Air filtering membrane and preparation method thereof
Through electrospinning technology of modified polypropylene and functional graphene oxide, an air filter membrane with high filtration efficiency, flame retardant and antibacterial properties was prepared, which solved the problem of insufficient filtration efficiency and flame retardant properties in the prior art. Effective filtering and flame retardant effects on fine pollutants and microorganisms are achieved.
Patent Information
- Application Number
- CN202411306525.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-22
AI Technical Summary
Existing electrospun air filter materials are difficult to efficiently filter fine pollutant particles and pathogenic microorganisms at the same time, and their flame retardant and antibacterial properties are insufficient.
The air filter membrane is prepared by electrospinning stacking using modified polypropylene and functional graphene oxide. The phosphorus element is introduced through phosphorus addition reaction to form a flame retardant layer. The anti-static properties are improved by capping graphene oxide by sodium hydroxide. Interfere with bacterial growth by grafting dicyandiamide.
The filtration efficiency, flame retardant properties, antibacterial properties and mechanical properties of the air filter membrane are improved, and the filtering capacity of pollutant particles less than 2.5μm and the killing effect on bacteria are enhanced.
Smart Images

Figure BDA0005049384680000021 
Figure BDA0005049384680000022 
Figure BDA0005049384680000031
Abstract
Description
Technical Field
[0001] The invention relates to the field of filter membranes, in particular to an air filter membrane and a preparation method thereof. Background Art
[0002] With the development of human society, the increasing level of urbanization and industrialization, environmental pollution, especially air pollution, is becoming increasingly serious, posing a serious threat to human health. Therefore, research on air filter materials is particularly important. Air filter materials are mainly divided into needle-punched air filter materials, electrostatically spun air filter materials and melt-blown air filter materials. Among them, electrostatically spun air filter materials are considered to have great potential in the field of air filtration due to their advantages such as high filtration efficiency, low resistance and high surface area. In addition to a large number of fine pollutant particles, there are also some pathogenic microorganisms in the polluted air. It is difficult for ordinary electrostatically spun air filter materials to filter these pollutants at the same time. Therefore, the present invention prepares an air filter membrane with excellent antibacterial properties. Summary of the invention
[0003] In view of the deficiencies in the prior art, the technical problem to be solved by the present invention is to provide an air filtration membrane and a preparation method thereof.
[0004] The technical solution of the present invention to solve the technical problem of the air filtration membrane is to provide an air filtration membrane, wherein the air filtration membrane is obtained by mixing modified polypropylene and functional graphene oxide and then electrostatically spinning and stacking them into a membrane.
[0005] As an optimization, the modified polypropylene is obtained by reacting polypropylene with maleic anhydride and 2,6-di-tert-butyl-4-hydroxymethylphenol in sequence.
[0006] As an optimization, the polypropylene comes from Shanghai Youcheng International Trading Co., Ltd.
[0007] As an optimization, the functional graphene oxide is obtained by reacting pre-modified graphene oxide, phosphorus-containing siloxane and 3-aminopropylmethyldimethoxysilane, and then grafting dicyandiamide.
[0008] As an optimization, the pre-modified graphene oxide is obtained by capping graphene oxide with sodium hydroxide and reacting it with 3-aminopropylmethyldimethoxysilane.
[0009] As an optimization, the graphene oxide model is GO1211, which comes from Angxing New Carbon Materials Changzhou Co., Ltd.
[0010] As an optimization, the phosphorus-containing siloxane is obtained by reacting allylmethyldimethoxysilane and DOPO.
[0011] The technical solution of the present invention to solve the technical problem of the method is to provide a method for preparing an air filtration membrane, comprising the following preparation steps:
[0012] (1) mixing allylmethyldimethoxysilane, DOPO and anhydrous ethanol in a mass ratio of 1:(1.4-1.6):(9-11), stirring and refluxing at 80-90° C. and 270-290 r / min for 2-4 h in a nitrogen atmosphere, rotary evaporating at 50-60° C. for 1-2 h, and drying at 75-85° C. for 3-5 h to obtain phosphorus-containing siloxane;
[0013] (2) mixing graphene oxide and 0.3-0.5wt% sodium hydroxide aqueous solution in a mass ratio of 1:(145-155), stirring at 35-45°C and 100-200rpm for 55-65min, filtering, washing with acetone and anhydrous ethanol for 3-5 times, respectively, and drying at 65-75°C for 5-7h to obtain alkaline-terminated graphene oxide; mixing alkaline-terminated graphene oxide, 3-aminopropylmethyldimethoxysilane and methanol in a mass ratio of 1:(2-3):(8-10), stirring at 60-70°C and 100-200rpm for 6-8h in a nitrogen atmosphere, cooling naturally to room temperature and centrifuging, washing with methanol and deionized water for 3-5 times, respectively, and drying at 55-65°C for 9-11h to obtain pre-modified graphene oxide;
