Tetrahydronaphthol-phosphine late transition metal complex as well as preparation method and application thereof
By preparing a tetrahydronaphthol-phosphine post-transition metal complex, the problem of low activity of existing catalysts in ethylene polymerization at high temperatures was solved, realizing efficient ethylene polymerization and polar monomer copolymerization, with good thermal stability and economy.
Patent Information
- Application Number
- CN202310573961.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-22
AI Technical Summary
Existing post-transition metal catalysts exhibit low activity in ethylene polymerization at high temperatures, cannot be directly homopolymerized with ethylene, and cannot coordinate copolymerize with acrylates. The preparation methods are complex and costly.
Develop tetrahydronaphthol-phosphine post-transition metal complexes, which react with M metal compounds through the reaction of compounds with specific structural formula (I) to form catalysts with good thermal stability, suitable for ethylene polymerization and polar monomer copolymerization.
By maintaining high ethylene polymerization activity at higher temperatures, polymers with narrow molecular weight distributions can be obtained, and the preparation method is simple and low in cost.
Smart Images

Figure CN118994260A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of olefin polymerization catalysts, and in particular to a tetralinol-phosphine late transition metal complex and a preparation method and application thereof. Background Art
[0002] Polyethylene materials are widely used due to their good chemical resistance, low price, simple preparation, low density, and good mechanical properties. Among them, late transition metal catalysts have attracted widespread attention in the scientific research community due to their high ethylene homopolymerization activity, good tolerance to polar groups, and the ability to directly coordinate copolymerize olefins with polar monomers under relatively mild conditions (see, for example, S. D. Ittel, Chem Rev, 2000, 100 (4), 1169-1203; H. Mu, Coord Chem Rev, 2021, 435, 213802).
[0003] In 1995, Brookhart et al. reported a class of α-diimine Ni(II) complexes that can polymerize ethylene with high activity. The cationic α-diimine palladium complexes they developed were successfully applied to the copolymerization of ethylene or propylene with acrylates. Due to the unique "β-H elimination" and "chain walking" characteristics, the polar groups in the highly branched copolymers are mostly located at the chain ends (see, for example, M. Brookhart, J Am Chem Soc, 1996, 118(1), 267-268). In 2000, Grubbs et al. developed a salicylaldehyde imine neutral nickel catalyst with good tolerance to heteroatoms, which achieved the copolymerization of ethylene and functionalized norbornene to form a linear copolymer with high insertion rate (see, for example, RH Grubbs, Science, 2000, 287, 460-462). In 2002, Drent et al. reported that the electronically asymmetric neutral phosphine sulfonic acid neutral palladium complex is another classic catalyst for ethylene homo / copolymerization (see, for example, E. Drent, Chem Commun, 2002, 7, 744-745), which can catalyze the copolymerization of ethylene with a variety of simple industrial bulk polar monomers (acrylonitrile, vinyl acetate, acrylic acid and acrylates, etc.) to form linear copolymers (see, for example, E. Drent, Chem. Commun. 2002, 7, 744-745); Mecking, Nozaki, Jordon and other research groups have conducted in-depth research on the copolymerization reaction behavior and catalytic mechanism of ethylene initiated by this type of catalyst, further promoting the development of late transition metal catalysts.
[0004] However, when the above catalyst is used at high temperature, its ethylene polymerization activity is low, it cannot directly homopolymerize with ethylene and cannot be coordinated and copolymerized with acrylic esters. At the same time, its preparation method is complicated and the cost is high. Summary of the invention
[0005] The invention aims to provide a tetralinol-phosphine late transition metal complex and a preparation method and application thereof. The tetralinol-phosphine late transition metal complex has good thermal stability. In particular, the tetralinol-phosphine late transition metal complex can still maintain high ethylene polymerization activity at a relatively high temperature, and the molecular weight distribution of the obtained polymer is relatively narrow. The preparation method is simple and the cost is relatively low.
[0006] In order to achieve the above object, the present invention provides a tetralin-phosphine late transition metal complex, the structural formula of which is shown in formula (I):
[0007]
[0008] M is selected from Group VIII metals, R7-R 11 Each is independently selected from hydrogen, halogen, hydroxyl and substituted or unsubstituted C1-C15 hydrocarbon group, R2 and R3 are independently selected from halogen, C1-C10 hydrocarbon group, P(R4)3, NR5R6 or OR 12 R 13 , or R2 and R3 are connected to each other to form an eight-membered ring or an eight-membered ring system;
[0009] Wherein R4 is selected from substituted or unsubstituted C1-C10 alkyl and substituted or unsubstituted C6-C10 aryl;
[0010] R5 and R6 are each independently selected from a C1-C10 hydrocarbon group, or R5, R6 and N are connected to each other to form a five-membered ring or a six-membered ring;
[0011] R 12 and R 13 Each independently selected from C1-C10 hydrocarbon group, or R 12 , R 13 Connected with O to form a five-membered ring or a six-membered ring.
