Ultra-low thermal conductivity micro-nano fiber composite VIP core material and preparation method thereof
Through the preparation method of composite fiber aerogel, the problem of insufficient structural strength and stability of VIP core material is solved, the mechanical properties and thermal insulation effect are improved, and high-efficiency thermal insulation and heat resistance are achieved.
Patent Information
- Application Number
- CN202411384137.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing VIP core materials have shortcomings in overall structural strength, stability, mechanical properties and thermal stability, resulting in problems such as unstable structural, low strength, inefficient heat resistance and poor thermal insulation performance.
The preparation method of composite fiber aerogels is adopted, including precise cutting of composite nanofiber membranes, bonding of chromium aluminum phosphate, freeze-drying and high-temperature calcination, forming composite fiber aerogels with porous structure and excellent thermal insulation properties. Spinning technology and aerogeling process improve the mechanical properties and thermal stability of materials.
The overall structural strength and stability of VIP core materials are improved, mechanical properties and thermal insulation effects are enhanced, and structural integrity and thermal insulation performance are ensured at high temperatures.
Smart Images

Figure CN118991173A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of vacuum insulation panels, and in particular to an ultra-low thermal conductivity micro-nano fiber composite VIP core material and a preparation method thereof. Background Art
[0002] VIP board, or vacuum insulation board, is a new type of insulation material based on the principle of vacuum insulation. It consists of three main parts: core material, barrier film, and getter. VIP board has extremely low thermal conductivity and excellent insulation performance, and is usually used in home appliances, storage and transportation, construction and other fields. Among them, the core material is the core material of VIP, which is used to support the structure of VIP and block heat transfer.
[0003] With the advancement of science and technology, people's requirements for energy efficiency are gradually increasing. Traditional insulation materials are difficult to meet the demand for ultra-low thermal conductivity in high-end application fields. Composite fiber aerogel can form a strong three-dimensional network structure through a special preparation process, thereby giving the VIP core material excellent mechanical properties. Through the composite structure of micro-nano fibers, the porosity and specific surface area of the material are effectively increased, thereby reducing the thermal conductivity. Therefore, an ultra-low thermal conductivity micro-nano fiber composite VIP core material and its preparation method are extremely important.
[0004] 1. Patent document CN103277631B discloses a glass fiber vacuum insulation panel nano core material and a preparation method thereof. The above patent realizes point contact connection between the core glass fiber chopped strands, reduces heat convection and radiation, and enhances thermal insulation performance. However, the above patent cannot achieve the function of improving the strength and stability of the overall structure of the VIP core material.
[0005] 2. Patent document CN106046675B discloses a composite core material and preparation method for vacuum insulation panels. The above patent improves the brittleness resistance of the core material, reduces the thermal conductivity and density of the core material, and ensures that the composite core material has good thermal insulation performance, but the above patent cannot achieve good mechanical performance functions.
[0006] 3. Patent document CN110156431B discloses an aerogel-modified cotton fiber vacuum insulation panel core material and a preparation method thereof. The above patent achieves the stability of the performance and structure of the core material and its vacuum insulation panel, so that the vacuum insulation panel has both excellent insulation performance and long life. However, the above patent cannot achieve the function of improving thermal stability.
[0007] 4. Patent document CN103242022B discloses a nano-composite core material for an energy storage vacuum insulation panel and a preparation method thereof. The above patent improves the thermal insulation effect and enables the product to have certain energy storage performance, but the above patent cannot achieve efficient thermal insulation function.
[0008] In summary, the above patents cannot achieve the function of improving the strength and stability of the overall structure of the VIP core material, cannot achieve good mechanical properties, cannot achieve the function of improving thermal stability, and cannot achieve efficient thermal insulation effect, resulting in the problems of unstable VIP core material structure, low strength, poor heat resistance, and poor thermal insulation performance; To this end, the present application proposes an ultra-low thermal conductivity micro-nano fiber composite VIP core material and a preparation method thereof, which can improve the strength and stability of the overall structure of the VIP core material, achieve good mechanical properties, improve thermal stability, and achieve efficient thermal insulation effects. Summary of the invention
[0009] The purpose of the present invention is to provide an ultra-low thermal conductivity micro-nano fiber composite VIP core material and a preparation method thereof, so as to solve the technical problems proposed in the above background technology that the VIP core material cannot achieve the function of improving the strength and stability of the overall structure, cannot achieve good mechanical properties, cannot achieve the function of improving thermal stability, and cannot achieve efficient thermal insulation effect, resulting in unstable VIP core material structure, low strength, heat resistance, and poor thermal insulation performance.
