Nickel silicate derived spherical catalyst as well as preparation method and application thereof
The preparation of nickel silicate-derived spherical catalysts by hydrothermal method solves the problem of easy agglomeration of Ru and Ni-based catalysts at high temperatures, achieves efficient and stable ammonia decomposition performance, reduces the amount of precious metals used and improves the stability of the catalyst.
Patent Information
- Application Number
- CN202411061062.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-05
AI Technical Summary
Existing Ru and Ni-based catalysts are prone to agglomeration at high temperatures, resulting in insufficient activity and stability of ammonia decomposition catalysts. Furthermore, they require large amounts of precious metals and have high preparation costs.
Nickel silicate-derived spherical catalysts were prepared by hydrothermal method. A mesoporous silica support was formed by TEOS hydrolysis, and nickel silicate was coated on its surface. Combined with Ru doping, Ru and Ni dual active components were formed, which enhanced the intermetallic interaction and inhibited particle agglomeration.
The prepared catalyst maintains good dispersion and stability at high temperatures, exhibits high ammonia conversion rate and excellent stability, and is suitable for ammonia decomposition to hydrogen production reaction.
Smart Images

Figure CN118988322A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a nickel silicate derived spherical catalyst and a preparation method and application thereof. Background Art
[0002] As an environmentally friendly and sustainable resource, hydrogen has attracted widespread attention from countries around the world. However, hydrogen has a low volume energy density, is highly dangerous, is not convenient for long-distance transportation, and has safety and cost issues during storage and transportation. Therefore, people have focused on on-site hydrogen production using hydrogen storage materials. Compared with hydrogen storage materials such as metal hydrides and metal amine salts, ammonia has a higher volume energy density (108kg H2 / m 3 ) and hydrogen content (17.6wt%), comprehensively speaking, ammonia has the lowest specific energy cost for hydrogen production. The general rule of the activity of metal catalysts used for ammonia decomposition is Ru>Ir>Rh>Co~Ni>Pt>Pd>Fe. Although Ru is expensive, 95% of Ru can be recovered in Ru-based catalysts after the reaction, and the excellent ammonia decomposition performance of Ru-based catalysts is incomparable to non-precious metal catalysts, so Ru is still an important ammonia decomposition catalyst. Ni-based catalysts are commonly used non-precious metal catalysts because of their low price and good ammonia decomposition performance. For example, patent CN117380198A uses nickel foam as raw material and nickel silicate as intermediate to prepare an integral nickel-based catalyst with a particle size of 3.4nm, but the sample has no regular morphology, and the ammonia decomposition stability at 450℃ is only 5h; patent CN117983245A uses graphite carbon as a carrier, precious metals as active components, and alkali metals as additives. Although the prepared series of catalysts are at an air velocity of 30000mL NH3 (g cat *h) -1 , the ammonia conversion rate is 72%-96% at 500°C, but the amount of metal used is large, the amount of precious metal and alkali metal added is 2wt%-15wt%, and the calcination temperature is as high as 1000°C, resulting in high catalyst preparation cost and strict equipment requirements. In addition, the catalyst catalytic activity decay rate is still as high as 5%-42% within 100h; Huang et al. reported a Ru / La2O3 catalyst prepared by co-precipitation in "Ru / La2O3 catalyst for ammonia decomposition to hydrogen" (Applied Surface Science, 2019, 476: 928-936.), which has good activity and can be used at a space velocity of 18000mL. NH3 (g cat *h) -1 The ammonia conversion rate was 91% at 525°C, but its stability test only lasted for 84 hours and still needs to be further improved.
[0003] Obviously, the agglomeration of Ru and Ni particles at high temperatures is still an important factor affecting the activity and stability of the catalyst. It is urgent to find a new preparation method to prepare a catalyst with good performance, which can not only have good ammonia decomposition performance while reducing the amount of precious metals, but also inhibit the agglomeration of particles at high temperatures to obtain excellent stability. Summary of the invention
[0004] The purpose of the present invention is to provide a nickel silicate-derived spherical catalyst and its preparation method and application in view of the shortcomings of the current technology. The catalyst is spherical nickel silicate-coated silicon dioxide, and the active components are Ru or Ru and Ni metals; in the preparation method, firstly, spherical silicon dioxide is obtained by hydrolyzing TEOS under alkaline conditions, and then the surface of the silicon sphere is etched by a hydrothermal method to form a nickel silicate derivative with a mesoporous structure. The nickel silicate derivative formed in this way has a mesoporous structure, but is not hollow, and has good mechanical strength. The NH3.H2O added in the hydrothermal process can not only etch the silicon sphere, but also participate in the formation of nickel silicate; the added CTAB is conducive to the formation of mesopores; Ru doping can obtain a spherical 1Ru-10Ni / SiO2 catalyst, which has more active sites and interaction forces between Ru and Ni metals. The present invention prepares an efficient and stable ammonia decomposition catalyst by a green and simple method, and the reagents used in the preparation process are harmless to the human body and will not produce environmental pollutants. The catalyst has the advantages of small particles, good metal dispersion, and not easy to agglomerate at high temperature.
