Garnet type structure coated ultrahigh nickel cobalt-free single crystal material and preparation method thereof
Ultra-high nickel cobalt-free single crystal material coated with garnet-type structure uses Fe, Al doping and garnet structural materials to solve the problem of poor circulation performance of cobalt-free positive electrode materials, achieving high cycle stability and low cost The lithium battery cathode material is suitable for industrial applications.
Patent Information
- Application Number
- CN202411472836.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-22
- Publication Date
- 2024-11-19
AI Technical Summary
Cobalt-free cathode material has degraded cyclic performance in lithium batteries due to the cation mixing problem, and the scarcity and high cost of cobalt are an important technical challenge.
Ultra-high nickel cobalt-free single crystal material coated with garnet structure was developed through Fe, Al doping and garnet structure materials to collaborate the coating and modify LiNixMn1-x-yAyO2·Li7-nLa3Zr2-n(Nb +Ta)nO12 positive electrode material, garnet-type coated substances are used to improve the structural performance and cycle stability of the material.
It achieves high cycle stability and good rate performance, reduces material costs, is suitable for industrial production, and is better than traditional core-shell structural designs.
Smart Images

Figure CN118983427A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium-ion batteries, and in particular to an ultra-high nickel cobalt-free single crystal material coated with a garnet-type structure and a preparation method thereof. Background Art
[0002] With the popularization and continuous promotion of new energy vehicles, lithium-ion batteries as a power source have developed rapidly, and the requirements for lithium battery performance have also been continuously improved. As the commonly used lithium battery positive electrode material, ternary cathode materials have the advantages of high energy density and good cycle performance. However, due to the scarcity and strategic value of cobalt, the price is expensive, making the cost of ternary materials higher than that of other lithium battery positive electrode materials. Therefore, the development of cobalt-free cathode materials is of great significance.
[0003] In ternary cathode materials, cobalt can prevent cation mixing (Ni 2+ and Li + The mixing of cations in the material is more obvious, which reduces the battery cycle performance. Summary of the invention
[0004] The purpose of the present invention is to provide a garnet-type structure coated ultra-high nickel cobalt-free single crystal material and a preparation method thereof, and a garnet-type structure coated ultra-high nickel cobalt-free single crystal positive electrode material LiNi is developed by using Fe, Al doping and garnet structure material for coating synergistic modification. x Mn 1-x-y A y O2·Li 7-n Ln3Z 2-n (Nb+Ta) n O 12 , has high cycle stability performance, and its preparation method is easy to operate, simple process, and has commercial application value. The structural design of the crystal is achieved through garnet-type coating material, which is better than the core-shell structure and other structural designs of positive electrode materials currently carried out in academia and industry, thereby improving the structural performance of the single crystal, and is beneficial to improving the cycle stability and good rate performance of cobalt-free materials.
[0005] To achieve the above purpose, the present invention provides a garnet-type structure-coated ultra-high nickel cobalt-free single crystal material, which is a positive electrode material for a battery and is sintered by a precursor and a lithium source, and has a chemical formula of LiNi x Mn 1-x-y A y O2·Li 7-n Ln3Z 2-n (Nb+Ta) n O12 ; Wherein A is Fe, Al, Y or Zr element, x, y and n are molar numbers, x≥0.9, y≤0.05 and n≤0.3.
[0006] Preferably, the particle size of the precursor is 2-5 μm, and the chemical formula of the precursor is Ni x Mn 1-x-y A y (OH)2, wherein A is Fe, Al, Y or Zr element, x and y are molar numbers, x≥0.9, y≤0.05.
[0007] Preferably, the positive electrode material is a hexagonal α-NaFeO2 rock salt structure, and its space group is R-3m The particle size of the positive electrode material is 2-5 μm, and its surface is dotted with a coating material. The coating material is a garnet-type structure with a particle size of 5-100 nm.
