980947APending Publication Date: 2024-11-19SVOLT ENERGY TECH (WUXI) CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411099670.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing battery cell electrode defect detection methods are complex and have a high misjudgment rate, making it difficult to effectively detect defects in battery cell inner electrodes, affecting battery performance and safety.

Method used

By obtaining the electrical performance parameters of the battery cell to be tested and comparing the parameters of the standard battery cell, a defect evaluation model is established, and the degree of the electrode defect of the battery cell is calculated, using leakage current, full-voltage shelving capacity loss, full-voltage shelving voltage drop and DC internal Parameters such as resistance value are evaluated to reduce the misjudgment rate.

Benefits of technology

It improves the accuracy and reliability of battery cell ear defect detection, reduces equipment requirements, simplifies detection steps, and improves the production yield rate of battery manufacturing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118980947A_ABST
    Figure CN118980947A_ABST
Patent Text Reader

Abstract

The invention provides a cell tab defect detection method and device and a storage medium. The battery cell tab defect detection method comprises the following steps: acquiring a first electrical performance parameter of a to-be-detected battery cell; comparing the first electrical performance parameter of the to-be-tested battery cell with a first standard electrical performance parameter threshold value of a standard battery cell; if the first electrical performance parameter of the to-be-detected battery cell exceeds a first standard electrical performance parameter threshold value of the standard battery cell, determining that the to-be-detected battery cell has a tab defect, and defining the to-be-detected battery cell with the tab defect as a defective battery cell; establishing a defect evaluation model; acquiring a second electrical performance parameter of the defective cell; and substituting the first electrical performance parameter and the second electrical performance parameter of the defective battery cell into the defect evaluation model, and evaluating the tab defect degree of the defective battery cell. According to the electrical core tab defect detection method, the tab defect degree can be obtained by processing the electrical performance signals of the electrical core, the mode of collecting the electrical performance signals is low in misjudgment rate, the requirement for equipment is low, and the detection steps are easier to operate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and in particular to a method for detecting defects in a battery cell tab. The present invention also relates to a battery cell tab defect detection device based on the above-mentioned battery cell tab defect detection method, and a computer-readable storage medium capable of implementing the above-mentioned battery cell tab defect detection method. Background Art

[0002] With the global pursuit of environmental protection and sustainable development, the new energy industry is developing at an unprecedented speed. As the most important energy storage device, the safety of battery technology has naturally become the most concerned issue. The battery cell, as the smallest energy storage unit in the battery pack, is the source of battery power.

[0003] The structure of the battery cell is relatively complex, but its core can be simplified as a combination of multiple single-piece positive and negative electrodes welded in parallel with pole ears. The positive and negative electrodes are important components of the battery cell, and they are responsible for storing and releasing electrical energy. Between the two sheets, the transfer of ions is achieved through the electrolyte, thereby completing the conversion of electrical energy. The positive and negative electrode current collectors usually use micron-level aluminum foil and copper foil. In key processes such as pole ear welding and pole assembly shelling, due to the micron-level size and fragile physical properties of aluminum foil and copper foil, it is easy to tear, fold or lose the pole ears during operation. These defects will not only affect the performance of the battery cell, but may also become a hidden danger to battery safety. If a pole ear in the battery cell has a defect, it may cause uneven current distribution, which in turn may cause serious consequences such as short circuit, overheating or even explosion inside the battery.

[0004] In the related art, the methods for detecting defects in the tabs in assembled battery cells are usually X-Ray detection, CCD (Charge-coupled Device) detection and manual detection. These means can, to a certain extent, screen out battery cells with tab defects through parameters such as abnormal tab morphology and poor alignment from the process end. However, these detection methods are relatively complex, require high equipment accuracy, and have a high misjudgment rate. Summary of the invention

[0005] In view of this, the present invention aims to propose a method for detecting defects in battery cell tabs, so as to optimize the method for detecting defects in battery cell tabs and reduce the misjudgment rate of tab defect detection.