[0005] The technical solution adopted by the present invention is:
[0006] A nickel silicate-derived spherical catalyst, comprising a carrier and an active component; wherein the carrier is silicon dioxide coated with nickel silicate, and the active component is Ni, or Ru and Ni; the mass ratio of the active component to the catalyst is 1-11%; when the active component is two elements, the ratio of Ru to Ni is 1:9-10;
[0007] The carrier is prepared from silicon dioxide (SiO2), hexadecyltrimethylammonium bromide (CTAB), Ni(NO3)2.6H2O and NH3.H2O by a hydrothermal method, and Ru is loaded on the carrier by an equal volume impregnation method; the content of active components on the catalyst is about 1-11%, and the rest is the carrier.
[0008] The method for preparing the nickel silicate-derived spherical catalyst comprises any of the following two methods:
[0009] Method 1 is the preparation of a nickel silicate-derived spherical catalyst whose active component is Ni, comprising the following steps:
[0010] (1) Tetraethyl orthosilicate (TEOS) is mixed with anhydrous ethanol and deionized water, and stirred at room temperature for 10-20 minutes. Ammonia water is then dropped into the mixture, and the mixture is stirred for 10-15 hours to obtain a suspension A.
[0011] Wherein, 13-14g tetraethyl orthosilicate (TEOS) and 10-12mL deionized water are added to every 140-150mL anhydrous ethanol, and 7-7.5mL ammonia water is added dropwise, and the concentration of ammonia water is 25-28wt%;
[0012] (2) centrifuging the suspension A obtained in step (1), washing the obtained solid with anhydrous ethanol and deionized water in sequence, and drying at 60-120° C. for 6-24 h to obtain SiO2;
[0013] (3) Mix the SiO2 obtained in step (2) with deionized water, CTAB, Ni(NO3)2.6H2O, and NH3.H2O, and stir for 2-3 hours to obtain solution A;
[0014] Among them, the mass ratio is SiO2: deionized water: CTAB: Ni(NO3)2.6H2O: NH3.H2O = 1: 40-50: 0.8-1: 0.54-0.56: 5.8-6.2;
[0015] (4) transferring the solution A obtained in step (3) into a high pressure reactor and maintaining it at 140-200° C. for 10-36 hours; then centrifuging, washing the obtained solid twice with anhydrous ethanol and deionized water in sequence, and drying at 60-120° C. for 6-24 hours to obtain solid A;
[0016] (5) The solid A obtained in step (4) is calcined at 250-550° C. for 1-4 h to obtain a nickel silicate-derived spherical catalyst A having Ni as the active component.
[0017] Alternatively, method 2 is the preparation of a nickel silicate-derived spherical catalyst whose active components are Ru and Ni, comprising the following steps:
[0018] Steps (1)-(5) are the same as those in method 1;
[0019] (6) dissolving RuCl3 in deionized water to obtain solution B; wherein 0.02-0.06 g of RuCl3 is added to every 1.0-1.5 mL of deionized water;
[0020] (7) adding the nickel silicate-derived spherical catalyst A whose active component is Ni obtained in method 1 to solution B, stirring evenly to obtain a wet solid B; wherein 0.9-1.1 g of catalyst A is added to every 1.2-1.5 mL of solution B;
[0021] (8) placing the solid B obtained in step (7) at room temperature for 12-24 hours, and then drying it in an oven at 40-80° C. for 3-6 hours to obtain a solid C;
[0022] (9) The solid C obtained in step (8) is calcined at 400-600° C. for 1-4 h under a hydrogen atmosphere to obtain a Ru-doped nickel silicate-derived spherical catalyst B.