[0008] The present invention provides a method for preparing an ultra-high nickel cobalt-free single crystal material coated with a garnet-type structure, comprising the following steps: Step 1: Mix soluble nickel salt, manganese salt and soluble salt of doping element according to a certain stoichiometric ratio and add deionized water to prepare a metal salt solution, add a precipitant into deionized water to dissolve to prepare a precipitant solution, and dilute the complexing agent to a certain concentration to prepare a complexing agent solution; Step 2: Heat the metal salt solution, the complexing agent solution and the precipitant solution separately, inject them into the reaction kettle and introduce the protective gas, then keep warm and stir to carry out the coprecipitation reaction, filter while hot, and finally wash the filtered precipitate with deionized water and vacuum dry it to obtain the precursor Ni x Mn 1-x-y A y (OH)2; Step 3: fully mix the lithium source and the precursor in step 2 in a high-speed mixer according to a certain ratio to obtain a mixture A; Step 4: Place the mixture A in step 3 into an atmosphere furnace for calcination. After calcination, cool, jet mill, and sieve to obtain the positive electrode material LiNi to be coated. x Mn 1-x-y A y O2; Step 5: The garnet-type coating material and the positive electrode material in step 4 are mixed in a high-speed mixer in a certain ratio to obtain a mixture B; Step 6: Place the mixture B in step 5 into an atmosphere furnace for calcination. After calcination, cool and sieve to obtain the positive electrode material LiNi x Mn 1-x-y Ay O2·Li 7-n Ln3Z 2-n (Nb+Ta) n O 12 .
[0009] Preferably, the nickel salt in step 1 is one or more of nickel sulfate, nickel nitrate and nickel chloride, the manganese salt is one or more of manganese sulfate, manganese nitrate and manganese chloride, the precipitant is one or more of sodium hydroxide, sodium carbonate, sodium bicarbonate, potassium hydroxide, potassium carbonate and potassium bicarbonate, the complexing agent is one or more of ammonia water and oxalic acid, the total concentration of metal cations in the metal salt solution is 3-10 mol / L, the concentration of the precipitant solution is 5-7 mol / L, and the concentration of the complexing agent solution is 1.5-2 mol / L.
[0010] Preferably, the heating temperature in step 2 is 40-80°C, the protective gas is one or more of N2 and Ar, the stirring speed is 200-500rpm, the pH is 10.5-11.0, and the vacuum drying temperature is 120-180°C.
[0011] Preferably, the lithium source in step three is one or more of lithium carbonate, lithium hydroxide, lithium hydroxide monohydrate, lithium nitrate, lithium chloride and lithium sulfate, the molar ratio of lithium element in the lithium source to the metal element in the precursor is Li:M=1.05-1.35, the speed of the high-speed mixer is 200-500rpm, the mixing time is 10-40min, and the volume of the mixed material does not exceed 1 / 3 of the volume of the high-speed mixer.
[0012] Preferably, the atmosphere in the atmosphere furnace in step 4 is nitrogen, oxygen or a mixed atmosphere of the two, and a two-step roasting process is adopted during roasting, including a first-stage roasting and a second-stage roasting, the first-stage roasting process conditions are a heat treatment at 200-600°C for 1-6h, and the second-stage roasting process conditions are a heat treatment at 700-1000°C for 5-30h; the heating rates of the first-stage roasting process and the second-stage roasting process are both 2°C / min-10°C / min, and the cooling method is natural cooling to room temperature.
[0013] Preferably, in step 5, the garnet-type coating material and LiNi x Mn 1-x-y A y The mass ratio of O2 does not exceed 5%, the speed of the high-speed mixer is 200-500rpm, the mixing time is 10-40min, and the mixed material does not exceed 1 / 3 of the volume of the high-speed mixer.
[0014] Preferably, the heating gas in the atmosphere furnace in step six is nitrogen, oxygen or a mixed atmosphere of the two, the roasting process is a heat treatment at 300-600°C for 5-30h, the heating rate is 2°C / min-10°C / min, and the cooling method is natural cooling to room temperature.
[0015] The soluble salt containing nickel, manganese and doping elements is mixed and added into deionized water, and the precursor Ni is obtained by coprecipitation method. x Mn 1-x-y A y The precursor and the lithium source are mixed evenly in a high-speed mixer, and then calcined, cooled, crushed and sieved to obtain the positive electrode material LiNi to be coated. x Mn 1-x-y A y O2, then the garnet-type coating material is mixed with the above-mentioned positive electrode material in a high-speed mixer, and then roasted, cooled, crushed and sieved again to obtain a stable positive electrode material LiNi x Mn 1-x-y A y O2·Li 7- n Ln3Z 2-n (Nb+Ta) n O 12 The garnet-type structure-coated ultra-high nickel-free cobalt single crystal positive electrode material of the present invention has a good crystal structure, and a battery prepared using the garnet-type structure-coated ultra-high nickel-free cobalt single crystal positive electrode material as the positive electrode material has excellent electrochemical performance. The preparation method is simple and controllable, the cost is low, and the battery is suitable for industrial production.
[0016] Therefore, the present invention adopts the above-mentioned garnet-type structure-coated ultra-high nickel cobalt-free single crystal material and its preparation method, and solves the problem of high material cost by using elements with abundant reserves instead of expensive cobalt. At the same time, iron-aluminum doping and boride coating are used to prepare the positive electrode material with excellent cycle stability and good rate performance. The preparation method is simple to operate, low in cost, and has commercial application value.