[0006] To achieve the above object, the technical solution of the present invention is achieved as follows:

[0007] A method for detecting defects in a battery cell tab, the method comprising:

[0008] Obtaining a first electrical performance parameter of the battery cell to be tested;

[0009] Comparing the first electrical performance parameter of the battery cell to be tested with the first standard electrical performance parameter threshold of a standard battery cell;

[0010] If the first electrical performance parameter of the battery cell to be tested exceeds the first standard electrical performance parameter threshold of the standard battery cell, the battery cell to be tested has a tab defect, and the battery cell to be tested with the tab defect is defined as a problematic battery cell;

[0011] Establishing a defect assessment model according to the first standard electrical performance parameters and the second standard electrical performance parameters of the standard battery cell;

[0012] Obtaining a second electrical performance parameter of the problematic battery cell;

[0013] Substitute the first electrical performance parameter and the second electrical performance parameter of the problematic battery cell into the defect assessment model, calculate the difference between the first electrical performance parameter of the problematic battery cell and the first standard electrical performance parameter, and the difference between the second electrical performance parameter of the problematic battery cell and the second standard electrical performance parameter, and assess the degree of tab defect of the problematic battery cell.

[0014] Furthermore, the first electrical performance parameter is the leakage current value I 漏 , any one of the fully charged shelf capacity loss ΔC, the fully charged shelf voltage drop ΔV or the DC internal resistance value R, wherein the second electrical performance parameter includes the leakage current value I 漏 , the remaining three items among the fully charged shelve capacity loss ΔC, the fully charged shelve voltage drop ΔV and the DC internal resistance value R.

[0015] Further, the establishing of the defect assessment model includes calculating the difference between the first electrical performance parameter of the problematic battery cell to be substituted and the first standard electrical performance parameter of the standard battery cell, and dividing the obtained difference by the first standard electrical performance parameter of the standard battery cell to obtain a ratio P1;

[0016] Difference is calculated between the second electrical performance parameter of the problematic battery cell to be substituted and the second standard electrical performance parameter of the corresponding standard battery cell, and the obtained difference is divided by the second standard electrical performance parameter of the corresponding standard battery cell to obtain ratios P2, P3, and P4;

[0017] Create a scoring table;

[0018] Compare P1, P2, P3, and P4 with the scoring table and assign points, then add up the scores to get the total score.

[0019] Further, obtaining the first electrical performance parameter and the second electrical performance parameter includes:

[0020] The problematic battery cell is charged at a standard rate with constant current and constant voltage, and then discharged at a constant voltage, and the capacity value is tested. Five cycles constitute one cycle.

[0021] If the capacity values ​​of the last two cycles of a cycle differ by less than 0.5%, the capacity value measured in the last cycle of the cycle is the stable capacity value C1;

[0022] If the capacity values ​​of the last two cycles of a cycle differ by more than or equal to 0.5%, the cycle is repeated until the stable capacity value C1 is measured;

[0023] Leave the problematic battery cell alone for three to ten days;

[0024] The problematic battery cell is charged at a standard rate, constant current and constant voltage, and then discharged at a constant voltage, and the capacity value C2 after standing is measured. The fully charged shelving capacity loss ΔC=C1-C2.

[0025] Further, obtaining the first electrical performance parameter and the second electrical performance parameter includes:

[0026] The fixed capacity battery is charged at a standard rate and constant current to the charging cut-off voltage;

[0027] Continuously charge the problematic cell with multiple currents of decreasing current values ​​to the charging cut-off voltage, and continue to charge the problematic cell at a constant voltage at the charging cut-off voltage, monitor the change of the current value of the problematic cell, and when the current value of the problematic cell continuously decreases to a constant value, this current value is the leakage current value I of the problematic cell 漏 .

[0028] Furthermore, the value range of the successively decreasing current value is 1 mA to 200 mA.

[0029] Further, obtaining the first electrical performance parameter and the second electrical performance parameter includes:

[0030] The problematic battery cell is charged at a standard rate constant current and constant voltage until the charging cut-off voltage V is reached;

[0031] Leave the problematic battery cell alone for three to ten days;

[0032] After measuring the voltage V of the problematic battery cell, the fully charged shelf voltage drop ΔV=Vbefore-Vafter.

[0033] Further, obtaining the first electrical performance parameter and the second electrical performance parameter includes:

[0034] A 100% charging rate test is performed on the problematic battery cell to measure the DC internal resistance R of the problematic battery cell.