[0023] The nickel silicate derived spherical catalyst is used for catalytic decomposition of ammonia to produce hydrogen and nitrogen. Specifically, the process comprises the following steps: introducing NH3 and Ar (in a ratio of 3:1) into a fixed bed reactor filled with the nickel silicate derived spherical catalyst at normal pressure and reacting at 300-650°C to obtain hydrogen and nitrogen;
[0024] Space velocity is 6000-120000mL NH3 (g cat *h) -1 .
[0025] The nickel silicate-derived spherical catalyst is characterized in that most of the Ni exists in the form of nickel silicate, the metal particles are small, the dispersion is good, there are interactions between metals and between metals and carriers, and it is not easy to agglomerate at high temperatures.
[0026] The method for preparing the nickel silicate-derived spherical catalyst is characterized in that: Ni(NO3)2.6H2O and SiO2 are firstly hydrothermally formed into nickel silicate Ni3Si4O 10 (OH)2.5H2O, at this time, Ni is evenly distributed in the catalyst, the specific surface area of the carrier is increased, and then Ru is impregnated with equal volume, so that the Ru particles are also evenly distributed.
[0027] The essential features of the present invention are:
[0028] Catalysts available for hydrogen production from ammonia decomposition include precious metals, non-precious metals, transition metals, bimetallics, metal nitrides, metal carbides, and imine catalysts. The main reason for the deactivation of Ru-based catalysts is the sintering and agglomeration of metal particles or hydrogen poisoning. Metal agglomeration also exists on Ni-based catalysts. In the catalyst preparation method for ammonia decomposition hydrogen production system, current technologies mostly use ordinary impregnation methods to prepare supported non-precious metal catalysts, such as Ni, Fe, Mo, etc. The size of the catalyst particles prepared by this method is difficult to control, and the particles are easy to agglomerate at high temperatures, resulting in poor stability. In addition, it is difficult for non-precious metals to achieve the ammonia decomposition performance of the precious metal Ru. The metal loading is large, the resource consumption is large, and the energy utilization rate is low.
[0029] The present invention develops a highly efficient and stable nickel silicate derived spherical catalyst, which uses a hydrothermal method to make Ni react with SiO2 to form a stable nickel silicate Ni3Si4O10 (OH)2.5H2O, and then impregnate a small amount of Ru by equal volume method, so that there is a strong interaction between Ru and Ni, so as to achieve the effect of small particle size and high dispersion. Compared with the supported catalyst prepared by the traditional impregnation method, the catalyst prepared by the present invention has a smaller particle size, a higher dispersion, and is not easy to agglomerate at high temperature. Therefore, it can achieve higher activity and excellent stability in the ammonia decomposition hydrogen production reaction.
[0030] In the present invention, most of the Ni species exist in the form of nickel silicate which is difficult to reduce. There is an interaction between Ni and Si, so the Ni is evenly distributed and is not easy to agglomerate at high temperatures. Under the action of the strong reducing atmosphere in the reaction, the Ni species in the nickel silicate can be further reduced to Ni 0 , providing more active sites for ammonia decomposition. The addition of Ru not only increases the number of active sites, but also strengthens the interaction between Ru and Ni, and between Ni and Si. The synergistic effect of these interactions further enhances the ammonia decomposition performance of the catalyst, and the catalyst can maintain a complete spherical morphology throughout the process, with a certain structural stability.
[0031] The beneficial effects of the present invention are:
[0032] The present invention prepares a nickel silicate-derived spherical catalyst. First, silicon dioxide is obtained by hydrolyzing TEOS under alkaline conditions. Then, nickel silicate is coated on the surface of silicon dioxide by a hydrothermal method to form a nickel silicate-derived catalyst with a mesoporous structure. In addition, the catalyst is doped with Ru to form a nickel silicate-derived catalyst with dual active components of Ru and Ni. The catalyst has a large specific surface area, good dispersion, strong interaction between the metal and the carrier, and a suitable particle size. The results show that the Ru-doped nickel silicate-derived spherical catalyst 1Ru-10Ni / SiO2 has a high specific surface area of 30,000 mL at a relatively high space velocity of 30,000 mL. NH3 (g cat *h) -1 , the ammonia conversion rate at 650°C reached 98%. In the stability test, the ammonia conversion rate of the comparative example 1Ru / SiO2-IW decreased rapidly with the extension of the reaction time, indicating that the catalyst was rapidly deactivated, while the 1Ru-10Ni / SiO2 was able to stably operate at 600°C for 165h, and the ammonia conversion rate hardly decreased, indicating that the catalyst was not deactivated within 165h and had excellent stability. The application of ammonia decomposition catalysts is largely limited by the stability of the catalysts, and the nickel silicate-derived spherical catalyst prepared by the present invention has both good ammonia decomposition performance and excellent stability, and is worth studying. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 11 and 2 are XRD spectra of the nickel silicate-derived spherical catalysts obtained in Examples 1 and 2 and the comparative example catalyst.