[0017] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a SEM image of the precursor prepared in Example 1 of the ultra-high nickel cobalt-free single crystal material coated with a garnet-type structure and the preparation method thereof of the present invention; Figure 2 This is a SEM image of the positive electrode material prepared in Example 1 of the ultra-high nickel cobalt-free single crystal material coated with a garnet-type structure of the present invention and the preparation method thereof; Figure 3This is the XRD diagram of the positive electrode material prepared in Example 1 of the ultra-high nickel cobalt-free single crystal material coated with a garnet-type structure and the preparation method thereof of the present invention; Figure 4 The charge and discharge curves of the battery made of the positive electrode material prepared in Example 1 and Comparative Example 1 of the ultra-high nickel cobalt-free single crystal material coated with a garnet-type structure of the present invention and its preparation method at a voltage range of 3.0-4.3V and a rate of 0.1C; Figure 5 The battery made of the positive electrode material prepared in Example 1 of the ultra-high nickel cobalt-free single crystal material coated with a garnet-type structure and its preparation method and Comparative Example 1 has a rate performance in the voltage range of 3.0-4.3V. DETAILED DESCRIPTION
[0019] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.
[0020] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.
[0021] Example The present invention provides a garnet-type structure-coated ultra-high nickel cobalt-free single crystal material, which is a positive electrode material for a battery and is sintered by a precursor and a lithium source, and has a chemical formula of LiNi x Mn 1-x-y A y O2·Li 7-n Ln3Z 2-n (Nb+Ta) n O 12 ; Wherein A is an element such as Fe, Al, Y or Zr, x, y and n are molar numbers, x≥0.9, y≤0.05 and n≤0.3.
[0022] The particle size of the precursor is 2-5 μm, and the chemical formula of the precursor is Ni x Mn 1-x-y A y (OH)2, wherein A is an element such as Fe, Al, Y or Zr, x and y are molar numbers, x≥0.9, y≤0.05.
[0023] The positive electrode material is a hexagonal α-NaFeO2 rock salt structure with a space group of R-3m The particle size of the positive electrode material is 2-5 μm, and its surface is dotted with coating materials. The coating materials have a garnet structure and a particle size of 5-100 nm.
[0024] The present invention also provides a method for preparing an ultra-high nickel cobalt-free single crystal material coated with a garnet-type structure, comprising the following steps: Step 1: Mix soluble nickel salt, manganese salt and soluble salt of doping element according to a certain stoichiometric ratio and add deionized water to prepare a metal salt solution, add a precipitant into deionized water to dissolve to prepare a precipitant solution, and dilute the complexing agent to a certain concentration to prepare a complexing agent solution; The nickel salt is one or more of nickel sulfate, nickel nitrate and nickel chloride, the manganese salt is one or more of manganese sulfate, manganese nitrate and manganese chloride, and the precipitant is one or more of sodium hydroxide, sodium carbonate, sodium bicarbonate, potassium hydroxide, potassium carbonate and potassium bicarbonate.
[0025] Nickel salts (such as nickel sulfate, nickel chloride, etc.) can increase the nickel content in the positive electrode material, thereby improving the energy density of the battery. The increase in the proportion of nickel can enable the battery to store more electrical energy and increase its endurance. The addition of manganese salts (such as manganese sulfate, manganese nitrate, etc.) can improve the structural stability and safety of the positive electrode material. Manganese helps to form a stable lattice structure, resisting structural changes caused during the charge and discharge cycle, thereby extending the battery life.
[0026] The complexing agent is one or more of ammonia water and oxalic acid, the total concentration of metal cations in the metal salt solution is 3-10 mol / L, the concentration of the precipitant solution is 5-7 mol / L, and the concentration of the complexing agent solution is 1.5-2 mol / L. The complexing agent can form a stable complex with the metal ions and can also improve the solubility of the metal salt. The precipitant can promote the pre-reaction of the metal ions in the solution to form a precipitate that is insoluble in water.
[0027] Step 2: Heat the metal salt solution, the complexing agent solution and the precipitant solution separately, inject them into the reaction kettle and introduce the protective gas, then keep warm and stir to carry out the coprecipitation reaction, filter while hot, and finally wash the filtered precipitate with deionized water and vacuum dry it to obtain the precursor Ni x Mn 1-x-y A y (OH)2; The heating temperature is 40-80°C, the protective gas is one or more of N2 and Ar, the stirring speed is 200-500rpm, the pH is 10.5-11.0, and the vacuum drying temperature is 120-180°C.