[0035] Compared with the prior art, the present invention has the following advantages:

[0036] The method for detecting defects in the battery cell tabs of the present invention measures a first electrical performance parameter of the battery cell to be tested, compares it with the first standard electrical performance parameter threshold of the standard battery cell, determines whether the battery cell to be tested has a tab defect, and then inputs the first electrical performance parameter and the second electrical performance parameter of the problematic battery cell with the tab defect and the first standard electrical performance parameter and the second standard electrical performance parameter of the standard battery cell into a defect assessment model to obtain the degree of the specific battery cell tab defect. The degree of the tab defect can be obtained by processing the electrical performance signal of the battery cell. Compared with traditional appearance inspection, the method of collecting electrical performance signals has a low misjudgment rate, lower equipment requirements, and easier detection steps. The collected electrical signals can also be used to upgrade BMS algorithms, serve battery manufacturing related processes, and improve the production yield of battery cells.

[0037] Leakage current value I 漏 , full-charge shelf capacity loss ΔC, full-charge shelf voltage drop ΔV and DC internal resistance R, these four values ​​can reflect the defects of the tabs. Superimposing these four variable factors can improve the accuracy of detection.

[0038] By assigning points to the calculated P1, P2, P3, and P4 and summing them up, the total score can better reflect the actual defects of the tabs. The higher the score, the more serious the tab defects.

[0039] By comparing the capacity value after telecommunication capacity setting with the capacity value after static condition, the ΔC obtained is more accurate and better expresses the tab defects.

[0040] Charging the problematic battery cells with decreasing current values ​​can achieve a higher charging rate of the battery cells. Then, charging the problematic battery cells at a constant voltage with a cut-off voltage can obtain a more accurate leakage current value after the current value tends to stabilize, which is more effective in expressing the tab defects.

[0041] Setting the decreasing current value to 1mA to 200mA can charge the problematic battery cell to a higher capacity.

[0042] By charging the problematic battery cell to the charging cut-off voltage, letting it stand, and then measuring the voltage of the problematic battery cell, the resulting voltage drop is relatively stable and can more accurately express the defects of the battery cell tabs.

[0043] The 100% charging rate test can measure the DC internal resistance of the problematic battery cell more accurately and better express the defects of the tabs of the problematic battery cell.

[0044] Another object of the present invention is to provide a battery cell tab defect detection device, the detection device comprising a first acquisition module, a first processing module, a second processing module, a second acquisition module and an evaluation module;

[0045] The first acquisition module is used to acquire the first electrical performance parameter of the battery cell to be tested and input it into the first processing module;

[0046] The first processing module is used to compare the first electrical performance parameter of the battery cell to be tested with the first standard electrical performance parameter threshold of the standard battery cell to determine whether the battery cell to be tested is a problematic battery cell. If the battery cell to be tested is a problematic battery cell, the first electrical performance parameter of the battery cell to be tested is input into the evaluation module;

[0047] The second processing module is used to obtain a defect assessment model according to the first standard electrical performance parameter and the second standard electrical performance parameter;

[0048] The second acquisition module is used to acquire the second electrical performance parameter of the problematic battery cell and input it into the defect assessment model;

[0049] The evaluation module is used to evaluate the defect degree of the problematic battery cell tab.

[0050] The battery cell tab defect detection device described in the present invention can perform electrical performance tests on battery cells and derive defects in the tabs within the battery cells after comparison with standard battery cells. It has a low misjudgment rate, low requirements on equipment accuracy, and easier detection steps.

[0051] Another object of the present invention is to provide a computer-readable storage medium, on which a program or instruction is stored. When the program or instruction is executed by a processor, the battery cell tab defect detection method as described above can be implemented.

[0052] The computer-readable storage medium described in the present invention has the same beneficial effects as the battery cell tab defect detection method described above, and will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:

[0054] Figure 1 This is a flow chart of a method for detecting defects in a battery cell tab according to an embodiment of the present invention;

[0055] Figure 2 A method for detecting the first standard electrical performance parameter and the second standard electrical performance parameter of a standard battery cell according to an embodiment of the present invention;

[0056] Figure 3 It is a numerical comparison diagram of battery cell 1, battery cell 2, battery cell 3 and a standard battery cell in the first embodiment of the present invention;

[0057] Figure 4It is a schematic diagram of the structure of the battery cell tab defect detection device in the second embodiment of the present invention.