[0034] Figure 2 1 and 2 are ammonia decomposition conversion curves of the nickel silicate-derived spherical catalysts obtained in Examples 1 and 2 and the comparative catalyst.
[0035] Figure 3 These are the stability test results of the nickel silicate-derived spherical catalysts obtained in Examples 1 and 2 and the comparative catalyst.
[0036] Figure 4 TEM images of the nickel silicate-derived spherical catalysts obtained in Examples 1 and 2, wherein: Figure 4 (a) is a TEM image of the Ru-doped nickel silicate-derived spherical catalyst obtained in Example 2, Figure 4 (b) is a TEM image of the nickel silicate-derived spherical catalyst obtained in Example 1; Figure 4 (c) is a TEM image of the nickel silicate-derived catalyst obtained in Example 1. DETAILED DESCRIPTION
[0037] The present invention is further described below by way of examples, but is not limited to these examples. Experimental methods for which specific conditions are not specified in the examples are generally carried out under conventional conditions and conditions described in the manual, or under conditions recommended by the manufacturer. The general equipment, materials, reagents, etc. used are all commercially available unless otherwise specified.
[0038] The nickel silicate-derived spherical catalyst, preparation method and application provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0039] The application of the nickel silicate derived spherical catalyst in the ammonia decomposition hydrogen production system comprises the following steps:
[0040] The ammonia decomposition reaction was carried out in a fixed bed reactor connected to an online gas chromatograph. First, 60 mg of a 40-60 mesh catalyst was weighed and placed in a quartz tube, and then 20 mL / min of H2 was introduced. The bed temperature was heated to 550°C (for nickel silicate-derived spherical catalyst) or 450°C (for comparative catalyst) at a heating rate of 5°C / min, and maintained for 1 hour for in-situ reduction. Subsequently, 30 mL / min NH3 and 10 mL / min Ar were introduced, and the ammonia decomposition reaction was carried out at 300-650°C, with a heating rate of 5°C / min, a temperature interval gradient of 50°C, and each temperature point was kept for 1 hour. The test space velocity was 30,000 mL NH3 (g cat *h) -1 .
[0041] The stability test was carried out at 30 mL / min NH3 and 10 mL / min Ar, 600 °C, a heating rate of 5 °C / min, and a test space velocity of 30000 mL NH3 (g cat *h) -1 .
[0042] The nickel silicate in the present invention is Ni3Si4O 10 (OH)2.5H2O.
[0043] Example 1
[0044] 10Ni / SiO2
[0045] 14g of tetraethyl orthosilicate (TEOS) was mixed with 150mL of anhydrous ethanol and 10mL of deionized water, and stirred for 20min. Then, 7.5mL of 25-28wt% NH3.H2O was added dropwise to the above solution, and stirred for 12h. The obtained suspension was centrifuged, and the obtained solid was washed twice with anhydrous ethanol and deionized water in sequence, and dried at 120°C for 24h to obtain silicon dioxide. Then 1g of SiO2, 1g of CTAB, 0.55g of Ni(NO3)2.6H2O, 6g of NH3.H2O (25-28wt%), and 45g of deionized water were mixed and stirred for 2h, and then the mixed solution was transferred to a high-pressure reactor, and the autoclave was sealed and placed in an oven at 180°C for 24h. The solid obtained by centrifugation was washed twice with anhydrous ethanol and deionized water, dried at 120°C for 24 hours, and then calcined at 550°C for 4 hours to obtain a nickel silicate-derived spherical catalyst 10Ni / SiO2. (The theoretical content of Ni is 10wt%)
[0046] The catalyst 10Ni / SiO2 was used for ammonia decomposition reaction. Figure 2 , at 30mL / min NH3 and 10mL / min Ar, the space velocity is 30000mL NH3 (g cat *h) -1 , the conversion rate of ammonia is 98% at 650℃; Figure 3 In the 165h stability test, the ammonia conversion rate of 10Ni / SiO2 dropped from 68% to 61%.