[0010] To achieve the above object, the present invention provides the following technical solution: an ultra-low thermal conductive micro-nano fiber composite VIP core material, comprising a composite fiber aerogel, and a preparation method of the composite fiber aerogel comprises the following steps: Step 1: Precisely cut the composite nanofiber membrane into fiber membrane pieces of the same size and shape, and place the cut membrane pieces into a 0.5%-5% concentration of chromium aluminum phosphate binder aqueous solution for 30 minutes; Step 2: stack the soaked membrane sheets to obtain a layered membrane, freeze the layered membrane using liquid nitrogen, freeze at -120°C for 15 minutes, dry using a freeze dryer to remove moisture, and continue drying in a vacuum drying oven for 24 hours to completely remove moisture; Step 3: Place the freeze-dried sample in an air furnace, heat it to 800°C at 2°C / min, keep it warm for 1h, cool it down at a rate of 3°C / min, cool it to 100°C and then cool it to room temperature to obtain a composite fiber aerogel.
[0011] Preferably, the method for preparing the composite nanofiber membrane comprises the following steps: Step 1: Add nitric acid to a reaction container, dissolve zirconium acetate and polyethylene oxide in the nitric acid, stir evenly, add silica sol, glass fiber slurry, carbon black powder and fiber reinforcement material, and disperse them using a stirrer to obtain a spinning mixed liquid precursor; Step 2: Spinning is performed using an electrospinning device to obtain a single-layer precursor spinning membrane on a receiving device; Step 3: Place the single-layer precursor spinning membrane in a vacuum drying oven and dry it for 5 hours to remove moisture. Place the dried sample in an air furnace for calcination. Heat it to 700°C at 5°C / min, keep it warm for 2 hours, and cool it at a cooling rate of 3°C / min. After cooling to 100°C, cool it to room temperature in the furnace to obtain a composite nanofiber membrane.
[0012] Preferably, the silica sol comprises the following steps: Step 1: Select a clean, dry and impurity-free reaction bottle and slowly add deionized water into the reaction bottle; Step 2: Under stirring conditions, slowly drop ethyl orthosilicate into the deionized water in the reaction bottle, and add acetic acid into the reaction bottle; Step 3: Stir the mixture using a magnetic stirrer to obtain silica sol.
[0013] Preferably, the method for preparing the glass fiber slurry comprises the following steps: pouring glass wool into a beating pool, setting the parameters of a beating machine, and beating to obtain a suspended glass fiber slurry that is entangled and uniformly dispersed.
[0014] Preferably, the preparation method of tetraethyl orthosilicate comprises the following steps: Step 1: Grind and sieve the silicon ash to obtain silicon powder, and disperse the silicon powder in ethanol to form a suspension; Step 2: Slowly add sulfuric acid to the suspension, stir, mix evenly, and heat to obtain ethyl orthosilicate.
[0015] Preferably, the method for preparing glass wool comprises the following steps: Step 1: Mix feldspar, dolomite, soda ash, borax, quartz sand, calcite and broken glass to obtain a mixture; Step 2: Put the mixture into a high-temperature kiln for high-temperature treatment. The mixture gradually becomes molten at high temperature to form glass slurry. After the molten glass slurry is cooled, a uniform, pure and transparent glass pretreatment liquid is obtained. Step 3: Send the glass pretreatment liquid to a centrifuge for treatment. The glass pretreatment liquid rotates at high speed under the action of centrifugal force and passes through the hot plate holes on the centrifuge to form glass fibers. Under the conditions of high-speed and high-temperature gas flow, the glass fibers are heated and stretched to obtain glass wool.
[0016] Preferably, the mass ratio of the aluminum chromium phosphate binder aqueous solution to the diaphragm is 50:1.
[0017] Preferably, the fiber reinforcement material is selected from one of mullite fiber, alumina fiber and polyester chopped filament fiber.
[0018] Preferably, the method for preparing the VIP core material comprises the following steps: S1. Cutting the composite fiber aerogel into specific sizes using a cutting machine to obtain a composite VIP core material; S2. Place the getter at an appropriate position on the VIP core material, and put the VIP core material with the getter into a barrier film bag with three sides sealed.