[0058] Description of reference numerals:

[0059] 100. Detection device;

[0060] 101. First acquisition module; 102. First processing module; 103. Second processing module; 104. Second acquisition module; 105. Evaluation module. DETAILED DESCRIPTION

[0061] In the following description, specific details such as specific system structures, technologies, etc. are provided for the purpose of illustration rather than limitation, so as to provide a thorough understanding of the embodiments of the present application. However, it should be clear to those skilled in the art that the present application may also be implemented in other embodiments without these specific details. In other cases, detailed descriptions of well-known systems, devices, circuits, and methods are omitted to prevent unnecessary details from obstructing the description of the present application.

[0062] It should be understood that when used in the present specification and the appended claims, the term "comprising" indicates the presence of described features, wholes, steps, operations, elements and / or components, but does not exclude the presence or addition of one or more other features, wholes, steps, operations, elements, components and / or combinations thereof.

[0063] It should also be understood that the term “and / or” used in the specification and appended claims refers to any and all possible combinations of one or more of the associated listed items, and includes these combinations.

[0064] As used in the specification and appended claims of this application, the term "if" can be interpreted as "when" or "uponce" or "in response to determining" or "in response to detecting", depending on the context. Similarly, the phrase "if it is determined" or "if [described condition or event] is detected" can be interpreted as meaning "uponce it is determined" or "in response to determining" or "uponce [described condition or event] is detected" or "in response to detecting [described condition or event]", depending on the context.

[0065] In addition, in the description of the present application specification and the appended claims, the terms "first", "second", "third", etc. are only used to distinguish the descriptions and cannot be understood as indicating or implying relative importance.

[0066] References to "one embodiment" or "some embodiments" etc. described in the specification of this application mean that one or more embodiments of the present application include specific features, structures or characteristics described in conjunction with the embodiment. Therefore, the statements "in one embodiment", "in some embodiments", "in some other embodiments", "in some other embodiments", etc. that appear in different places in this specification do not necessarily refer to the same embodiment, but mean "one or more but not all embodiments", unless otherwise specifically emphasized in other ways. The terms "including", "comprising", "having" and their variations all mean "including but not limited to", unless otherwise specifically emphasized in other ways.

[0067] The present invention will be described in detail below with reference to the accompanying drawings and in conjunction with embodiments.

[0068] Embodiment 1

[0069] The present embodiment relates to a method for detecting defects in a battery cell tab, which collects electrical performance signals from the battery cell, processes and compares the electrical performance signals, and thereby evaluates the degree of tab defects inside the battery cell.

[0070] Before describing the battery cell tab defect detection method of this embodiment, it is necessary to briefly introduce the battery cell tab. The tab is the current collector, which is usually made of micron-sized aluminum foil and copper foil. In key processes such as tab welding and electrode assembly shelling, due to the micron-sized size and fragile physical properties of aluminum foil and copper foil, it is easy to cause defects such as tearing, folding or falling off of the tab during operation. In terms of the degree of defects, tearing < folding < falling off.

[0071] Therefore, based on the above introduction, combined with Figure 1 As shown, in terms of overall design, the power battery evaluation method of this embodiment includes the following steps.

[0072] Step S1, obtaining a first electrical performance parameter of a battery cell to be tested.

[0073] Step S2: Compare the first electrical performance parameter of the cell to be tested with the first standard electrical performance parameter threshold of the standard cell. If the first electrical performance parameter of the cell to be tested exceeds the first standard electrical performance parameter threshold of the standard cell, the cell to be tested has a tab defect, and the cell to be tested with the tab defect is defined as a defective cell.

[0074] Step S3: establishing a defect assessment model according to the first standard electrical performance parameter and the second standard electrical performance parameter of the standard battery cell.

[0075] Step S4: Obtain a second electrical performance parameter of the problematic battery cell.

[0076] Step S5, substitute the first electrical performance parameter and the second electrical performance parameter of the problem battery cell into the defect assessment model, calculate the difference between the first electrical performance parameter of the problem battery cell and the first standard electrical performance parameter, and the difference between the second electrical performance parameter of the problem battery cell and the second standard electrical performance parameter, and evaluate the degree of tab defect of the problem battery cell.