[0028] Step 3: fully mix the lithium source and the precursor in step 2 in a high-speed mixer according to a certain ratio to obtain a mixture A; The lithium source is one or more of lithium carbonate, lithium hydroxide, lithium hydroxide monohydrate, lithium nitrate, lithium chloride and lithium sulfate. The molar ratio of lithium element in the lithium source to the metal element in the precursor is Li:M=1.05-1.35. The speed of the high-speed mixer is 200-500rpm, the mixing time is 10-40min, and the volume of the mixed material does not exceed 1 / 3 of the volume of the high-speed mixer.
[0029] Step 4: Place the mixture A in step 3 into an atmosphere furnace for calcination. After calcination, cool, jet mill, and sieve to obtain the positive electrode material LiNi to be coated. x Mn 1-x-y A y O2; The atmosphere in the atmosphere furnace is nitrogen, oxygen or a mixture of the two. A two-step roasting process is adopted during roasting, including a first-stage roasting and a second-stage roasting. The first-stage roasting process conditions are a heat treatment at 200-600°C for 1-6h, and the second-stage roasting process conditions are a heat treatment at 700-1000°C for 5-30h. The heating rates of the first-stage roasting process and the second-stage roasting process are both 2°C / min-10°C / min, and the cooling method is natural cooling to room temperature.
[0030] Step 5: Garnet-type coating material and the positive electrode material in step 4 in a certain ratio, and are fully mixed in a high-speed mixer to obtain a mixture B; the garnet-type coating material and LiNi x Mn 1-x-y A y The mass ratio of O2 does not exceed 5%, the speed of the high-speed mixer is 200-500rpm, the mixing time is 10-40min, and the mixed material does not exceed 1 / 3 of the volume of the high-speed mixer.
[0031] Step 6: Place the mixture B in step 5 into an atmosphere furnace for calcination. After calcination, cool and sieve to obtain the positive electrode material LiNi x Mn 1-x-y A y O2·Li 7-n Ln3Z 2-n (Nb+Ta) n O 12 The heating gas in the atmosphere furnace is nitrogen, oxygen or a mixed atmosphere of the two, the roasting process is a heat treatment at 300-600°C for 5-30h, the heating rate is 2°C / min-10°C / min, and the cooling method is natural cooling to room temperature.
[0032] Example 1 A method for preparing an ultra-high nickel cobalt-free single crystal material coated with a garnet structure comprises the following steps: (1) Nickel sulfate, manganese sulfate, yttrium sulfate and deionized water are prepared into a 4 mol / L metal salt solution in which the molar ratio of Ni:Mn:Y is 94:5:1; 6.5 mol / L sodium hydroxide solution and 2 mol / L ammonia solution are then prepared; the solution is pumped into a reactor at a rate of metal salt solution: sodium hydroxide solution = 1:2, N2 is introduced into the reactor, the temperature in the reactor is 50°C, the reactor is kept warm, and the stirring speed is 500 r / min; after the reaction is complete, the solution is filtered while hot, the filtrate is washed with deionized water, and vacuum dried to obtain a precursor.
[0033] (2) Lithium carbonate and the metal element in the precursor are uniformly mixed at a molar ratio of Li:M=1.05:1 to obtain a mixture A.
[0034] (3) Mixture A is placed in an oxygen atmosphere and calcined using a two-step calcination process, including a first-stage calcination and a second-stage calcination. The process conditions for the first-stage calcination are: heat treatment at 300°C for 3 hours, and the process conditions for the second-stage calcination are: heat treatment at 850°C for 30 hours. The heating rate of the two calcination methods is 6°C / min. After calcination, it is cooled, jet milled, and sieved to obtain the positive electrode material LiNi to be coated. 0.94 Mn 0.05 Y 0.01 O2.
[0035] (4) Garnet-type coating material With LiNi 0.94 Mn 0.05 Y 0.01 O2 was mixed evenly at a mass ratio of 4.5% to obtain a mixture B, which was then calcined in an atmosphere furnace with an oxygen atmosphere. The temperature of the atmosphere furnace was 400°C, the heat treatment was performed for 15 hours, and the heating rate was 2°C / min. After calcination, the mixture was cooled and sieved to obtain the positive electrode material LiNi 0.94 Mn 0.05 Y 0.01 O2·Li 6.9 Ln3Z 1.9 (Nb+Ta) 0.1 O 12 .
[0036] (5) Test the discharge specific capacity of the ultra-high nickel cobalt-free single crystal material coated with the garnet structure at 0.1C and 10C.