[0014] (3) Pre-modified graphene oxide, phosphorus-containing siloxane, 3-aminopropylmethyldimethoxysilane, ferric chloride and dichloroethane were mixed in a mass ratio of 1:(1-2):(1.3-1.5):(2-3):(14-16), stirred at 35-45°C and 100-200 rpm for 3-5 h, heated to 75-85°C and continued to stir for 19-21 h, naturally cooled to room temperature and filtered, washed with dichloromethane and anhydrous methanol for 4-6 times respectively, and dried at 55-65°C for 2 hours. 3 to 25 hours to obtain modified graphene oxide; the modified graphene oxide, dicyandiamide and deionized water are mixed in a mass ratio of 1: (1.2 to 1.4): (7 to 9), 5 to 7 mol / L hydrochloric acid solution is added to adjust the solution pH to 3 to 4, reflux reaction is carried out in a nitrogen atmosphere at 95 to 105° C. and 100 to 200 rpm for 5 to 7 hours, naturally cooled to room temperature and then filtered, washed with deionized water for 3 to 5 times, and dried at 65 to 75° C. for 6 to 8 hours to obtain functional graphene oxide;
[0015] (4) heating polypropylene at 175-185° C. and 55-65 rpm for 2-4 min, adding maleic anhydride in an amount of 0.02-0.04 times the mass of polypropylene, stirring for 2-4 min, adding dicumyl peroxide in an amount of 0.0002-0.0003 times the mass of polypropylene, reacting for 5-15 min, and naturally cooling to room temperature to obtain pre-modified polypropylene; mixing the pre-modified polypropylene and toluene in a mass ratio of 1:(8-10), and stirring at 40-50° C. and 200-3 00rpm and stirred for 1 to 2 hours, adding 0.09 to 0.11 mol / L sodium hydroxide solution to adjust the pH to 8 to 9, adding 1 to 2 times the mass of pre-modified polypropylene 2,6-di-tert-butyl-4-hydroxymethylphenol, continuing stirring for 4 to 6 hours, adding 0.09 to 0.11 mol / L hydrochloric acid solution to adjust the pH to 6 to 7, naturally cooling to room temperature and filtering, washing with anhydrous ethanol for 3 to 5 times, and drying at 55 to 65°C for 23 to 25 hours to obtain modified polypropylene;
[0016] (5) Modified polypropylene, functional graphene oxide and N,N-dimethylformamide are mixed in a mass ratio of 1:(0.011-0.013):(6-7), stirred at 20-30°C and 200-300 rpm for 1-2 hours, and allowed to stand for 10-20 minutes to obtain a spinning solution; the spinning solution is electrospun and stacked into a film, and dried at 75-85°C for 23-25 hours to obtain an air filtration membrane.
[0017] As an optimization, the reaction equation of the phosphorus-containing siloxane in step (1) is:
[0018]
[0019] As an optimization, the reaction equation of the pre-modified graphene oxide in step (2) is:
[0020]
[0021] As an optimization, the reaction equation for modifying graphene oxide in step (3) is:
[0022]
[0023] As an optimization, the reaction equation of the functional graphene oxide in step (3) is:
[0024]
[0025] As an optimization, the reaction equation of the pre-modified polypropylene in step (4) is:
[0026]
[0027] As an optimization, the reaction equation of the modified polypropylene in step (4) is:
[0028]
[0029] As an optimization, the electrospinning process parameters of step (5) are: spinning voltage 25 kV, ambient humidity 35%, receiving distance 18 cm, drum spindle speed 70 r / min, injection rate 1.5 mL / h.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] When preparing an air filter membrane, the present invention comprises the following steps: reacting allylmethyldimethoxysilane with DOPO to obtain phosphorus-containing siloxane; capping graphene oxide with sodium hydroxide and reacting the resulting graphene oxide with 3-aminopropylmethyldimethoxysilane to obtain pre-modified graphene oxide; reacting the pre-modified graphene oxide, the phosphorus-containing siloxane and 3-aminopropylmethyldimethoxysilane, and then grafting dicyandiamide to obtain functional graphene oxide; reacting polypropylene with maleic anhydride and 2,6-di-tert-butyl-4-hydroxymethylphenol in sequence to obtain modified polypropylene; and evenly mixing the modified polypropylene and the functional graphene oxide and performing electrostatic spinning and deposition to form a membrane to obtain the air filter membrane.
[0032] First, allylmethyldimethoxysilane and DOPO are reacted to obtain phosphorus-containing siloxane; graphene oxide is capped with sodium hydroxide and reacted with 3-aminopropylmethyldimethoxysilane to obtain pre-modified graphene oxide; pre-modified graphene oxide, phosphorus-containing siloxane and 3-aminopropylmethyldimethoxysilane are reacted, and then dicyandiamide is grafted to obtain functional graphene oxide; phosphorus-containing siloxane is obtained by phosphorus-hydrogen addition reaction, and phosphorus element that can react with free radicals generated by thermal decomposition is introduced. Compounds such as phosphorus hydroxide generated by the reaction can consume fuel supply, reduce the occurrence of combustion reaction, form an inert carbon layer, and prevent , slow down the spread of flames and improve the flame retardant properties of the air filtration membrane; use sodium hydroxide to end-cap graphene oxide to prevent carboxyl and hydroxyl groups from affecting the reaction of amino and epoxy groups, and introduce metal cations to improve the antistatic properties of the air filtration membrane; graft 3-aminopropylmethyldimethoxysilane on the surface of graphene oxide to provide reaction sites for the polymerization of long silicon oxygen chains, which can form a non-flammable ceramic layer at high temperatures, further improving the flame retardant properties of the air filtration membrane; the amino groups retained on the long silicon oxygen chains react with dicyandiamide to obtain a biguanide structure, which can interfere with cell metabolism, affect bacterial growth and reproduction, and improve the antibacterial properties of the air filtration membrane.