[0019] Preferably, the method for preparing the VIP core material comprises the following steps: S21, placing the barrier film bag in a vacuum packaging machine, and extracting the air in the bag through a vacuum pumping device to obtain a vacuum insulation panel.
[0020] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention uses a chromium aluminum phosphate binder to bond the composite nanofiber membrane, and after freeze drying and vacuum drying, improves the stability and density of the layered structure, improves the overall performance of the composite fiber aerogel, and achieves an improvement in the strength and stability of the overall structure of the VIP core material; 2. The present invention improves the strength and toughness of the spinning membrane, improves the mechanical properties of the composite fiber aerogel, stabilizes the internal skeleton structure of the aerogel, and improves the resistance to deformation and damage under external forces by adding glass fiber slurry, carbon black powder and fiber reinforcement materials to the spinning mixed liquid precursor; 3. The present invention performs high-temperature calcination treatment on the precursor film after spinning, and the zirconium acetate is converted into zirconium oxide to form a stable crystal structure. The high-temperature treatment promotes the densification and phase change inside the material, enhances the mechanical properties and thermal stability of the material, and enables the VIP core material to maintain structural integrity and stability at high temperatures; 4. The composite nanofiber membrane prepared by the spinning technology of the present invention, combined with the subsequent calcination treatment and aerogel process, forms a composite fiber aerogel with a porous structure and excellent thermal insulation performance. The porous structure of the aerogel effectively limits the thermal conduction of gas molecules and achieves ultra-low thermal conductivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a schematic diagram of the preparation process of the composite fiber aerogel of the present invention; Figure 2 This is a schematic diagram of the preparation process of the composite nanofiber membrane of the present invention; Figure 3 This is a schematic diagram of the preparation process of the silica sol of the present invention; Figure 4 This is a schematic diagram of the preparation process of tetraethyl orthosilicate of the present invention; Figure 5 This is a schematic diagram of the glass fiber slurry preparation process of the present invention; Figure 6This is a schematic diagram of the glass wool preparation process of the present invention; Figure 7 is a schematic diagram of a fiber-reinforced material of the present invention; Figure 8 It is a schematic diagram of the VIP core material preparation process of the present invention. DETAILED DESCRIPTION
[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Example 1, please refer to Figure 1 - Figure 7 , an ultra-low thermal conductive micro-nano fiber composite VIP core material, comprising a composite fiber aerogel, and a preparation method of the composite fiber aerogel comprises the following steps: Step 1: Add nitric acid to a reaction container, dissolve zirconium acetate and polyethylene oxide in nitric acid, stir evenly, add silica sol, glass fiber slurry, carbon black powder and fiber reinforcement material, use a stirrer to disperse, obtain a spinning mixture precursor, use an electrospinning machine to spin, obtain a single-layer precursor spinning membrane on a receiving device, place the single-layer precursor spinning membrane in a vacuum drying oven, remove moisture, dry for 5 hours, place the dried sample in an air furnace for calcination, heat to 700°C at 5°C / min, keep warm for 2 hours, cool at a rate of 3°C / min, cool to 100°C and then cool to room temperature to obtain a composite nanofiber membrane; Step 2: Precisely cut the composite nanofiber membrane into fiber membrane sheets of the same size and shape, place the cut membrane sheets in a 1% concentration of chromium aluminum phosphate binder aqueous solution, soak for 30 minutes, stack the soaked membrane sheets to obtain a layered structure membrane, freeze the layered structure membrane with liquid nitrogen, freeze at -120°C for 15 minutes, and after freezing, use a freeze dryer to dry it to remove moisture. After drying, use a vacuum drying oven to continue drying for 24 hours to completely remove moisture; Step 3: Place the freeze-dried sample in an air furnace, heat it to 800°C at 2°C / min, keep it warm for 1h, cool it down at a rate of 3°C / min, cool it down to 100°C and then cool it down to room temperature to obtain a composite fiber aerogel; Furthermore, during the immersion and stacking process, the chromium aluminum phosphate binder tightly binds the fibrous membrane sheets, thereby maintaining the integrity and stability of the membrane during subsequent processes such as freeze drying and calcination. During the freeze drying process in the layered structure membrane, the liquid water in the layered structure membrane solidifies into ice crystals, and the ice crystals squeeze the nanofibers and the chromium aluminum phosphate binder in the solution, thereby aggregating the nanofibers and chromium aluminum phosphate in the solution. Under the influence of the fiber force, the chromium aluminum phosphate is adsorbed on the surface of the nanofibers. Since the nanofibers have a high specific surface area and a porous structure, the chromium aluminum phosphate binder molecules can penetrate into the pores of the fibers and form bridges between the fibers, thereby forming a fiber aerogel solvent with a porous structure in which the fibers are entangled with each other. Through high-temperature curing treatment, the chromium aluminum phosphate binder undergoes a ceramic transformation, which enhances the bonding force between the fibers and improves the overall strength and thermal stability of the fiber aerogel, so that the VIP core material prepared from the composite fiber aerogel not only has good temperature resistance, but the multi-layer nanofiber structure stacked layer by layer improves the mechanical properties of the core material at extreme temperatures, giving it good mechanical properties.