[0077] The battery cell tab defect detection method of the present embodiment measures a first electrical performance parameter of the battery cell to be tested, compares it with the first standard electrical performance parameter threshold of the standard battery cell, determines whether the battery cell to be tested has a tab defect, and then inputs the first electrical performance parameter and the second electrical performance parameter of the problematic battery cell with the tab defect and the first standard electrical performance parameter and the second standard electrical performance parameter of the standard battery cell into a defect assessment model to obtain the degree of the specific battery cell tab defect. The tab defect degree can be obtained by processing the electrical performance signal of the battery cell. Compared with traditional appearance inspection, the method of collecting electrical performance signals has a low misjudgment rate, lower equipment requirements, and easier detection steps. The collected electrical signals can also be used to upgrade BMS (Battery Management System) algorithms, serve battery manufacturing related processes, and improve the production yield of battery cells.

[0078] Among them, in step S1, the first electrical performance parameter is the leakage current value I 漏 , full-charge shelf capacity loss ΔC, full-charge shelf voltage drop ΔV or DC internal resistance R, these four parameters can play a certain role in expressing the tab defects in the battery cell. 漏 As the first electrical performance parameter, the leakage current I 漏 Compared with the other three parameters, it has a stronger ability to express the defects of the tabs. As for the test method of leakage current, any existing test method can be used.

[0079] Secondly, in step S2, the first standard electrical performance parameter corresponds to the first electrical performance parameter, which is the standard leakage current I 漏标 The first standard electrical performance parameter threshold is a design value of the battery cell when it is designed. When the working condition in the battery cell is normal, the first electrical performance parameter is less than the first standard electrical performance parameter threshold. The full-charged shelving capacity loss ΔC, the full-charged shelving voltage drop ΔV and the DC internal resistance value R are the second electrical performance parameters of the problematic battery cell.

[0080] Among them, in step S3, corresponding to the second electrical performance parameter, the second standard electrical performance parameter is the full-charge storage capacity loss ΔC of the standard battery cell 标 , Fully charged voltage drop ΔV 标 And the DC internal resistance R 标 The method for obtaining the first standard electrical performance parameter and the second standard electrical performance parameter is:

[0081] The standard battery cell is charged at a standard rate with constant current and constant voltage, and then discharged at a constant voltage to detect the capacity value. Five cycles are considered a cycle. If the capacity value of the last two cycles of a cycle differs by less than 0.5%, the capacity value measured in the last cycle of the cycle is the stable capacity value C1 标 If the capacity value difference between the last two cycles of a cycle is greater than or equal to 0.5%, repeat the cycle until a stable capacity value C1 is measured. 标 The total number of cycles of the standard battery cell shall not exceed fifteen cycles. Exceeding fifteen cycles may affect the accuracy of the capacity test. 标 , replace the standard battery cell and test again.

[0082] The standard battery cell after the cycle is charged at a standard rate constant current to the charge cut-off voltage. The standard battery cell is charged to the charge cut-off voltage at multiple currents with decreasing current values ​​in sequence, and the standard battery cell is charged at a constant voltage at the charge cut-off voltage. The current value change of the standard battery cell is monitored. When the current value of the standard battery cell continuously decreases to a constant value, this current value is the leakage current value I of the standard battery cell. 漏标 The value range of the decreasing current value is 1 mA to 200 mA, preferably 200 mA, 100 mA, 50 mA, 10 mA, 5 mA, and 1 mA.

[0083] Charge the standard battery at a standard rate with constant current and constant voltage until the charging cut-off voltage V 前标 The standard battery cell is left to stand for three to ten days. If it is less than three days, the test result is inaccurate. If it is more than ten days, although the test result is more accurate, it takes a long time and affects production efficiency. The voltage V of the standard battery cell is measured. 后标 , fully charged standby voltage drop ΔV 标 =V 前标 -V 后标 .

[0084] The standard battery cell after standing still is charged at a standard rate with constant current and constant voltage, and then discharged at a constant voltage, and the capacity value C2 after standing still is measured. 标 , Fully charged shelved capacity loss ΔC 标 =C1 标 -C2 标 .

[0085] Perform a 100% SOC (States of Charge) test on the problematic battery cell to measure the DCIR (Direct Current Internal Resistance) R of the problematic battery cell. 标 .

[0086] Take three to five standard batteries and perform the above test to obtain I 漏标 , ΔV 标 , ΔC标 and R 标 The average value is used as the first standard electrical performance parameter and the second standard electrical performance parameter.