[0033] Secondly, polypropylene is reacted with maleic anhydride and 2,6-di-tert-butyl-4-hydroxymethylphenol in sequence to obtain modified polypropylene; the modified polypropylene and functional graphene oxide are mixed and then electrospun and deposited into a film to obtain an air filtration membrane; maleic anhydride polar groups are introduced into the polypropylene main chain by melt grafting, and then 2,6-di-tert-butyl-4-hydroxymethylphenol is grafted by esterification reaction, which can capture oxygen free radicals to provide protons, thereby destroying the activity of free radicals and improving the aging resistance of the air filtration membrane; at the same time, the esterification reaction of maleic anhydride and hydroxyl groups can form a large number of carboxyl anions, which are cross-linked with functional graphene oxide through electrostatic bonding, thereby improving the mechanical properties of the air filtration membrane. DETAILED DESCRIPTION
[0034] The specific embodiments of the present invention are given below. The specific embodiments are only used to further illustrate the present invention in detail and do not limit the protection scope of the present invention.
[0035] Example 1
[0036] A method for preparing an air filtration membrane, the method comprising the following steps:
[0037] (1) Allylmethyldimethoxysilane, DOPO and anhydrous ethanol were mixed in a mass ratio of 1:1.4:9, stirred and refluxed at 80°C and 270 r / min in a nitrogen atmosphere for 4 h, rotary evaporated at 50°C for 2 h, and dried at 75°C for 5 h to obtain phosphorus-containing siloxane;
[0038] (2) Graphene oxide and 0.3wt% sodium hydroxide aqueous solution were mixed in a mass ratio of 1:145, stirred at 35°C and 100rpm for 65min, filtered, washed with acetone and anhydrous ethanol for 3 times, dried at 65°C for 7h, and obtained alkaline-terminated graphene oxide; alkaline-terminated graphene oxide, 3-aminopropylmethyldimethoxysilane and methanol were mixed in a mass ratio of 1:2:8, stirred at 60°C and 100rpm for 8h in a nitrogen atmosphere, cooled naturally to room temperature and centrifuged, washed with methanol and deionized water for 3 times, dried at 55°C for 11h, and obtained pre-modified graphene oxide;
[0039] (3) Pre-modified graphene oxide, phosphorus-containing siloxane, 3-aminopropylmethyldimethoxysilane, ferric chloride and dichloroethane were mixed in a mass ratio of 1:1:1.3:2:14, stirred at 35°C and 100 rpm for 5 h, heated to 75°C and continued to stir for 21 h, naturally cooled to room temperature and filtered, washed with dichloromethane and anhydrous methanol for 4 times respectively, and dried at 55°C for 25 h to obtain modified graphene oxide; modified graphene oxide, dicyandiamide and deionized water were mixed in a mass ratio of 1:1.2:7, 5 mol / L hydrochloric acid solution was added to adjust the solution pH to 3, refluxed in a nitrogen atmosphere at 95°C and 100 rpm for 7 h, naturally cooled to room temperature and filtered, washed with deionized water 3 times, and dried at 65°C for 8 h to obtain functional graphene oxide;
[0040] (4) heating the polypropylene at 175° C. and 55 rpm for 4 min, adding maleic anhydride in an amount of 0.02 times the mass of the polypropylene, stirring for 4 min, adding diisopropylbenzene peroxide in an amount of 0.0002 times the mass of the polypropylene, reacting for 15 min, and naturally cooling to room temperature to obtain pre-modified polypropylene; mixing the pre-modified polypropylene and toluene in a mass ratio of 1:8, stirring at 40° C. and 200 rpm for 2 h, adding 0.09 mol / L sodium hydroxide solution to adjust the pH to 8, adding 2,6-di-tert-butyl-4-hydroxymethylphenol in an amount of 1 times the mass of the pre-modified polypropylene, continuing to stir for 6 h, adding 0.091 mol / L hydrochloric acid solution to adjust the pH to 6, naturally cooling to room temperature, filtering, washing with anhydrous ethanol 3 times, and drying at 55° C. for 25 h to obtain modified polypropylene;
[0041] (5) Modified polypropylene, functional graphene oxide and N,N-dimethylformamide were mixed in a mass ratio of 1:0.011:6, stirred at 20°C and 200 rpm for 2 h, and allowed to stand for 20 min to obtain a spinning solution; the spinning solution was electrospun and stacked into a film, and dried at 75°C for 25 h to obtain an air filtration membrane.