[0012] Preferably, M is selected from nickel or palladium.
[0013] Preferably, R7-R 11 Each is independently selected from hydrogen, halogen, hydroxyl, substituted or unsubstituted C1-C15 alkyl and substituted or unsubstituted C6-C15 aryl, and the substituent is selected from halogen, hydroxyl, C1-C10 alkyl, halogenated C1-C10 alkyl, C1-C10 alkoxy or halogenated C1-C10 alkoxy.
[0014] Preferably, R2 and R3 are each independently selected from halogen, C1-C8 hydrocarbon, P(R4)3, NR5R6 or OR 12 R 13, or R2 and R3 are connected to form an eight-membered ring; wherein R4 is selected from substituted or unsubstituted C1-C10 alkyl and substituted or unsubstituted C6-C10 aryl; R5 and R6 are each independently selected from C1-C6 hydrocarbon group, or R5, R6 and N are connected to form a five-membered ring or a six-membered ring; R 12 and R 13 Each independently selected from C1-C6 hydrocarbon group, or R 12 , R 13 Connected with O to form a five-membered ring or a six-membered ring.
[0015] Preferably, the substituents are selected from halogen, hydroxy, C1-C6 alkyl, halogenated C1-C6 alkyl, C1-C6 alkoxy or halogenated C1-C6 alkoxy.
[0016] Preferably, the C1-C6 alkyl group is selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, n-pentyl, isopentyl, n-hexyl, isohexyl or 3,3-dimethylbutyl.
[0017] Preferably, the C1-C6 alkoxy group is selected from methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, n-pentoxy, isopentoxy, n-hexoxy, isohexoxy or 3,3-dimethylbutoxy.
[0018] Preferably, the halogen is selected from fluorine, chlorine, bromine or iodine.
[0019] The second aspect of the present invention provides a method for preparing the above-mentioned tetrahydronaphthol-phosphine late transition metal complex, which comprises the following steps:
[0020] (1) reacting the compound represented by formula (II) with the compound represented by formula (III) to obtain a ligand;
[0021] (2) reacting the ligand with an M metal compound;
[0022]
[0023] Wherein the metal M is selected from Group VIII metals, preferably nickel or palladium; R7-R 11 The definition of is the same as described above.
[0024] Preferably, the M metal compound is selected from one or more of dimethyldipyridinium nickel, bis(1,5-cyclooctadiene)nickel, dichlorotetrapyridinium nickel, ethylene glycol dimethyl ether nickel bromide, ethylene glycol dimethyl ether nickel chloride, dichlorobis(trimethylphosphine)nickel, bis(pyridine)bis[(trimethylsilyl)methyl]nickel, bromo(phenyl)(N,N,N',N'-tetramethyl-1,2-ethylenediamine)nickel, dibenzyldipyridinium nickel, phenyl(trimethylphosphine)nickel bromide, phenyl(triethylphosphine)nickel chloride, diphenylbis(trimethylphosphine)nickel, dichlorobis(trimethylphosphine)nickel, dimethyldipyridinium palladium, dichlorodipyridinium palladium, bis(pyridine)bis[(trimethylsilyl)methyl]palladium, dibenzyldipyridinium palladium, methyl-1,5-cyclooctadiene-palladium chloride and dimethyl(N,N,N',N'-tetramethyl-1,2-ethylenediamine)palladium.
[0025] Preferably, the reaction in step (2) is carried out in the presence of a reaction solvent, and the reaction solvent is toluene or tetrahydrofuran.
[0026] The third aspect of the present invention provides the use of the above-mentioned tetralinol-phosphine late transition metal complex in olefin polymerization.
[0027] Preferably, the olefins include ethylene and α-olefins containing polar groups.
[0028] The fourth aspect of the present invention provides an olefin polymerization method, comprising carrying out an olefin polymerization reaction in the presence of the above-mentioned tetralinol-phosphine late transition metal complex.
[0029] Preferably, the polymerization reaction temperature is -78°C to 200°C, more preferably -20°C to 150°C; the polymerization pressure is 0.01 to 10 MPa, more preferably 0.01 to 5 MPa.
[0030] Through the above technical scheme, the tetralin-phosphine late transition metal complex of the present invention has good thermal stability. In particular, the tetralin-phosphine late transition metal complex can still maintain high ethylene polymerization activity at a higher temperature, and the molecular weight distribution of the obtained polymer is narrow.