[0047] like Figure 1 As shown, there is Ni3Si4O in 10Ni / SiO2 10The diffraction peak of (OH)2.5H2O indicates that nickel silicate has been successfully generated. At the same time, the intensity of the diffraction peak in 10Ni / SiO2 is significantly weaker than that of the catalyst obtained in the comparative example, indicating that the size of the Ni particles in the catalyst is small and the dispersion is good. Figure 4 (b) Figure 4 As can be seen in (c), 10Ni / SiO2 still maintains a spherical morphology, and metal particles can be seen on the surface.
[0048] Table 1
[0049]
[0050] Table 1 shows the specific surface area, average pore size, average particle size, metal dispersion and Ni of the nickel silicate-derived spherical catalyst and the comparative catalyst before and after the ammonia decomposition reaction. 0 with Ni 2+ Content ratio data. The catalyst after the reaction is added with the suffix -used, for example, the catalyst of Example 1 is loaded into a reaction tube and subjected to an ammonia decomposition reaction at 300-650°C. The catalyst after the reaction is 10Ni / SiO2-used, and the same applies to other catalysts.
[0051] From Table 1, it can be seen that the average particle size of 10Ni / SiO2 is 2.73nm, which is much smaller than that of 10Ni / SiO2-IW (whose average particle size is 17.54nm) obtained in the comparative example, and the dispersion of 10Ni / SiO2 is 29.97%, which is 7.83% for 10Ni / SiO2-IW, which is consistent with the XRD results. From Table 1, it can also be seen that the specific surface area of 10Ni / SiO2 is 129.34m 2 / g, which is much larger than the 10Ni / SiO2-IW obtained in the comparative example (whose specific surface area is 10.52m 2 / g), indicating that 10Ni / SiO2 has more mesoporous structures (average pore size greater than 2nm, less than 50nm is mesopores), which can provide more space for ammonia decomposition reaction on the one hand, and on the other hand, the larger specific surface area is also conducive to the improvement of metal dispersion, thereby enhancing the catalytic ability of the catalyst. It can also be seen from Table 1 that Ni in 10Ni / SiO2 0 / Ni 2+ The Ni content in 10Ni / SiO2 before the reaction is less than 1Ru-10Ni / SiO2-IW, indicating that there is an interaction between Ni and the carrier, making it difficult for Ni species to be reduced. 0 / Ni 2+ was 0.53, and increased to 0.58 after the reaction, indicating that the Ni species in the nickel silicate can be further reduced to Ni 0 , leading to Ni 0 The content of Ni increases 0 / Ni 2+ After the reaction, the particles of the catalyst obtained in the comparative example agglomerated and the particle size increased, while the particle size of 10Ni / SiO2 increased by only 0.22nm after the reaction. This is because the strong interaction between the metal and the carrier inhibits the agglomeration of Ni particles at high temperature, thereby enhancing the stability of the catalyst.
[0052] Example 2
[0053] 1Ru-10Ni / SiO2
[0054] 0.04 g of RuCl3 was dissolved in 1.2 mL of deionized water, and 1 g of 10Ni / SiO2 obtained in Example 1 was added to the above solution and allowed to stand at room temperature for 12 h. The solution was then dried in an oven at 50°C for 6 h, and the obtained solid was calcined at 500°C for 2 h under a hydrogen atmosphere to obtain a Ru-doped nickel silicate-derived spherical catalyst 1Ru-10Ni / SiO2.
[0055] The catalyst 1Ru-10Ni / SiO2 was used for ammonia decomposition reaction. Figure 2 , at 30mL / min NH3 and 10mL / min Ar, the space velocity is 30000mL NH3 (g cat *h) -1 , the conversion rate of ammonia is 98% at 650℃; Figure 3 In the 165h stability test, the ammonia conversion rate corresponding to 1Ru-10Ni / SiO2 hardly decreased.