[0042] Example 2
[0043] A method for preparing an air filtration membrane, the method comprising the following steps:
[0044] (1) Allylmethyldimethoxysilane, DOPO and anhydrous ethanol were mixed in a mass ratio of 1:1.5:10, stirred and refluxed at 85°C and 280 r / min in a nitrogen atmosphere for 3 h, rotary evaporated at 55°C for 1.5 h, and dried at 80°C for 4 h to obtain phosphorus-containing siloxane;
[0045] (2) Graphene oxide and 0.4wt% sodium hydroxide aqueous solution were mixed in a mass ratio of 1:150, stirred at 40°C and 150rpm for 60min, filtered, washed with acetone and anhydrous ethanol for 4 times, dried at 70°C for 6h, and obtained alkaline-terminated graphene oxide; alkaline-terminated graphene oxide, 3-aminopropylmethyldimethoxysilane and methanol were mixed in a mass ratio of 1:2.5:9, stirred at 65°C and 150rpm for 7h in a nitrogen atmosphere, cooled naturally to room temperature and centrifuged, washed with methanol and deionized water for 4 times, dried at 60°C for 10h, and obtained pre-modified graphene oxide;
[0046] (3) Pre-modified graphene oxide, phosphorus-containing siloxane, 3-aminopropylmethyldimethoxysilane, ferric chloride and dichloroethane were mixed in a mass ratio of 1:1.5:1.4:2.5:15, stirred at 40°C and 150rpm for 4h, heated to 80°C and continued to stir for 20h, naturally cooled to room temperature and filtered, washed with dichloromethane and anhydrous methanol for 5 times respectively, and dried at 60°C for 24h to obtain modified graphene oxide; modified graphene oxide, dicyandiamide and deionized water were mixed in a mass ratio of 1:1.3:8, 6mol / L hydrochloric acid solution was added to adjust the solution pH to 3.5, refluxed in a nitrogen atmosphere at 100°C and 150rpm for 6h, naturally cooled to room temperature and filtered, washed with deionized water 4 times, and dried at 70°C for 7h to obtain functional graphene oxide;
[0047] (4) heating the polypropylene at 180° C. and 60 rpm for 3 min, adding maleic anhydride in an amount of 0.03 times the mass of the polypropylene, stirring for 3 min, adding diisopropylbenzene peroxide in an amount of 0.00025 times the mass of the polypropylene, reacting for 10 min, and naturally cooling to room temperature to obtain pre-modified polypropylene; mixing the pre-modified polypropylene and toluene in a mass ratio of 1:9, stirring at 45° C. and 250 rpm for 1.5 h, adding 0.1 mol / L sodium hydroxide solution to adjust the pH to 8.5, adding 2,6-di-tert-butyl-4-hydroxymethylphenol in an amount of 1.5 times the mass of the pre-modified polypropylene, continuing to stir for 5 h, adding 0.1 mol / L hydrochloric acid solution to adjust the pH to 6.5, naturally cooling to room temperature, filtering, washing with anhydrous ethanol 4 times, and drying at 60° C. for 24 h to obtain modified polypropylene;
[0048] (5) Modified polypropylene, functional graphene oxide and N,N-dimethylformamide were mixed in a mass ratio of 1:0.012:6.5, stirred at 25°C and 250 rpm for 1.5 h, and allowed to stand for 15 min to obtain a spinning solution; the spinning solution was electrospun and stacked into a film, and dried at 80°C for 24 h to obtain an air filtration membrane.
[0049] Example 3
[0050] A method for preparing an air filtration membrane, the method comprising the following steps:
[0051] (1) Allylmethyldimethoxysilane, DOPO and anhydrous ethanol were mixed in a mass ratio of 1:1.6:11, stirred and refluxed at 90°C and 290 r / min in a nitrogen atmosphere for 2 h, rotary evaporated at 60°C for 1 h, and dried at 85°C for 3 h to obtain phosphorus-containing siloxane;
[0052] (2) Graphene oxide and 0.5wt% sodium hydroxide aqueous solution were mixed in a mass ratio of 1:155, stirred at 45°C and 200rpm for 55min, filtered, washed with acetone and anhydrous ethanol for 5 times, and dried at 75°C for 5h to obtain alkaline-terminated graphene oxide; alkaline-terminated graphene oxide, 3-aminopropylmethyldimethoxysilane and methanol were mixed in a mass ratio of 1:3:10, stirred at 70°C and 200rpm for 6h in a nitrogen atmosphere, cooled naturally to room temperature and centrifuged, washed with methanol and deionized water for 5 times, and dried at 65°C for 9h to obtain pre-modified graphene oxide;
[0053] (3) Pre-modified graphene oxide, phosphorus-containing siloxane, 3-aminopropylmethyldimethoxysilane, ferric chloride and dichloroethane were mixed in a mass ratio of 1:2:1.5:3:16, stirred at 45°C and 200 rpm for 3 h, heated to 85°C and continued to stir for 19 h, naturally cooled to room temperature and filtered, washed with dichloromethane and anhydrous methanol for 6 times respectively, and dried at 65°C for 23 h to obtain modified graphene oxide; modified graphene oxide, dicyandiamide and deionized water were mixed in a mass ratio of 1:1.4:9, 7 mol / L hydrochloric acid solution was added to adjust the solution pH to 4, refluxed in a nitrogen atmosphere at 105°C and 200 rpm for 5 h, naturally cooled to room temperature and filtered, washed with deionized water 5 times, and dried at 75°C for 6 h to obtain functional graphene oxide;
[0054] (4) heating the polypropylene at 185° C. and 65 rpm for 2 min, adding maleic anhydride in an amount of 0.04 times the mass of the polypropylene, stirring for 2 min, adding diisopropylbenzene peroxide in an amount of 0.0003 times the mass of the polypropylene, reacting for 5 min, and naturally cooling to room temperature to obtain pre-modified polypropylene; mixing the pre-modified polypropylene and toluene in a mass ratio of 1:10, stirring at 50° C. and 300 rpm for 1 h, adding 0.11 mol / L sodium hydroxide solution to adjust the pH to 9, adding 2,6-di-tert-butyl-4-hydroxymethylphenol in an amount of 2 times the mass of the pre-modified polypropylene, continuing to stir for 4 h, adding 0.11 mol / L hydrochloric acid solution to adjust the pH to 7, naturally cooling to room temperature, filtering, washing with anhydrous ethanol 5 times, and drying at 65° C. for 23 h to obtain modified polypropylene;
[0055] (5) Modified polypropylene, functional graphene oxide and N,N-dimethylformamide were mixed in a mass ratio of 1:0.013:7, stirred at 30°C and 300 rpm for 1 hour, and allowed to stand for 10 minutes to obtain a spinning solution; the spinning solution was electrospun and stacked into a film, and dried at 85°C for 23 hours to obtain an air filtration membrane.