[0037] Figure 1 This is the SEM image of the prepared precursor. It can be seen from the image that a spherical precursor was prepared. Figure 2This is the SEM image of the prepared positive electrode material. The SEM image shows the morphological characteristics of the positive electrode material, such as particle size, shape, distribution and surface structure. The particle size is about 1 micron, polyhedral in shape, densely distributed, and has fine texture and unevenness on the surface. Figure 3 This is the XRD diagram of the prepared positive electrode material. The XRD spectrum shows that the ultra-high nickel-free cobalt single crystal material coated with a garnet-type structure has good crystallinity, large grain size, and high crystal quality. These characteristics indicate that the material has good structural stability and electrochemical performance, and is suitable for use as a positive electrode material.
[0038] Example 2 A method for preparing an ultra-high nickel cobalt-free single crystal material coated with a garnet structure comprises the following steps: (1) Nickel sulfate, manganese sulfate, aluminum sulfate and deionized water are prepared into a 4 mol / L metal salt solution, wherein the molar ratio of Ni:Mn:Al is 94:5:1; 6.5 mol / L sodium hydroxide solution and 2 mol / L ammonia solution are then prepared; the solution is pumped into a reactor at a rate of 1:2, and N2 is introduced into the reactor. The temperature in the reactor is kept at 50°C and the stirring speed is 500 r / min. After the reaction is complete, the solution is filtered while hot, the filtrate is washed with deionized water, and vacuum dried to obtain a precursor.
[0039] (2) Lithium carbonate and the metal element in the precursor are uniformly mixed at a molar ratio of Li:M=1.05:1 to obtain a mixture A.
[0040] (3) Mixture A is placed in an oxygen atmosphere and calcined using a two-step calcination process, including a first-stage calcination and a second-stage calcination. The process conditions for the first stage calcination are: heat treatment at 550°C for 3 hours, and the process conditions for the second stage calcination are: heat treatment at 850°C for 30 hours. The heating rate of the two calcination methods is 2°C / min. After calcination, it is cooled, jet milled, and sieved to obtain the positive electrode material LiNi to be coated. 0.94 Mn 0.05 Al 0.01 O2.
[0041] (4) Garnet-type coating material With LiNi 0.94 Mn 0.05 Al 0.01 O2 was mixed evenly at a mass ratio of 4.5% to obtain a mixture B, which was then calcined in an atmosphere furnace with an oxygen atmosphere. The temperature of the atmosphere furnace was 400°C, the heat treatment was performed for 15 hours, and the heating rate was 2°C / min. After calcination, the mixture was cooled and sieved to obtain the positive electrode material LiNi 0.94 Mn 0.05 Al 0.01 O2·Li6.9 Ln3Z 1.9 (Nb+Ta) 0.1 O 12 .
[0042] (5) Test the discharge specific capacity of the ultra-high nickel cobalt-free single crystal material coated with the garnet structure at 0.1C and 10C.
[0043] Example 3 A method for preparing an ultra-high nickel cobalt-free single crystal material coated with a garnet structure comprises the following steps: (1) Nickel sulfate, manganese sulfate, iron sulfate and deionized water are prepared into a 4 mol / L metal salt solution, wherein the molar ratio of Ni:Mn:Fe is 94:5:1; 6.5 mol / L sodium hydroxide solution and 2 mol / L ammonia solution are then prepared; the solution is pumped into a reactor at a rate of metal salt solution: sodium hydroxide solution = 1:2, N2 is introduced into the reactor, the temperature in the reactor is 50°C, the reactor is kept warm, and the stirring speed is 500 r / min; after the reaction is complete, the solution is filtered while hot, the filtrate is washed with deionized water, and vacuum dried to obtain a precursor.
[0044] (2) Lithium carbonate and the metal element in the precursor are uniformly mixed at a molar ratio of Li:M=1.05:1 to obtain a mixture A.
[0045] (3) Mixture A is placed in an oxygen atmosphere and calcined using a two-step calcination process, including a first-stage calcination and a second-stage calcination. The process conditions for the first stage calcination are: heat treatment at 550°C for 3 hours, and the process conditions for the second stage calcination are: heat treatment at 850°C for 30 hours. The heating rate of the two calcination methods is 2°C / min. After calcination, it is cooled, jet milled, and sieved to obtain the positive electrode material LiNi to be coated. 0.94 Mn 0.05 Fe 0.01 O2.