[0056] like Figure 1 As shown, Ni3Si4O appeared in 1Ru-10Ni / SiO2 10 The diffraction peak of (OH)2.5H2O indicates that nickel silicate has been successfully generated. At the same time, there is no diffraction peak of Ru species in 1Ru-10Ni / SiO2, and the intensity of the diffraction peak of Ni species is significantly weaker than that of the catalyst obtained in the comparative example, indicating that the average size of Ru and Ni particles in the catalyst is small and the dispersion is good. Figure 4 It can be seen that 1Ru-10Ni / SiO2 still maintains a spherical morphology. From Table 1, it can be seen that the average particle size of 1Ru-10Ni / SiO2 is 2.88nm, which is much smaller than the 1Ru-10Ni / SiO2-IW and 1Ru / SiO2-IW obtained in the comparative example (the average particle sizes are 15.87 and 11.03nm respectively); and 1Ru-10Ni / SiO2 has the largest dispersion of 31.58%, while 1Ru-10Ni / SiO2-IW is 8.77% and 1Ru / SiO2-IW is 14.27%. It can also be seen from Table 1 that the specific surface area of 1Ru-10Ni / SiO2 is 124.57m 2 / g, which is much larger than 1Ru-10Ni / SiO2-IW and 1Ru / SiO2-IW obtained in the comparative example (whose specific surface areas are 11.25 and 13.47 m 2 / g), indicating that 1Ru-10Ni / SiO2 has more mesoporous structures. It can also be seen from Table 1 that Ni in 1Ru-10Ni / SiO2 0 / Ni 2+ is 0.56, which is less than 2.83 of 1Ru-10Ni / SiO2-IW, indicating that there is an interaction between Ni and the carrier in 1Ru-10Ni / SiO2, making it difficult for Ni species to be reduced. 0 / Ni 2+ increased to 1.02, indicating that the Ni species in the nickel silicate can be further reduced to Ni 0 , leading to Ni 0 The content of Ni increases 0 / Ni 2+ At the same time, the particle size of 1Ru-10Ni / SiO2 hardly increases after the reaction, because the strong interaction between the metal and the carrier inhibits the agglomeration of Ru and Ni particles at high temperature, thereby enhancing the stability of the catalyst.
[0057] Comparative Example 1
[0058] 1Ru / SiO2-IW
[0059] 0.04 g of RuCl3 was dissolved in 0.8 mL of deionized water, and 1 g of the silicon dioxide obtained in Example 1 was added to the solution and allowed to stand at room temperature for 12 h. The solution was then dried in an oven at 50°C for 6 h, and the obtained solid was calcined at 500°C for 2 h to obtain 1Ru / SiO2-IW.
[0060] The catalyst 1Ru / SiO2-IW was used for ammonia decomposition reaction. Figure 2 , at 30mL / min NH3 and 10mL / min Ar, the space velocity is 30000mL NH3 (g cat *h) -1 , the conversion rate of ammonia at 650℃ is 99%; the stability test results are as follows Figure 3 , the ammonia conversion rate continued to decrease during the 115h stability test, from 97% to 55%.
[0061] Comparative Example 2
[0062] 10Ni / SiO2-IW
[0063] 0.55 g Ni(NO3)2.6H2O was dissolved in 0.8 mL deionized water, and 1 g of the silicon dioxide obtained in Example 1 was added to the above solution and placed at room temperature for 12 h. It was then dried in an oven at 50°C for 6 h, and the obtained solid was calcined at 500°C for 2 h to obtain 10Ni / SiO2-IW.
[0064] The catalyst 10Ni / SiO2-IW was used for ammonia decomposition reaction. Figure 2 , at 30mL / min NH3 and 10mL / min Ar, the space velocity is 30000mL NH3 (g cat *h) -1 , the ammonia conversion rate is 88% at 650℃.
[0065] Comparative Example 3
[0066] 1Ru-10Ni / SiO2-IW
[0067] 0.04 g of RuCl3 was dissolved in 0.8 mL of deionized water, and 1 g of 10Ni / SiO2-IW obtained in Comparative Example 2 was added to the above solution and placed at room temperature for 12 h. The solution was then dried in an oven at 50°C for 6 h, and the obtained solid was calcined at 500°C for 2 h to obtain 1Ru-10Ni / SiO2-IW.
[0068] The catalyst 1Ru-10Ni / SiO2-IW was used for ammonia decomposition reaction. Figure 2 , at 30mL / min NH3 and 10mL / min Ar, the space velocity is 30000mL NH3 (g cat *h) -1 , the ammonia conversion rate is 88% at 650℃.