[0056] Comparative Example 1
[0057] A method for preparing an air filtration membrane, the method comprising the following steps:
[0058] (1) Graphene oxide and 0.4wt% sodium hydroxide aqueous solution were mixed in a mass ratio of 1:150, stirred at 40°C and 150rpm for 60min, filtered, washed with acetone and anhydrous ethanol for 4 times, dried at 70°C for 6h, and obtained alkaline-terminated graphene oxide; alkaline-terminated graphene oxide, 3-aminopropylmethyldimethoxysilane and methanol were mixed in a mass ratio of 1:2.5:9, stirred at 65°C and 150rpm for 7h in a nitrogen atmosphere, cooled naturally to room temperature and centrifuged, washed with methanol and deionized water for 4 times, dried at 60°C for 10h, and obtained pre-modified graphene oxide;
[0059] (2) Pre-modified graphene oxide, 3-aminopropylmethyldimethoxysilane, ferric chloride and dichloroethane were mixed in a mass ratio of 1:1.5:1.4:2.5:15, stirred at 40°C and 150rpm for 4h, heated to 80°C and continued to stir for 20h, naturally cooled to room temperature and filtered, washed with dichloromethane and anhydrous methanol for 5 times respectively, and dried at 60°C for 24h to obtain modified graphene oxide; modified graphene oxide, dicyandiamide and deionized water were mixed in a mass ratio of 1:1.3:8, 6mol / L hydrochloric acid solution was added to adjust the solution pH to 3.5, refluxed in a nitrogen atmosphere at 100°C and 150rpm for 6h, naturally cooled to room temperature and filtered, washed with deionized water 4 times, and dried at 70°C for 7h to obtain functional graphene oxide;
[0060] (3) heating the polypropylene at 180° C. and 60 rpm for 3 min, adding maleic anhydride in an amount of 0.03 times the mass of the polypropylene, stirring for 3 min, adding diisopropylbenzene peroxide in an amount of 0.00025 times the mass of the polypropylene, reacting for 10 min, and naturally cooling to room temperature to obtain pre-modified polypropylene; mixing the pre-modified polypropylene and toluene in a mass ratio of 1:9, stirring at 45° C. and 250 rpm for 1.5 h, adding 0.1 mol / L sodium hydroxide solution to adjust the pH to 8.5, adding 2,6-di-tert-butyl-4-hydroxymethylphenol in an amount of 1.5 times the mass of the pre-modified polypropylene, continuing to stir for 5 h, adding 0.1 mol / L hydrochloric acid solution to adjust the pH to 6.5, cooling naturally to room temperature, filtering, washing with anhydrous ethanol 4 times, and drying at 60° C. for 24 h to obtain modified polypropylene;
[0061] (4) Modified polypropylene, functional graphene oxide and N,N-dimethylformamide were mixed in a mass ratio of 1:0.012:6.5, stirred at 25°C and 250 rpm for 1.5 h, and allowed to stand for 15 min to obtain a spinning solution; the spinning solution was electrospun and stacked into a film, and dried at 80°C for 24 h to obtain an air filtration membrane.