[0024] Example 2, please refer to Figure 1 , Figure 2 , Figure 3 and Figure 4 , an ultra-low thermal conductive micro-nano fiber composite VIP core material, comprising a composite fiber aerogel, and a preparation method of the composite fiber aerogel comprises the following steps: Step 1: Add nitric acid to a reaction container, dissolve zirconium acetate and polyethylene oxide in the nitric acid, stir evenly, add silica sol, use a stirrer to disperse, obtain a spinning mixture precursor, use an electrospinning machine to spin, and obtain a single-layer precursor spinning membrane on a receiving device. Place the single-layer precursor spinning membrane in a vacuum drying oven to remove moisture and dry for 5 hours. Place the dried sample in an air furnace for calcination, heat to 700°C at 5°C / min, keep warm for 2 hours, and cool at a rate of 3°C / min. After cooling to 100°C, cool to room temperature in the furnace to obtain a composite nanofiber membrane; Step 2: Precisely cut the composite nanofiber membrane into fiber membrane sheets of the same size and shape, place the cut membrane sheets in a 0.5% concentration of chromium aluminum phosphate binder aqueous solution, soak for 30 minutes, stack the soaked membrane sheets to obtain a layered structure membrane, freeze the layered structure membrane with liquid nitrogen, freeze at -120°C for 15 minutes, and after freezing, use a freeze dryer to dry it to remove moisture. After drying, use a vacuum drying oven to continue drying for 24 hours to completely remove moisture; Step 3: Place the freeze-dried sample in an air furnace, heat it to 800°C at 2°C / min, keep it warm for 1h, cool it down at a rate of 3°C / min, cool it down to 100°C and then cool it down to room temperature to obtain a composite fiber aerogel; Furthermore, the silica nanoparticles in the silica sol are evenly dispersed in the fibers during the spinning process, forming bridges between the fibers and enhancing the connection strength between the fibers, thereby improving the structural stability and mechanical properties of the entire fiber membrane. During the calcination process, the silica nanoparticles in the silica sol release gas to form pores. The increase in pores reduces the path of heat conduction, thereby reducing the thermal conductivity of the fiber membrane. Zirconium acetate is converted into zirconium oxide during the calcination process. The nanoparticles of zirconium oxide improve the mechanical properties of the fiber membrane. At the same time, the thermal conductivity of zirconium oxide is relatively low. The uniform distribution of zirconium oxide nanoparticles in the fiber membrane can form more thermal resistance interfaces, increase the difficulty of heat conduction, and thus reduce the thermal conductivity of the fiber membrane. In addition, the silica in the silica sol interacts with zirconium oxide to form a complex and stable porous structure, which further reduces the thermal conductivity of the fiber membrane, thereby obtaining an ultra-low conductivity VIP core material with excellent mechanical properties.