[0087] Preferably, step S3 further includes the following steps:

[0088] S31, the first electrical performance parameter of the problematic battery cell to be substituted is calculated to be different from the first standard electrical performance parameter of the standard battery cell, and the obtained difference is divided by the first standard electrical performance parameter of the standard battery cell to obtain a ratio P1, P1=(I 漏 -I 漏标 ) / I 漏标 .

[0089] S32, the second electrical performance parameter of the problematic battery cell to be substituted is calculated from the second standard electrical performance parameter of the corresponding standard battery cell, and the difference is divided by the second standard electrical performance parameter of the corresponding standard battery cell to obtain ratios P2, P3, and P4. The second standard electrical performance parameter is the full-charged storage capacity loss ΔC of the standard battery cell. 标 , Fully charged voltage drop ΔV 标 And the DC internal resistance R 标 , P2=(ΔV-ΔV 标 ) / ΔV 标 , P3=(ΔC-ΔC 标 ) / ΔC 标 , P4=(RR 标 ) / R 标 .

[0090] S33. Create a scoring table, which is shown in Table 1.

[0091] Table 1:

[0092] ratio ≤20% 20%~40% 40~60% 60~80% >80% P1 0 1 2 3 4 P2 0 1 2 3 4 P3 0 1 2 3 4 P4 0 1 2 3 4

[0093] S44. Compare P1, P2, P3, and P4 with Table 1 and assign points, and sum up the points to get the total score.

[0094] Preferably, in step S4, the second electrical performance parameter test method of the problematic battery cell is a test method for the full-charge shelf capacity loss ΔC, the full-charge shelf voltage drop ΔV and the DC internal resistance R, which is different from the test method for the full-charge shelf capacity loss ΔC of the standard battery cell. 标 , Fully charged voltage drop ΔV 标 And the DC internal resistance R 标 The test method is the same as that of the first embodiment, and the measured second electrical performance parameter is more accurate.

[0095] Preferably, in step S5, Table 2 for evaluating the total score of the problematic battery cells is obtained according to experiments.

[0096] Table 2:

[0097]

[0098] Compare the total score of the problematic battery cells with Table 2 to get the tab defect level corresponding to the problematic battery cells. It should be noted that when the total scores of the battery cells of the same batch are concentrated in a certain area in Table 2, ten battery cells with total scores in this area are selected, and these ten battery cells are disassembled to check the specific tab defects. The most common defect level is defined as the tab defect level of the battery cells with total scores in this area.

[0099] It should also be noted that for battery cells with the same score, the single score of the leakage current is compared. The larger the score, the greater the degree of the tab defect.

[0100] The following is an example of the specific implementation of the battery cell tab defect detection method of this embodiment.

[0101] In the production of battery cells, three problematic battery cells with tab defects were found through leakage current detection. The three problematic battery cells were numbered as battery cell 1, battery cell 2, and battery cell 3, and their leakage current I was obtained. 漏 , full-charge shelf voltage drop ΔV, full-charge shelf capacity loss ΔC and DCIR DC internal resistance R, and leakage current I of standard battery cells 漏标 , Fully charged voltage drop ΔV 标 , Fully charged shelved capacity loss ΔC 标 DCIR DC internal resistance R 标 For example Figure 3 As shown, the total score is obtained through the defect assessment model, and combined with Table 2, the results in Table 3 are obtained.

[0102] Table 3

[0103] Voltage drop ΔV ΔC <![CDATA[I 漏 ]]> R Total score determination Battery 1 1 0 1 1 3 Minor tear Battery 2 3 2 2 1 8 Folding ear Battery 3 3 3 4 4 14 Tabs fall off

[0104] Cell 1, cell 2, and cell 3 were disassembled, and the actual tab defect levels of cell 1, cell 2, and cell 3 were the same as the results in Table 3.

[0105] This embodiment can obtain the degree of tab defects by processing the electrical performance signals of the battery cell. Compared with the traditional appearance inspection, the method of collecting electrical performance signals has a low misjudgment rate, low equipment requirements, and easier inspection steps. The collected electrical signals can also be used to upgrade the BMS algorithm, serve battery manufacturing related processes, and improve the production yield of battery cells.