[0062] Comparative Example 2
[0063] A method for preparing an air filtration membrane, the method comprising the following steps:
[0064] (1) Allylmethyldimethoxysilane, DOPO and anhydrous ethanol were mixed in a mass ratio of 1:1.5:10, stirred and refluxed at 85°C and 280 r / min in a nitrogen atmosphere for 3 h, rotary evaporated at 55°C for 1.5 h, and dried at 80°C for 4 h to obtain phosphorus-containing siloxane;
[0065] (2) Graphene oxide and 0.4wt% sodium hydroxide aqueous solution were mixed in a mass ratio of 1:150, stirred at 40°C and 150rpm for 60min, filtered, washed with acetone and anhydrous ethanol for 4 times, dried at 70°C for 6h, and obtained alkaline-terminated graphene oxide; alkaline-terminated graphene oxide, 3-aminopropylmethyldimethoxysilane and methanol were mixed in a mass ratio of 1:2.5:9, stirred at 65°C and 150rpm for 7h in a nitrogen atmosphere, cooled naturally to room temperature and centrifuged, washed with methanol and deionized water for 4 times, dried at 60°C for 10h, and obtained pre-modified graphene oxide;
[0066] (3) Pre-modified graphene oxide, phosphorus-containing siloxane, 3-aminopropylmethyldimethoxysilane, ferric chloride and dichloroethane were mixed in a mass ratio of 1:1.5:1.4:2.5:15, stirred at 40°C and 150 rpm for 4 h, heated to 80°C and continued to stir for 20 h, naturally cooled to room temperature and filtered, washed with dichloromethane and anhydrous methanol for 5 times respectively, and dried at 60°C for 24 h to obtain modified graphene oxide;
[0067] (4) heating the polypropylene at 180° C. and 60 rpm for 3 min, adding maleic anhydride in an amount of 0.03 times the mass of the polypropylene, stirring for 3 min, adding diisopropylbenzene peroxide in an amount of 0.00025 times the mass of the polypropylene, reacting for 10 min, and naturally cooling to room temperature to obtain pre-modified polypropylene; mixing the pre-modified polypropylene and toluene in a mass ratio of 1:9, stirring at 45° C. and 250 rpm for 1.5 h, adding 0.1 mol / L sodium hydroxide solution to adjust the pH to 8.5, adding 2,6-di-tert-butyl-4-hydroxymethylphenol in an amount of 1.5 times the mass of the pre-modified polypropylene, continuing to stir for 5 h, adding 0.1 mol / L hydrochloric acid solution to adjust the pH to 6.5, naturally cooling to room temperature, filtering, washing with anhydrous ethanol 4 times, and drying at 60° C. for 24 h to obtain modified polypropylene;
[0068] (5) Modified polypropylene, modified graphene oxide and N,N-dimethylformamide were mixed in a mass ratio of 1:0.012:6.5, stirred at 25°C and 250 rpm for 1.5 h, and allowed to stand for 15 min to obtain a spinning solution; the spinning solution was electrospun and stacked into a film, which was dried at 80°C for 24 h to obtain an air filtration membrane.
[0069] Comparative Example 3
[0070] A method for preparing an air filtration membrane, the method comprising the following steps:
[0071] (1) Allylmethyldimethoxysilane, DOPO and anhydrous ethanol were mixed in a mass ratio of 1:1.5:10, stirred and refluxed at 85°C and 280 r / min in a nitrogen atmosphere for 3 h, rotary evaporated at 55°C for 1.5 h, and dried at 80°C for 4 h to obtain phosphorus-containing siloxane;
[0072] (2) Graphene oxide and 0.4wt% sodium hydroxide aqueous solution were mixed in a mass ratio of 1:150, stirred at 40°C and 150rpm for 60min, filtered, washed with acetone and anhydrous ethanol for 4 times, dried at 70°C for 6h, and obtained alkaline-terminated graphene oxide; alkaline-terminated graphene oxide, 3-aminopropylmethyldimethoxysilane and methanol were mixed in a mass ratio of 1:2.5:9, stirred at 65°C and 150rpm for 7h in a nitrogen atmosphere, cooled naturally to room temperature and centrifuged, washed with methanol and deionized water for 4 times, dried at 60°C for 10h, and obtained pre-modified graphene oxide;
[0073] (3) Pre-modified graphene oxide, phosphorus-containing siloxane, 3-aminopropylmethyldimethoxysilane, ferric chloride and dichloroethane were mixed in a mass ratio of 1:1.5:1.4:2.5:15, stirred at 40°C and 150rpm for 4h, heated to 80°C and continued to stir for 20h, naturally cooled to room temperature and filtered, washed with dichloromethane and anhydrous methanol for 5 times respectively, and dried at 60°C for 24h to obtain modified graphene oxide; modified graphene oxide, dicyandiamide and deionized water were mixed in a mass ratio of 1:1.3:8, 6mol / L hydrochloric acid solution was added to adjust the solution pH to 3.5, refluxed in a nitrogen atmosphere at 100°C and 150rpm for 6h, naturally cooled to room temperature and filtered, washed with deionized water 4 times, and dried at 70°C for 7h to obtain functional graphene oxide;
[0074] (4) heating the polypropylene at 180° C. and 60 rpm for 3 min, adding maleic anhydride at 0.03 times the mass of the polypropylene, stirring for 3 min, adding dicumyl peroxide at 0.00025 times the mass of the polypropylene, reacting for 10 min, and naturally cooling to room temperature to obtain pre-modified polypropylene;
[0075] (5) Pre-modified polypropylene, functional graphene oxide and N,N-dimethylformamide were mixed in a mass ratio of 1:0.012:6.5, stirred at 25°C and 250 rpm for 1.5 h, and allowed to stand for 15 min to obtain a spinning solution; the spinning solution was electrospun and stacked into a film, which was dried at 80°C for 24 h to obtain an air filtration membrane.
[0076] Test Example 1
[0077] 1. Filtering effect
[0078] Test method: Take samples of 150 mm × 150 mm in size from the air filter membranes obtained in each embodiment and the comparative example, and use TOPASAFC-131 automatic filter material tester to test the air filter membranes at a wind speed of 32 L / min (5.3 cm / s) and an ash supply rate of 1 g / m 3ISO12103-A2 dust was filtered under the conditions of , and the filtration efficiency of pollutant particles smaller than 2.5μm was tested.