[0046] (4) Garnet-type coating material and Mix evenly at a mass ratio of 4.5% to obtain a mixture B, which is then calcined in an atmosphere furnace in an oxygen atmosphere at a temperature of 400°C for 15 hours at a heating rate of 2°C / min. After calcination, cool and sieve to obtain the positive electrode material LiNi 0.94 Mn 0.05 Fe 0.01 O2·Li 6.9 Ln3Z 1.9 (Nb+Ta) 0.1 O 12 .
[0047] (5) Test the discharge specific capacity of the ultra-high nickel cobalt-free single crystal material coated with the garnet structure at 0.1C and 10C.
[0048] Example 4 A method for preparing an ultra-high nickel cobalt-free single crystal material coated with a garnet structure comprises the following steps: (1) Nickel sulfate, manganese sulfate, zirconium sulfate and deionized water are prepared into a 4 mol / L metal salt solution in which the molar ratio of Ni:Mn:Zr is 94:5:1; 6.5 mol / L sodium hydroxide solution and 2 mol / L ammonia solution are then prepared; the solution is pumped into a reactor at a rate of metal salt solution: sodium hydroxide solution = 1:2, N2 is introduced into the reactor, the temperature in the reactor is 50°C, the reactor is kept warm, and the stirring speed is 500 r / min; after the reaction is complete, the solution is filtered while hot, the filtrate is washed with deionized water, and vacuum dried to obtain a precursor.
[0049] (2) Lithium carbonate and the metal element in the precursor are mixed evenly at a molar ratio of Li:M=1.05:1.35 to obtain a mixture A.
[0050] (3) Mixture A is placed in an oxygen atmosphere and calcined using a two-step calcination process, including a first-stage calcination and a second-stage calcination. The process conditions for the first-stage calcination are: heat treatment at 300°C for 3 hours, and the process conditions for the second-stage calcination are: heat treatment at 850°C for 30 hours. The heating rate of the two calcination methods is 6°C / min. After calcination, it is cooled, jet milled, and sieved to obtain the positive electrode material LiNi to be coated. 0.94 Mn 0.05 Zr 0.01 O2.
[0051] (4) Garnet-type coating material With LiNi 0.94 Mn 0.05 Zr 0.01 O2 was mixed evenly at a mass ratio of 4.5% to obtain a mixture B, which was then calcined in an atmosphere furnace with an oxygen atmosphere. The temperature of the atmosphere furnace was 400°C, the heat treatment was performed for 15 hours, and the heating rate was 2°C / min. After calcination, the mixture was cooled and sieved to obtain the positive electrode material LiNi 0.94 Mn 0.05 Zr 0.01 O2·Li 6.9 Ln3Z 1.9 (Nb+Ta) 0.1 O 12 .
[0052] (5) Test the discharge specific capacity of the ultra-high nickel cobalt-free single crystal material coated with the garnet structure at 0.1C and 10C.
[0053] Comparative Example 1 A method for preparing a positive electrode material for a lithium ion battery comprises the following steps: (1) Nickel sulfate, manganese sulfate, cobalt sulfate and deionized water are prepared into a 4 mol / L metal salt solution in which the molar ratio of Ni:Mn:Co is 94:5:1; 6.5 mol / L sodium hydroxide solution and 2 mol / L ammonia solution are then prepared; the solution is pumped into a reactor at a rate of metal salt solution: sodium hydroxide solution = 1:2, N2 is introduced into the reactor, the temperature in the reactor is 50°C, the reactor is kept warm, and the stirring speed is 500 r / min; after the reaction is complete, the solution is filtered while hot, the filtrate is washed with deionized water, and vacuum dried to obtain a precursor.
[0054] (2) Lithium carbonate and the metal element in the precursor are uniformly mixed at a molar ratio of Li:M=1.05:1 to obtain a mixture A.
[0055] (3) Mixture A is placed in an oxygen atmosphere and calcined using a two-step calcination process, including a first-stage calcination and a second-stage calcination. The process conditions for the first stage calcination are: heat treatment at 550°C for 3 hours, and the process conditions for the second stage calcination are: heat treatment at 850°C for 30 hours. The heating rate of the two calcination methods is 2°C / min. After calcination, it is cooled, jet milled, and sieved to obtain the positive electrode material LiNi 0.94 Mn 0.05 Co 0.01 O2.
[0056] (4) Test the discharge specific capacity of the positive electrode material at 0.1C and 10C.