[0106] Embodiment 2

[0107] This embodiment relates to a battery cell tab defect detection device (hereinafter referred to as "detection device 100"), which is based on the battery cell tab defect detection method in the first embodiment. Figure 4 As shown, in terms of overall structure, the detection device 100 of this embodiment includes a first acquisition module 101 , a first processing module 102 , a second processing module 103 , a second acquisition module 104 and an evaluation module 105 .

[0108] The first acquisition module 101 is used to acquire a first electrical performance parameter of the battery cell to be tested and input the first electrical performance parameter into the first processing module 102 .

[0109] The first processing module 102 is used to compare the first electrical performance parameter of the battery cell to be tested with the first standard electrical performance parameter threshold of the standard battery cell to determine whether the battery cell to be tested is a problematic battery cell. If the battery cell to be tested is a problematic battery cell, the first electrical performance parameter of the battery cell to be tested is input into the evaluation module 105.

[0110] The second processing module 103 is used to obtain a defect assessment model according to the first standard electrical performance parameter and the second standard electrical performance parameter.

[0111] The second acquisition module 104 is used to acquire the second electrical performance parameter of the problematic battery cell and input it into the defect assessment model.

[0112] The evaluation module 105 is used to evaluate the degree of defects of the tabs of the problematic battery cells.

[0113] The detection device 100 of this embodiment, when used specifically, the corresponding detection method can refer to the relevant description in the first embodiment. Moreover, the detection device 100 of this embodiment can obtain the degree of tab defects by processing the electrical performance signal of the battery cell. Compared with the traditional appearance inspection, the method of collecting electrical performance signals has a low misjudgment rate, low equipment requirements, and easier detection steps. The collected electrical signals can also be used to upgrade the BMS algorithm, serve battery manufacturing related processes, and improve the production yield of battery cells.

[0114] Embodiment 3

[0115] The present embodiment relates to a computer-readable storage medium, which stores a computer program. When the computer program is executed by a processor, the method for detecting defects in a battery cell tab in the first embodiment can be implemented.

[0116] The computer-readable storage medium of this embodiment is generally a memory, and includes permanent and non-permanent, removable and non-removable media, and can implement information storage by any method or technology.

[0117] In addition, the above information can be computer-readable instructions, data structures, modules of programs or other data. Examples of computer-readable storage media include, but are not limited to, phase change memory (PRAM), static random access memory (SRAM), dynamic random access memory (DRAM), other types of random access memory (RAM), read-only memory (ROM), electrically erasable programmable read-only memory (EEPROM), flash memory, or other memory technology, compact disk read-only memory (CD-ROM), digital versatile disk (DVD) or other optical storage, magnetic cassettes, magnetic tape, disk storage or other magnetic storage devices, or any other non-transmission media that can be used to store information that can be accessed by a computing device.

[0118] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for detecting defects in a battery cell tab, characterized in that: The test method includes: Obtaining a first electrical performance parameter of the battery cell to be tested; Comparing the first electrical performance parameter of the battery cell to be tested with the first standard electrical performance parameter threshold of a standard battery cell; If the first electrical performance parameter of the battery cell to be tested exceeds the first standard electrical performance parameter threshold of the standard battery cell, the battery cell to be tested has a tab defect, and the battery cell to be tested with the tab defect is defined as a problematic battery cell; Establishing a defect assessment model according to the first standard electrical performance parameters and the second standard electrical performance parameters of the standard battery cell; Obtaining a second electrical performance parameter of the problematic battery cell; Substitute the first electrical performance parameter and the second electrical performance parameter of the problematic battery cell into the defect assessment model, calculate the difference between the first electrical performance parameter of the problematic battery cell and the first standard electrical performance parameter, and the difference between the second electrical performance parameter of the problematic battery cell and the second standard electrical performance parameter, and assess the degree of tab defect of the problematic battery cell.

2. The method for detecting defects in a battery cell tab according to claim 1, characterized in that: The first electrical performance parameter is the leakage current value I 漏 , any one of the fully charged shelf capacity loss ΔC, the fully charged shelf voltage drop ΔV or the DC internal resistance value R, wherein the second electrical performance parameter includes the leakage current value I 漏 , the remaining three items among the fully charged shelve capacity loss ΔC, the fully charged shelve voltage drop ΔV and the DC internal resistance value R.