[0079] Table 1 below shows the analysis results of the filtration effects of the air filtration membranes of Examples 1 to 3 of the present invention and Comparative Examples 1 to 3.
[0080] Table 1
[0081] Filtration efficiency % Filtration efficiency % Example 1 99.2 Comparative Example 1 99.1 Example 2 99.6 Comparative Example 2 98.9 Example 3 99.5 Comparative Example 3 99.2
[0082] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 1, it can be found that the air filtration membrane prepared by the present invention has a good filtration effect.
[0083] By comparison, the filtration efficiency of Examples 1 to 3 and Comparative Examples 1 to 3 is not significantly different, which shows that the air filtration membranes prepared by the electrospinning method of the present invention have good filtration effects.
[0084] Test Example 2
[0085] 1. Antibacterial
[0086] Test method: Take circular samples with a diameter of 25 mm from the air filter membranes obtained in each embodiment and the comparative example, put the samples into an agar medium containing Staphylococcus aureus according to GB / T20944, culture for 24 hours, and measure the width of the sterile zone.
[0087] 2. Mechanical properties
[0088] Test method: Take samples of 20mm×100mm in size from the air filtration membranes obtained in each embodiment and the comparative example, and test the tensile strength σ0 using a universal strength testing machine at a tensile speed of 100mm / min.
[0089] 3. Anti-aging
[0090] Test method: Take samples of 20mm×100mm size from the air filtration membrane obtained in each embodiment and the comparative example, use a 401AB type heated air drying oven to stand at 60°C for 5 days, use a universal strength testing machine, at a tensile speed of 100mm / min, test the tensile strength σ1 again, and calculate the strength retention rate = σ1 / σ0*100%.
[0091] 4. Flame retardancy
[0092] Test method: The air filtration fibers obtained in each example (directly dried without depositing into a film after electrospinning) and the comparative example were tested for limiting oxygen index according to GB / T2406.
[0093] Table 2 below shows the analysis results of the antibacterial property, flame retardancy, mechanical properties and anti-aging property of the air filtration membranes of Examples 1 to 3 of the present invention and Comparative Examples 1 to 3.
[0094] Table 2
[0095] Sterile belt width cm Tensile strength MPa Strength retention rate % Limiting oxygen index % Example 1 4.8 31.1 87.3 29.2 Example 2 4.9 31.4 87.6 29.6 Example 3 4.6 31.2 87.1 29.5 Comparative Example 1 4.4 31.1 86.9 20.4 Comparative Example 2 0.1 21.9 84.7 29.1 Comparative Example 3 4.6 20.5 43.9 29.2
[0096] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 2, it can be found that the air filtration membrane prepared by the present invention has good antibacterial properties, flame retardancy, mechanical properties and anti-aging properties.
[0097] By comparison, the limiting oxygen index of Examples 1, 2, and 3 is higher than that of Comparative Example 1, which illustrates that phosphorus-containing siloxane is obtained by phosphorus-hydrogen addition reaction, phosphorus element which can react with free radicals generated by thermal decomposition is introduced, and compounds such as phosphorus hydroxide generated by the reaction can consume fuel supply, reduce the occurrence of combustion reaction, form an inert carbon layer, prevent and slow down the spread of flame, and improve the flame retardant properties of the air filtration membrane.
[0098] By comparison, the width and tensile strength of the sterile belt of Examples 1, 2 and 3 are larger than that of Comparative Example 2, which shows that 3-aminopropylmethyldimethoxysilane is grafted on the surface of graphene oxide to provide reaction sites for the polymerization of long silicon oxygen chains. The amino groups on the long silicon oxygen chains react with dicyandiamide to obtain a biguanide structure, which can interfere with cell metabolism, affect bacterial growth and reproduction, and improve the antibacterial property of the air filtration membrane. At the same time, it can also electrostatically combine with a large number of carboxyl anions formed after esterification with maleic anhydride to form crosslinks, thereby improving the mechanical properties of the air filtration membrane.
[0099] By comparison, the tensile strength and strength retention rate of Examples 1, 2, and 3 are higher than that of Comparative Example 3, which shows that the introduction of maleic anhydride polar groups on the polypropylene main chain by melt grafting and then grafting 2,6-di-tert-butyl-4-hydroxymethylphenol by esterification reaction can capture oxygen free radicals to provide protons, thereby destroying the activity of free radicals and improving the aging resistance of the air filtration membrane; at the same time, the esterification reaction of maleic anhydride and hydroxyl groups can form a large number of carboxyl anions, which are cross-linked with functional graphene oxide through electrostatic bonding, thereby improving the mechanical properties of the air filtration membrane.
[0100] Any matters not described in the present invention are applicable to the prior art.
Claims
1. An air filtration membrane, characterized in that: The air filtration membrane is obtained by mixing modified polypropylene and functional graphene oxide and then electrospinning and stacking them into a membrane; The modified polypropylene is obtained by sequentially reacting polypropylene with maleic anhydride and 2,6-di-tert-butyl-4-hydroxymethylphenol; The functional graphene oxide is obtained by reacting pre-modified graphene oxide, phosphorus-containing siloxane and 3-aminopropylmethyldimethoxysilane, and then grafting dicyandiamide; The pre-modified graphene oxide is obtained by capping graphene oxide with sodium hydroxide and reacting with 3-aminopropylmethyldimethoxysilane; The phosphorus-containing siloxane is obtained by reacting allylmethyldimethoxysilane and DOPO.