[0057] The ultra-high nickel cobalt-free single crystal lithium ion battery positive electrode material obtained in Examples 1-4 was compared with the LiNi obtained in Comparative Example 1. 0.94 Mn 0.05 Co 0.01 O2 material is used as the positive electrode, and metal lithium sheet is used as the negative electrode. They are assembled into button batteries for charge and discharge comparison tests. The test results are as follows: Table 1 Discharge capacity test data of battery positive electrode materials ; It can be concluded from Table 1 that the garnet-type structure-coated ultra-high nickel cobalt-free single crystal material obtained in Examples 1-4 is used as the positive electrode, and the metal lithium sheet is used as the negative electrode to assemble a button-type battery for charge and discharge comparison test. The first cycle discharge capacity at a rate of 0.1C can reach up to 213.9 mAh / g, and the ratio of the first cycle discharge capacity to 0.1C at a rate of 10C is as high as 74.5. The LiNi in Comparative Example 1 0.94 Mn 0.05 Co 0.01The first cycle discharge capacity of O2 material as positive electrode at 0.1C is 208.4, but the ratio of the first cycle discharge capacity at 10C to the first cycle discharge capacity at 0.1C is only 34.8. It can be seen that the battery made of the garnet-type coated ultra-high nickel cobalt-free single crystal positive electrode material obtained in the present invention has better electrical performance than the ordinary ternary ultra-high nickel positive electrode material, and the best doping element in the present invention is yttrium.
[0058] Figure 4 It is the charge and discharge curve of the battery made of the positive electrode material prepared in Example 1 and Comparative Example 1 at 0.1C rate in the voltage range of 3.0-4.3V. It can be seen from the figure that at 0.1C rate 3.0-4.3V, the first cycle discharge capacity of Example 1 is higher than that of Comparative Example 1, and the battery energy retention rate performance is better than that of Comparative Example 1.
[0059] Figure 5 It is the rate performance of the battery made of the positive electrode materials prepared in Example 1 and Comparative Example 1 in the voltage range of 3.0-4.3V. It can be seen from the figure that the specific capacity of Example 1 at different cycle numbers at 0.1C, 0.2C, 0.5C, 1C, 5C, and 10C rates is better than that of Comparative Example 1, and the capacity retention rate of the battery in Example 1 is higher than that in Comparative Example 1.
[0060] Therefore, the present invention adopts the above-mentioned garnet-type structure-coated ultra-high nickel cobalt-free single crystal material and its preparation method, and solves the problem of high material cost by using elements with abundant reserves instead of expensive cobalt. At the same time, iron-aluminum doping and boride coating are used to prepare the positive electrode material with excellent cycle stability and good rate performance. The preparation method is simple to operate, low in cost, and has commercial application value.
[0061] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. Ultra-high nickel cobalt-free single crystal material coated with garnet structure, characterized by: Ultra-high nickel cobalt-free single crystal material is a positive electrode material for batteries. It is sintered by precursor and lithium source, and its chemical formula is LiNi x Mn 1-x-y A y O2·Li 7-n Ln3Z 2-n (Nb+Ta) n O 12 ; Wherein A is Fe, Al, Y or Zr element, x, y and n are molar numbers, x≥0.9, y≤0.05 and n≤0.
3.
2. The garnet-type structure-coated ultra-high nickel cobalt-free single crystal material according to claim 1, characterized in that: The particle size of the precursor is 2-5 μm, and the chemical formula of the precursor is Ni x Mn 1-x-y A y (OH)2, wherein A is Fe, Al, Y or Zr element, x and y are molar numbers, x≥0.9, y≤0.
05.
3. The garnet-type structure-coated ultra-high nickel cobalt-free single crystal material according to claim 1, characterized in that: The positive electrode material is a hexagonal α-NaFeO2 rock salt structure, and its space group is R-3m The particle size of the positive electrode material is 2-5 μm, and its surface is dotted with a coating material. The coating material is a garnet-type structure with a particle size of 5-100 nm.
4. A method for preparing the ultra-high nickel cobalt-free single crystal material coated with a garnet-type structure according to any one of claims 1 to 3, characterized in that: The following steps are involved: Step 1: Mix soluble nickel salt, manganese salt and soluble salt of doping element according to a certain stoichiometric ratio and add deionized water to prepare a metal salt solution, add a precipitant into deionized water to dissolve to prepare a precipitant solution, and dilute the complexing agent to a certain concentration to prepare a complexing agent solution; Step 2: Heat the metal salt solution, the complexing agent solution and the precipitant solution separately, inject them into the reaction kettle and introduce the protective gas, then keep warm and stir to carry out the coprecipitation reaction, filter while hot, and finally wash the filtered precipitate with deionized water and vacuum dry it to obtain the precursor Ni x Mn 1-x-y A y (OH)2; Step 3: fully and uniformly mix the lithium source and the precursor in step 2 in a high-speed mixer according to a certain ratio to obtain a mixture A; Step 4: Place the mixture A in step 3 into an atmosphere furnace for calcination. After calcination, cool, jet mill, and sieve to obtain the positive electrode material LiNi to be coated. x Mn 1-x-y A y O2; Step 5: The garnet-type coating material and the positive electrode material in step 4 are mixed in a high-speed mixer in a certain ratio to obtain a mixture B; Step 6: Place the mixture B in step 5 into an atmosphere furnace for calcination. After calcination, cool and sieve to obtain the positive electrode material LiNi x Mn 1-x-y A y O2·Li 7-n Ln3Z 2-n (Nb+Ta) n O 12 .