[0025] Example 3, please refer to Figure 1 , Figure 2 , Figure 5 and Figure 6 , an ultra-low thermal conductive micro-nano fiber composite VIP core material, comprising a composite fiber aerogel, and a preparation method of the composite fiber aerogel comprises the following steps: Step 1: Add nitric acid to a reaction container, dissolve zirconium acetate and polyethylene oxide in nitric acid, stir evenly, add silica sol and glass fiber slurry, use a stirrer to disperse, obtain a spinning mixture precursor, use an electrospinning machine to spin, obtain a single-layer precursor spinning membrane on a receiving device, place the single-layer precursor spinning membrane in a vacuum drying oven, remove moisture, dry for 5 hours, place the dried sample in an air furnace for calcination, heat to 700°C at 5°C / min, keep warm for 2 hours, cool at a rate of 3°C / min, cool to 100°C and then cool to room temperature to obtain a composite nanofiber membrane; Step 2: Precisely cut the composite nanofiber membrane into fiber membrane sheets of the same size and shape, place the cut membrane sheets in a 2% concentration of chromium aluminum phosphate binder aqueous solution, soak for 30 minutes, stack the soaked membrane sheets to obtain a layered structure membrane, freeze the layered structure membrane with liquid nitrogen, freeze at -120°C for 15 minutes, dry it with a freeze dryer to remove moisture, and continue drying in a vacuum drying oven for 24 hours to completely remove moisture; Step 3: Place the freeze-dried sample in an air furnace, heat it to 800°C at 2°C / min, keep it warm for 1h, cool it down at a rate of 3°C / min, cool it down to 100°C and then cool it down to room temperature to obtain a composite fiber aerogel; Furthermore, during the preparation of the spinning mixture precursor, the fibers in the glass fiber slurry are evenly dispersed in the nanofiber matrix to form a solid skeleton. Electrospinning spins out the glass fibers and nanofibers to form a composite fiber membrane with a reinforced structure. The glass fibers have excellent heat resistance and can maintain the stability of their physical and chemical properties in a high temperature environment, thereby improving the heat resistance of the composite nanofiber membrane.
[0026] Example 4, please refer to Figure 1 and Figure 2 , an ultra-low thermal conductive micro-nano fiber composite VIP core material, comprising a composite fiber aerogel, and a preparation method of the composite fiber aerogel comprises the following steps: Step 1: Add nitric acid to a reaction container, dissolve zirconium acetate and polyethylene oxide in the nitric acid, stir evenly, add silica sol and carbon black powder, use a stirrer to disperse, obtain a spinning mixture precursor, use an electrospinning machine to spin, obtain a single-layer precursor spinning membrane on a receiving device, place the single-layer precursor spinning membrane in a vacuum drying oven, remove moisture, dry for 5 hours, place the dried sample in an air furnace for calcination, heat to 700°C at 5°C / min, keep warm for 2 hours, cool at a rate of 3°C / min, cool to 100°C and then cool to room temperature to obtain a composite nanofiber membrane; Step 2: Precisely cut the composite nanofiber membrane into fiber membrane sheets of the same size and shape, place the cut membrane sheets in a 3% concentration of chromium aluminum phosphate binder aqueous solution, soak for 30 minutes, stack the soaked membrane sheets to obtain a layered structure membrane, freeze the layered structure membrane with liquid nitrogen, freeze at -120°C for 15 minutes, and after freezing, use a freeze dryer to dry it to remove moisture. After drying, use a vacuum drying oven to continue drying for 24 hours to completely remove moisture; Step 3: Place the freeze-dried sample in an air furnace, heat it to 800°C at 2°C / min, keep it warm for 1h, cool it down at a rate of 3°C / min, cool it down to 100°C and then cool it down to room temperature to obtain a composite fiber aerogel; Furthermore, carbon black particles form a large number of interface scattering and thermal resistance barriers in the fiber membrane, which can scatter and hinder the conduction of heat between fibers, thereby reducing the heat conduction efficiency and improving the thermal insulation performance. At the same time, carbon black powder can absorb and convert radiant heat energy, reduce the transfer of radiant heat, and further enhance the thermal insulation effect.
[0027] Example 5, please refer to Figure 1 , Figure 2 and Figure 7 , an ultra-low thermal conductive micro-nano fiber composite VIP core material, comprising a composite fiber aerogel, and a preparation method of the composite fiber aerogel comprises the following steps: Step 1: Add nitric acid to a reaction container, dissolve zirconium acetate and polyethylene oxide in the nitric acid, stir evenly, add silica sol and fiber reinforcement material, use a stirrer to disperse, obtain a spinning mixture precursor, use an electrospinning machine to spin, obtain a single-layer precursor spinning membrane on a receiving device, place the single-layer precursor spinning membrane in a vacuum drying oven, remove moisture, dry for 5 hours, place the dried sample in an air furnace for calcination, heat to 700°C at 5°C / min, keep warm for 2 hours, cool at a rate of 3°C / min, cool to 100°C and then cool to room temperature to obtain a composite nanofiber membrane; Step 2: Precisely cut the composite nanofiber membrane into fiber membrane sheets of the same size and shape, place the cut membrane sheets in a 4% concentration of chromium aluminum phosphate binder aqueous solution, soak for 30 minutes, stack the soaked membrane sheets to obtain a layered structure membrane, freeze the layered structure membrane with liquid nitrogen, freeze at -120°C for 15 minutes, and after freezing, use a freeze dryer to dry it to remove moisture. After drying, use a vacuum drying oven to continue drying for 24 hours to completely remove moisture; Step 3: Place the freeze-dried sample in an air furnace, heat it to 800°C at 2°C / min, keep it warm for 1h, cool it down at a rate of 3°C / min, cool it down to 100°C and then cool it down to room temperature to obtain a composite fiber aerogel; Furthermore, the fiber-reinforced material forms a three-dimensional network structure through interweaving with nanofibers, which can withstand and disperse external stress and prevent the fiber membrane from being damaged due to excessive local stress. The fiber-reinforced material and the nanofiber matrix are combined with each other to form a stable interface, which can transmit stress and prevent the expansion of cracks, further improving the strength and toughness of the fiber membrane.