2. A method for preparing an air filtration membrane, characterized in that: The method comprises the following preparation steps: (1) mixing allylmethyldimethoxysilane, DOPO and anhydrous ethanol in a mass ratio of 1:(1.4-1.6):(9-11), stirring and refluxing at 80-90° C. and 270-290 r / min for 2-4 h in a nitrogen atmosphere, rotary evaporating at 50-60° C. for 1-2 h, and drying at 75-85° C. for 3-5 h to obtain phosphorus-containing siloxane; (2) mixing graphene oxide and 0.3-0.5wt% sodium hydroxide aqueous solution in a mass ratio of 1:(145-155), stirring at 35-45°C and 100-200rpm for 55-65min, filtering, washing with acetone and anhydrous ethanol for 3-5 times, respectively, and drying at 65-75°C for 5-7h to obtain alkaline-terminated graphene oxide; mixing alkaline-terminated graphene oxide, 3-aminopropylmethyldimethoxysilane and methanol in a mass ratio of 1:(2-3):(8-10), stirring at 60-70°C and 100-200rpm for 6-8h in a nitrogen atmosphere, cooling naturally to room temperature and centrifuging, washing with methanol and deionized water for 3-5 times, respectively, and drying at 55-65°C for 9-11h to obtain pre-modified graphene oxide; (3) Pre-modified graphene oxide, phosphorus-containing siloxane, 3-aminopropylmethyldimethoxysilane, ferric chloride and dichloroethane were mixed in a mass ratio of 1:(1-2):(1.3-1.5):(2-3):(14-16), stirred at 35-45°C and 100-200 rpm for 3-5 h, heated to 75-85°C and continued to stir for 19-21 h, naturally cooled to room temperature and filtered, washed with dichloromethane and anhydrous methanol for 4-6 times respectively, and heated at 55- Dry at 65° C. for 23 to 25 hours to obtain modified graphene oxide; mix the modified graphene oxide, dicyandiamide and deionized water in a mass ratio of 1:(1.2 to 1.4):(7 to 9), add 5 to 7 mol / L hydrochloric acid solution to adjust the solution pH to 3 to 4, reflux in a nitrogen atmosphere at 95 to 105° C. and 100 to 200 rpm for 5 to 7 hours, wash with deionized water 3 to 5 times, and dry at 65 to 75° C. for 6 to 8 hours to obtain functional graphene oxide; (4) heating polypropylene at 175-185° C. and 55-65 rpm for 2-4 min, adding maleic anhydride in an amount of 0.02-0.04 times the mass of polypropylene, stirring for 2-4 min, adding dicumyl peroxide in an amount of 0.0002-0.0003 times the mass of polypropylene, reacting for 5-15 min, and naturally cooling to room temperature to obtain pre-modified polypropylene; mixing the pre-modified polypropylene and toluene in a mass ratio of 1:(8-10), and stirring at 40-50° C. and 200-3 00rpm and stirred for 1 to 2 hours, adding 0.09 to 0.11 mol / L sodium hydroxide solution to adjust the pH to 8 to 9, adding 1 to 2 times the mass of pre-modified polypropylene 2,6-di-tert-butyl-4-hydroxymethylphenol, continuing stirring for 4 to 6 hours, adding 0.09 to 0.11 mol / L hydrochloric acid solution to adjust the pH to 6 to 7, naturally cooling to room temperature and filtering, washing with anhydrous ethanol for 3 to 5 times, and drying at 55 to 65°C for 23 to 25 hours to obtain modified polypropylene; (5) Modified polypropylene, functional graphene oxide and N,N-dimethylformamide are mixed in a mass ratio of 1:(0.011-0.013):(6-7), stirred at 20-30°C and 200-300 rpm for 1-2 hours, and allowed to stand for 10-20 minutes to obtain a spinning solution; the spinning solution is electrospun and stacked into a film, and dried at 75-85°C for 23-25 hours to obtain an air filtration membrane.
3. The method for preparing an air filtration membrane according to claim 2, characterized in that: The reaction equation of the phosphorus-containing siloxane in step (1) is:
4. The method for preparing an air filtration membrane according to claim 2, characterized in that: The reaction equation of the pre-modified graphene oxide in step (2) is:
5. The method for preparing an air filtration membrane according to claim 2, characterized in that: The reaction equation for the modified graphene oxide in step (3) is:
6. The method for preparing an air filtration membrane according to claim 2, characterized in that: The reaction equation of the functional graphene oxide in step (3) is:
7. The method for preparing an air filtration membrane according to claim 2, characterized in that: The reaction equation of the pre-modified polypropylene in step (4) is:
8. The method for preparing an air filtration membrane according to claim 2, characterized in that: The reaction equation of the modified polypropylene in step (4) is:
9. The method for preparing an air filtration membrane according to claim 2, characterized in that: The electrospinning process parameters of step (5) are: spinning voltage 25 kV, ambient humidity 35%, receiving distance 18 cm, drum spindle speed 70 r / min, injection rate 1.5 mL / h.