3. The method for detecting defects in battery tabs according to claim 2, characterized in that: The step of establishing a defect assessment model comprises: Difference is calculated between the first electrical performance parameter of the problematic battery cell and the first standard electrical performance parameter of the standard battery cell, and the difference is divided by the first standard electrical performance parameter of the standard battery cell to obtain a ratio P1; Difference is calculated between the second electrical performance parameter of the problematic battery cell to be substituted and the second standard electrical performance parameter of the corresponding standard battery cell, and the obtained difference is divided by the second standard electrical performance parameter of the corresponding standard battery cell to obtain ratios P2, P3, and P4; Create a scoring table; Compare P1, P2, P3, and P4 with the scoring table and assign points, then add up the scores to get the total score.

4. The method for detecting defects in battery tabs according to claim 3, characterized in that: Acquiring the first electrical performance parameter and the second electrical performance parameter includes: The problematic battery cell is charged at a standard rate with constant current and constant voltage, and then discharged at a constant voltage, and the capacity value is tested. Five cycles constitute one cycle. If the capacity values ​​of the last two cycles of a cycle differ by less than 0.5%, the capacity value measured in the last cycle of the cycle is the stable capacity value C1; If the capacity values ​​of the last two cycles of a cycle differ by more than or equal to 0.5%, the cycle is repeated until the stable capacity value C1 is measured; Leave the problematic battery cell alone for three to ten days; The problematic battery cell is charged at a standard rate, constant current and constant voltage, and then discharged at a constant voltage, and the capacity value C2 after standing is measured. The fully charged shelving capacity loss ΔC=C1-C2.

5. The method for detecting defects in battery tabs according to claim 3, characterized in that: Acquiring the first electrical performance parameter and the second electrical performance parameter includes: The fixed capacity battery is charged at a standard rate and constant current to the charging cut-off voltage; Continuously charge the problematic cell with multiple currents of decreasing current values ​​to the charging cut-off voltage, and continue to charge the problematic cell at a constant voltage at the charging cut-off voltage, monitor the change of the current value of the problematic cell, and when the current value of the problematic cell continuously decreases to a constant value, this current value is the leakage current value I of the problematic cell 漏 .

6. The method for detecting defects in a battery cell tab according to claim 5, characterized in that: The value range of the successively decreasing current value is 1 mA to 200 mA.

7. The method for detecting defects in battery tabs according to claim 3, characterized in that: Acquiring the first electrical performance parameter and the second electrical performance parameter includes: The problematic cell is charged at a standard rate with constant current and constant voltage until the charging cut-off voltage V 前 ; Leave the problematic battery cell alone for three to ten days; After measuring the voltage V of the problematic cell, the fully charged standby voltage drop ΔV = V 前 -V 后 .

8. The method for detecting defects in battery tabs according to claim 3, characterized in that: Acquiring the first electrical performance parameter and the second electrical performance parameter includes: A 100% charging rate test is performed on the problematic battery cell to measure the DC internal resistance R of the problematic battery cell.

9. A battery cell tab defect detection device, characterized in that: The detection device comprises a first acquisition module, a first processing module, a second processing module, a second acquisition module and an evaluation module; The first acquisition module is used to acquire the first electrical performance parameter of the battery cell to be tested and input it into the first processing module; The first processing module is used to compare the first electrical performance parameter of the battery cell to be tested with the first standard electrical performance parameter threshold of the standard battery cell to determine whether the battery cell to be tested is a problematic battery cell. If the battery cell to be tested is a problematic battery cell, the first electrical performance parameter of the battery cell to be tested is input into the evaluation module; The second processing module is used to obtain a defect assessment model according to the first standard electrical performance parameter and the second standard electrical performance parameter; The second acquisition module is used to acquire the second electrical performance parameter of the problematic battery cell and input it into the defect assessment model; The evaluation module is used to evaluate the defect degree of the problematic battery cell tab.

10. A computer-readable storage medium, characterized in that: The computer-readable storage medium stores programs or instructions, and when the programs or instructions are executed by the processor, the battery cell tab defect detection method as described in any one of claims 1 to 8 can be implemented.

Citation Information

Cited By

  • Secondary cell tab tearing detection method, device, battery, system and equipment

    CN120028391A

  • Battery tab abnormity screening method

    CN121410574A

  • A battery tab abnormality screening method

    CN121410574B