[0028] Example 6, please refer to Figure 1 and Figure 8 , an ultra-low thermal conductive micro-nano fiber composite VIP core material, comprising a composite fiber aerogel, and a preparation method of the composite fiber aerogel comprises the following steps: Step 1: Add silica sol, glass fiber slurry, carbon black powder and fiber reinforcement material into a reaction container, use a stirrer to disperse, obtain a spinning mixture precursor, use an electrospinning machine to spin, and obtain a single-layer precursor spinning membrane on a receiving device. Place the single-layer precursor spinning membrane in a vacuum drying oven to remove moisture and dry for 5 hours. Place the dried sample in an air furnace for calcination, heat to 700°C at 5°C / min, keep warm for 2 hours, and cool at a rate of 3°C / min. After cooling to 100°C, cool to room temperature in the furnace to obtain a composite nanofiber membrane; Step 2: Precisely cut the composite nanofiber membrane into fiber membrane sheets of the same size and shape, place the cut membrane sheets in a 5% concentration of chromium aluminum phosphate binder aqueous solution, soak for 30 minutes, stack the soaked membrane sheets to obtain a layered structure membrane, freeze the layered structure membrane with liquid nitrogen at -120°C for 15 minutes, and after freezing, use a freeze dryer to dry it to remove moisture. After drying, use a vacuum drying oven to continue drying for 24 hours to completely remove moisture; Step 3: Place the freeze-dried sample in an air furnace, heat it to 800°C at 2°C / min, keep it warm for 1h, cool it down at a rate of 3°C / min, cool it down to 100°C and then cool it down to room temperature to obtain a composite fiber aerogel; Step 4: Use a cutting machine to cut the composite fiber aerogel into specific sizes to obtain a composite VIP core material, place the getter at an appropriate position on the VIP core material, put the VIP core material with the getter into a barrier film bag with three sides sealed, place the barrier film bag in a vacuum packaging machine, and extract the air in the bag through a vacuum device to obtain a vacuum insulation panel; Furthermore, the composite fiber aerogel is composed of micro-nano fibers with a large number of pores and air layers inside, which greatly hinders heat conduction and convection heat transfer, so that the VIP core material prepared from the composite fiber aerogel has an ultra-low thermal conductivity, allowing the VIP panel to achieve efficient thermal insulation while having good structural stability and mechanical strength.
[0029] Comparative Example 1, an ultra-low thermal conductive micro-nano fiber composite VIP core material, comprising a composite fiber aerogel, wherein the preparation method of the composite fiber aerogel comprises the following steps: Step 1: Add nitric acid to a reaction container, dissolve zirconium acetate and polyethylene oxide in the nitric acid, stir evenly, add glass fiber slurry, carbon black powder and fiber reinforcement material, use a stirrer to disperse, obtain a spinning mixture precursor, use an electrospinning machine to spin, obtain a single-layer precursor spinning membrane on a receiving device, place the single-layer precursor spinning membrane in a vacuum drying oven, remove moisture, dry for 5 hours, place the dried sample in an air furnace for calcination, heat to 700°C at 5°C / min, keep warm for 2 hours, cool at a rate of 3°C / min, cool to 100°C and then cool to room temperature to obtain a composite nanofiber membrane; Step 2: Precisely cut the composite nanofiber membrane into fiber membrane sheets of the same size and shape, place the cut membrane sheets in a 1% concentration of chromium aluminum phosphate binder aqueous solution, soak for 30 minutes, stack the soaked membrane sheets to obtain a layered structure membrane, freeze the layered structure membrane with liquid nitrogen, freeze at -120°C for 15 minutes, and after freezing, use a freeze dryer to dry it to remove moisture. After drying, use a vacuum drying oven to continue drying for 24 hours to completely remove moisture; Step 3: Place the freeze-dried sample in an air furnace, heat it to 800°C at 2°C / min, keep it warm for 1h, cool it down at a rate of 3°C / min, cool it to 100°C and then cool it to room temperature to obtain a composite fiber aerogel.