[0069] The carriers of Comparative Examples 1-3 are nonporous spherical silica with a specific surface area of less than 15 m 2 / g, its surface can anchor Ru, Ni functional groups are relatively few, the metal nanoparticle size on the catalysts obtained in Comparative Examples 1-3 is greater than 10nm, and the dispersion of the catalysts is relatively small, so the catalysts obtained in Comparative Examples 2 and 3 have poor ammonia decomposition activity; since Ru is the best ammonia decomposition catalyst, the ammonia conversion rate corresponding to the catalyst 1Ru / SiO2-IW obtained in Comparative Example 1 is still relatively high. The particle size on the catalysts obtained in Comparative Examples 1-3 continues to increase after one ammonia decomposition reaction, and the agglomeration of particles at high temperatures will inhibit the ammonia decomposition reaction, such as Figure 3As shown, the ammonia conversion rate corresponding to the catalyst 1Ru / SiO2-IW obtained in Comparative Example 1 decreases rapidly with the extension of the reaction time. For the catalysts obtained in Examples 1 and 2, the surface of the spherical SiO2 is etched during the hydrothermal process to form a porous structure, which increases the specific surface area of the catalyst; nickel silicate is successfully generated on the surface of SiO2, and a strong interaction is formed between Ni and Si, which improves the metal dispersion; Ru doping increases the number of active sites on the one hand, and forms an interaction force between Ru and Ni on the other hand, and the particle size of the generated metal particles is less than 3nm. The large specific surface area, metal dispersion, suitable metal particle size and the synergistic effect of the two interaction forces inhibit the agglomeration of particles at high temperatures, improve the ammonia decomposition performance of the catalysts obtained in Examples 1 and 2, and keep the ammonia conversion rate of the catalyst basically stable in the 165h ammonia decomposition test.
[0070] Example 3
[0071] First, SiO2 was prepared, and the other steps were the same as in Example 1, except that the TEOS hydrolysis time was replaced by 10 h instead of 12 h; after obtaining SiO2, it was mixed with CTAB, Ni(NO3)2.6H2O, NH3.H2O, and deionized water for hydrothermal treatment, and the other steps were the same as in Example 1, except that the hydrothermal treatment time was replaced by 36 h instead of 24 h; the other steps were the same as in Example 1, and the catalyst of Example 3 was obtained. The performance of the obtained catalyst was close to that of Example 1.
[0072] Example 4
[0073] The other steps are the same as those of Example 2, except that the amount of RuCl3 is replaced by 0.06g instead of 0.04g, and the catalyst of Example 4 is obtained. The obtained material is used for ammonia decomposition reaction at 30mL / min NH3 and 10mL / min Ar, with a space velocity of 30000mL NH3 (g cat *h) -1 , the ammonia conversion rate is 97% at 650℃.
[0074] Example 5
[0075] The other steps were the same as in Example 2, except that the amount of RuCl3 was replaced by 0.02 g from 0.04 g to obtain the catalyst of Example 5. The obtained material was used for ammonia decomposition reaction at 30 mL / min NH3 and 10 mL / min Ar, with a space velocity of 30000 mL NH3 (g cat *h) -1 , the ammonia conversion rate is 97% at 650℃.
[0076] Example 6
[0077] The other steps are the same as those of Example 2, except that the temperature of the treatment in hydrogen is replaced by 450°C instead of 500°C, and the catalyst of Example 6 is obtained. The obtained material is used for ammonia decomposition reaction at 30 mL / min NH3 and 10 mL / min Ar, with a space velocity of 30000 mL NH3 (g cat *h) -1 , the ammonia conversion rate is 99% at 650℃.
[0078] Example 7
[0079] The other steps are the same as those of Example 2, except that the temperature of the treatment in hydrogen is replaced by 550°C from 500°C, and the catalyst of Example 7 is obtained. The obtained material is used for ammonia decomposition reaction at 30 mL / min NH3 and 10 mL / min Ar, with a space velocity of 30000 mL NH3 (g cat *h) -1 , the ammonia conversion rate is 98% at 650℃.
[0080] The present invention is described in detail above with specific embodiments. Obviously, the described examples are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0081] Matters not covered by the present invention are known technologies.