5. The method for preparing the garnet-type structure-coated ultra-high nickel cobalt-free single crystal material according to claim 4, characterized in that: The nickel salt in step 1 is one or more of nickel sulfate, nickel nitrate and nickel chloride, the manganese salt is one or more of manganese sulfate, manganese nitrate and manganese chloride, the precipitant is one or more of sodium hydroxide, sodium carbonate, sodium bicarbonate, potassium hydroxide, potassium carbonate and potassium bicarbonate, the complexing agent is one or more of ammonia water and oxalic acid, the total concentration of metal cations in the metal salt solution is 3-10 mol / L, the concentration of the precipitant solution is 5-7 mol / L, and the concentration of the complexing agent solution is 1.5-2 mol / L.
6. The method for preparing the garnet-type structure-coated ultra-high nickel cobalt-free single crystal material according to claim 4, characterized in that: The heating temperature in the step 2 is 40-80°C, the protective gas is one or more of N2 and Ar, the stirring speed is 200-500rpm, the pH is 10.5-11.0, and the vacuum drying temperature is 120-180°C.
7. The method for preparing the garnet-type structure-coated ultra-high nickel cobalt-free single crystal material according to claim 4, characterized in that: The lithium source in step three is one or more of lithium carbonate, lithium hydroxide, lithium hydroxide monohydrate, lithium nitrate, lithium chloride and lithium sulfate, the molar ratio of lithium element in the lithium source to the metal element in the precursor is Li:M=1.05-1.35, the speed of the high-speed mixer is 200-500rpm, the mixing time is 10-40min, and the volume of the mixed material does not exceed 1 / 3 of the volume of the high-speed mixer.
8. The method for preparing the garnet-type structure-coated ultra-high nickel cobalt-free single crystal material according to claim 4, characterized in that: The atmosphere in the atmosphere furnace of step 4 is nitrogen, oxygen or a mixed atmosphere of the two. A two-step roasting process is adopted during roasting, including a first-stage roasting and a second-stage roasting. The first-stage roasting process conditions are a heat treatment at 200-600°C for 1-6h, and the second-stage roasting process conditions are a heat treatment at 700-1000°C for 5-30h. The heating rates of the first-stage roasting process and the second-stage roasting process are both 2°C / min-10°C / min, and the cooling method is natural cooling to room temperature.
9. The method for preparing the garnet-type structure-coated ultra-high nickel cobalt-free single crystal material according to claim 4, characterized in that: In step 5, the garnet-type coating material and LiNi x Mn 1-x-y A y The mass ratio of O2 does not exceed 5%, the speed of the high-speed mixer is 200-500rpm, the mixing time is 10-40min, and the mixed material does not exceed 1 / 3 of the volume of the high-speed mixer.
10. The method for preparing the garnet-type structure-coated ultra-high nickel cobalt-free single crystal material according to claim 4, characterized in that: The heating gas in the atmosphere furnace of step six is nitrogen, oxygen or a mixed atmosphere of the two, the roasting process is a heat treatment at 300-600°C for 5-30h, the heating rate is 2°C / min-10°C / min, and the cooling method is natural cooling to room temperature.
Citation Information
Patent Citations
Garnet-type ion conductor-coated high-nickel ternary positive electrode material, preparation method and lithium ion battery obtained by preparation
CN109904427A
High-nickel cobalt-free quaternary positive electrode material and preparation method thereof
CN111816877A
Quick-charge type cobalt-free high-nickel ternary concentration gradient core-shell structure lithium ion battery positive electrode material and preparation method thereof
CN114551837A
Monocrystal type cobalt-free high-nickel positive electrode material pre-lithiation and preparation method thereof
CN114551839A
Cobalt-free high-nickel ternary gradient lithium ion battery positive electrode material and preparation method thereof
CN114843468A
Cited By
Composite positive electrode material and preparation method thereof, lithium ion battery and electric equipment
CN119841359A
Positive electrode material and preparation method thereof
CN119920896A