[0030] Performance Testing Test 1 Thermal insulation performance test: The composite fiber aerogel samples prepared in Examples 1 to 6 and Comparative Example 1 were cut into square samples with a size of 10 mm × 10 mm × 5 mm, and the square samples were placed on the test bench of a flash thermal conductivity meter. The laser pulse was started, and the temperature change on the other side of the sample over time was recorded, and the thermal conductivity of the sample was calculated.
[0031] Test 2 Tensile strength performance test: The composite nanofiber membrane samples prepared in Example 1 to Example 3 and Example 5 were cut into samples with a size of 20 mm×15 mm, and the samples were clamped on the upper and lower clamps of a tensile testing machine, and the tensile load when the samples were destroyed was recorded.
[0032] Table 1 Test results of thermal insulation performance test Example Thermal conductivity (W / m·K) Example 1 0.030 Example 2 0.034 Example 3 0.036 Example 4 0.037 Example 5 0.041 Example 6 0.046 Comparative Example 1 0.035 Table 2 Test results of tensile strength test Example Tensile strength (KPa) Example 1 232.4 Example 2 182.5 Example 3 196.7 Example 5 201.6 Working principle: By adding glass fiber slurry, carbon black powder and fiber reinforcement materials to the spinning mixture precursor, not only the strength and toughness of the spinning membrane are improved, but also the final composite fiber aerogel has better mechanical properties. These reinforcement materials can form a stable skeleton structure inside the aerogel to resist deformation and damage under external forces. Nanofibers have extremely high specific surface area and microstructure, which can effectively reduce thermal conductivity, thereby reducing heat conduction; The silica sol is evenly mixed with other ingredients during the spinning process. After electrospinning to form a precursor spinning membrane and in the subsequent calcination process, the silica sol undergoes pyrolysis and phase change, and finally forms nano-scale silica particles. These particles are evenly distributed in the fiber network to form a dense microporous structure, thereby improving the thermal insulation performance and mechanical strength of the material. The organic part of the zirconium acetate molecule is pyrolyzed and removed to obtain zirconium oxide, which works together with the silica particles to form a dense microporous structure. The phase change characteristics of zirconium oxide enable the material to absorb more heat at high temperatures, thereby further improving the thermal insulation effect.
[0033] The chromium aluminum phosphate binder can effectively bond the contact points between the composite nanofiber membranes to form a stable layered structure, which not only improves the bonding force between the membranes, but also enhances the strength and stability of the entire layered structure, avoiding the membrane slippage or separation that may occur during the stacking, freezing, drying and other processes. The integrity of the structure is maintained during the freeze-drying process, so that the final composite fiber aerogel has a uniform layered structure, thereby maintaining the uniform distribution and stability of the pores inside the aerogel, further improving its thermal insulation performance; the porous structure of the composite fiber aerogel gives it extremely low thermal conductivity, and the pore structure in the aerogel effectively limits the thermal conduction of gas molecules, thereby achieving excellent thermal insulation performance. Carbon black powder, as a sunshade, further enhances the thermal insulation effect through its high reflectivity and low emissivity characteristics.
[0034] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
Claims
1. An ultra-low thermal conductivity micro-nano fiber composite VIP core material, characterized by: The invention comprises a composite fiber aerogel, and the preparation method of the composite fiber aerogel comprises the following steps: Step 1: Precisely cut the composite nanofiber membrane into fiber membrane pieces of the same size and shape, and place the cut membrane pieces into a 0.5%-5% concentration of chromium aluminum phosphate binder aqueous solution for 30 minutes; Step 2: stack the soaked membrane sheets to obtain a layered membrane, freeze the layered membrane using liquid nitrogen, freeze at -120°C for 15 minutes, dry using a freeze dryer to remove moisture, and continue drying in a vacuum drying oven for 24 hours to completely remove moisture; Step 3: Place the freeze-dried sample in an air furnace, heat it to 800°C at 2°C / min, keep it warm for 1h, cool it down at a rate of 3°C / min, cool it to 100°C and then cool it to room temperature to obtain a composite fiber aerogel.