Claims
1. A nickel silicate-derived spherical catalyst, characterized in that the catalyst comprises two parts: a carrier and an active component; wherein the carrier is silicon dioxide coated with nickel silicate, and the active component is Ni, or Ru and Ni; the mass ratio of the active component to the catalyst is 1-11%; when the active component is two elements, the ratio of Ru to Ni is 1:9-10.
2. The method for preparing the nickel silicate-derived spherical catalyst according to claim 1, characterized in that it comprises any of the following two methods: Method 1 is the preparation of a nickel silicate-derived spherical catalyst whose active component is Ni, comprising the following steps: (1) Tetraethyl orthosilicate (TEOS) is mixed with anhydrous ethanol and deionized water, and stirred at room temperature for 10-20 minutes. Ammonia water is then dropped into the mixture, and the mixture is stirred for 10-15 hours to obtain a suspension A. in, For every 140-150 mL of anhydrous ethanol, add 13-14 g of tetraethyl orthosilicate (TEOS) and 10-12 mL of deionized water, and drop 7-7.5 mL of ammonia water; (2) centrifuging the suspension A obtained in step (1), washing the obtained solid with anhydrous ethanol and deionized water in sequence, and then drying to obtain silicon dioxide (SiO2); (3) Mix the SiO2 obtained in step (2) with deionized water, CTAB, Ni(NO3)2.6H2O, and aqueous ammonia, and stir for 2-3 hours to obtain solution A; Among them, the mass ratio is SiO2: deionized water: CTAB: Ni(NO3)2.6H2O: NH3.H2O = 1: 40-50: 0.8-1: 0.54-0.56: 5.8-6.2; (4) transferring the solution A obtained in step (3) into a high pressure reactor and maintaining it at 140-200° C. for 10-36 hours; then centrifuging, washing the obtained solid twice with anhydrous ethanol and deionized water in sequence, and then drying to obtain solid A; (5) calcining the solid A obtained in step (4) at 250-550° C. for 1-4 h to obtain a nickel silicate-derived spherical catalyst A having Ni as an active component; Alternatively, method 2 is the preparation of a nickel silicate-derived spherical catalyst whose active components are Ru and Ni, comprising the following steps: Steps (1)-(5) are the same as those in method 1; (6) Dissolve RuCl3 in deionized water to obtain solution B; add 0.02-0.06 g of RuCl3 per 1.0-1.5 mL of deionized water; (7) adding the nickel silicate-derived spherical catalyst A whose active component is Ni obtained in step (5) to solution B, stirring evenly to obtain a wet solid B; wherein 0.9-1.1 g of catalyst A is added to every 1.2-1.5 mL of solution B; (8) placing the solid B obtained in step (7) at room temperature for 12-24 hours, and then drying it in an oven at 40-80° C. for 3-6 hours to obtain a solid C; (9) The solid C obtained in step (8) is treated in a hydrogen atmosphere at 400-600° C. for 1-4 h to obtain a Ru-doped nickel silicate-derived spherical catalyst B.
3. The method for preparing a nickel silicate-derived spherical catalyst as claimed in claim 2, characterized in that In steps (1) and (3), the concentration of aqueous ammonia is 25-28 wt %.
4. The method for preparing a nickel silicate-derived spherical catalyst as claimed in claim 2, characterized in that The drying in steps (2) and (4) is carried out at 60-120° C. for 6-24 h.
5. Use of the nickel silicate derived spherical catalyst as claimed in claim 1, characterized in that it is used to catalyze the decomposition of ammonia to produce hydrogen and nitrogen.
6. The use of the nickel silicate derived spherical catalyst as claimed in claim 5, characterized in that it comprises the following steps: introducing NH3 and Ar into a fixed bed reactor containing the nickel silicate derived spherical catalyst, reacting at normal pressure and 300-650°C to obtain hydrogen and nitrogen; the space velocity is 6000-120000mL NH3 (g cat *h) -1 .
Citation Information
Patent Citations
Method and device for preparing polyether amine
CN106810683A
Preparation method for multi-core-shell hollow nickel-nickel silicate catalyst used for reformation of methane and carbon dioxide
CN108636412A
Low-temperature low-pressure direct hydrogenation catalyst for coal-based 1,4-butynediol and preparation method thereof
CN112473669A
Application of nickel-based catalyst in ammonia decomposition hydrogen production reaction
CN117380199A
Negative-electrode active material, method of manufacturing the same, and nonaqueous secondary battery
US20190181433A1