2. The ultra-low thermal conductivity micro-nano fiber composite VIP core material according to claim 1, characterized in that: The preparation method of the composite nanofiber membrane comprises the following steps: Step 1: Add nitric acid to a reaction container, dissolve zirconium acetate and polyethylene oxide in the nitric acid, stir evenly, add silica sol, glass fiber slurry, carbon black powder and fiber reinforcement material, and disperse them using a stirrer to obtain a spinning mixed liquid precursor; Step 2: Spinning is performed using an electrospinning device to obtain a single-layer precursor spinning membrane on a receiving device; Step 3: Place the single-layer precursor spinning membrane in a vacuum drying oven and dry it for 5 hours to remove moisture. Place the dried sample in an air furnace for calcination. Heat it to 700°C at 5°C / min, keep it warm for 2 hours, and cool it at a cooling rate of 3°C / min. After cooling to 100°C, cool it to room temperature in the furnace to obtain a composite nanofiber membrane.
3. The ultra-low thermal conductivity micro-nano fiber composite VIP core material according to claim 2, characterized in that: The silica sol comprises the following steps: Step 1: Select a clean, dry and impurity-free reaction bottle and slowly add deionized water into the reaction bottle; Step 2: Under stirring conditions, slowly drop ethyl orthosilicate into the deionized water in the reaction bottle, and add acetic acid into the reaction bottle; Step 3: Stir the mixture using a magnetic stirrer to obtain silica sol.
4. The ultra-low thermal conductivity micro-nano fiber composite VIP core material according to claim 2, characterized in that: The glass fiber slurry preparation method comprises the following steps: pouring glass wool into a beating pool, setting parameters of a beating machine, and beating to obtain non-entangled and uniformly dispersed suspended glass fiber slurry.
5. The ultra-low thermal conductivity micro-nano fiber composite VIP core material according to claim 3, characterized in that: The preparation method of tetraethyl orthosilicate comprises the following steps: Step 1: Grind and sieve the silicon ash to obtain silicon powder, and disperse the silicon powder in ethanol to form a suspension; Step 2: Slowly add sulfuric acid to the suspension, stir, mix evenly, and heat to obtain ethyl orthosilicate.
6. The ultra-low thermal conductivity micro-nano fiber composite VIP core material according to claim 4, characterized in that: The preparation method of the glass wool comprises the following steps: Step 1: Mix feldspar, dolomite, soda ash, borax, quartz sand, calcite and broken glass to obtain a mixture; Step 2: Put the mixture into a high-temperature kiln for high-temperature treatment. The mixture gradually becomes molten at high temperature to form glass slurry. After the molten glass slurry is cooled, a uniform, pure and transparent glass pretreatment liquid is obtained. Step 3: Send the glass pretreatment liquid to a centrifuge for treatment. The glass pretreatment liquid rotates at high speed under the action of centrifugal force and passes through the hot plate holes on the centrifuge to form glass fibers. Under the conditions of high-speed and high-temperature gas flow, the glass fibers are heated and stretched to obtain glass wool.
7. The ultra-low thermal conductivity micro-nano fiber composite VIP core material according to claim 1, characterized in that: The mass ratio of the chromium aluminum phosphate binder aqueous solution to the membrane is 50:
1.
8. The ultra-low thermal conductivity micro-nano fiber composite VIP core material according to claim 1, characterized in that: The fiber reinforcement material is selected from one of mullite fiber, alumina fiber and polyester chopped filament fiber.
9. A method for preparing an ultra-low thermal conductivity micro-nano fiber composite VIP core material, applicable to an ultra-low thermal conductivity micro-nano fiber composite VIP core material according to any one of claims 1 to 8, characterized in that: The preparation method of the VIP core material comprises the following steps: S1. Cutting the composite fiber aerogel into specific sizes using a cutting machine to obtain a composite VIP core material; S2. Place the getter at an appropriate position on the VIP core material, and put the VIP core material with the getter into a barrier film bag with three sides sealed.
10. The method for preparing an ultra-low thermal conductive micro-nano fiber composite VIP core material according to claim 9, characterized in that: The preparation method of the VIP core material comprises the following steps: S21, placing the barrier film bag in a vacuum packaging machine, and extracting the air in the bag through a vacuum pumping device to obtain a vacuum insulation panel.