[0031] Compared with the prior art, the present invention has the following advantages:
[0032] 1. The synthesis method of the tetrahydronaphthol-phosphine late transition metal complex of the present invention is simple, has high yield and low cost;
[0033] 2. The tetralinol-phosphine post-transition metal complex of the present invention can catalyze ethylene polymerization with high activity, especially can maintain high polymerization activity at a relatively high polymerization temperature, and can obtain linear polyethylene with adjustable relative molecular mass;
[0034] 3. The tetralinol-phosphine late transition metal complex of the present invention has a high copolymerization performance with acrylic ester monomers. DETAILED DESCRIPTION
[0035] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0036] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be deemed to be specifically disclosed herein.
[0037] The present invention provides a tetralinol-phosphine late transition metal complex, the structural formula of which is shown in formula (I):
[0038]
[0039] M is selected from Group VIII metals, R7-R 11 Each is independently selected from hydrogen, halogen, hydroxyl and substituted or unsubstituted C1-C15 hydrocarbon group, R2 and R3 are independently selected from halogen, C1-C10 hydrocarbon group, P(R4)3, NR5R6 or OR 12 R 13 , or R2 and R3 are connected to each other to form an eight-membered ring or an eight-membered ring system;
[0040] Wherein R4 is selected from substituted or unsubstituted C1-C10 alkyl and substituted or unsubstituted C6-C10 aryl;
[0041] R5 and R6 are each independently selected from a C1-C10 hydrocarbon group, or R5, R6 and N are connected to each other to form a five-membered ring or a six-membered ring;
[0042] R 12 and R 13 Each independently selected from C1-C10 hydrocarbon group, or R 12 , R 13 Connected with O to form a five-membered ring or a six-membered ring.
[0043] In a more preferred embodiment, R7-R 11 Each is independently selected from hydrogen, halogen, hydroxyl, substituted or unsubstituted C1-C15 alkyl and substituted or unsubstituted C6-C15 aryl, and the substituent is selected from halogen, hydroxyl, C1-C10 alkyl, halogenated C1-C10 alkyl, C1-C10 alkoxy or halogenated C1-C10 alkoxy.
[0044] In a preferred embodiment, M is selected from nickel or palladium.
[0045] Preferably, at least one of R2 and R3 is selected from halogen or C1-C10 hydrocarbon group, or R2 and R3 are connected to each other to form an eight-membered ring or an eight-membered ring system.
[0046] In a preferred embodiment, R2 and R3 are each independently selected from halogen or C1-C10 hydrocarbon group (such as C1-C10 alkyl or C6-C10 aryl).
[0047] In a more preferred embodiment, R2 is selected from halogen or C1-C8 hydrocarbon group (such as C1-C8 alkyl or C6-C8 aryl), and R3 is selected from P(R4)3, NR5R6 or OR 12 R 13 , wherein R4 is selected from substituted or unsubstituted C1-C10 alkyl and substituted or unsubstituted C6-C10 aryl; R5 and R6 are each independently selected from C1-C6 hydrocarbon groups, and R5, R6 and N are interconnected to form a five-membered ring or a six-membered ring; R 12 and R 13 are each independently selected from C1-C10 hydrocarbon groups, and R 12 , R 13 Connected with O to form a five-membered ring or a six-membered ring.
[0048] According to some embodiments of the present invention, R2 and R3 are connected to each other to form an eight-membered ring.
[0049] In a preferred embodiment, when R2 and R3 are each independently selected from P(R4)3, P(R4)3 may be PMe3, PPh3 or PEt3; when R2 and R3 are each independently selected from NR5R6, NR5R6 may be pyridine (C5H5N), 2-methylpyridine, 3-methylpyridine or 4-methylpyridine; when R2 and R3 are each independently selected from OR 12 R 13 When, OR 12 R 13 It may be tetrahydrofuran (C4H8O), 2-methyltetrahydrofuran, 3-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran or 2,2-dimethyltetrahydrofuran.
[0050] As used herein, "Me" refers to methyl, "Ph" refers to phenyl, and "Et" refers to ethyl.
[0051] In the present invention, the "substituted" in "substituted or unsubstituted" refers to containing substituents, and the substituents here can be selected from halogen, hydroxyl, C1-C6 alkyl, halogenated C1-C6 alkyl, C1-C6 alkoxy or halogenated C1-C6 alkoxy.
[0052] In a preferred embodiment, the C1-C6 alkyl group is selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, n-pentyl, isopentyl, n-hexyl, isohexyl or 3,3-dimethylbutyl.
[0053] In a preferred embodiment, the C1-C6 alkoxy group is selected from methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, n-pentoxy, isopentoxy, n-hexoxy, isohexoxy or 3,3-dimethylbutoxy.
[0054] In the present invention, the halogen is selected from fluorine, chlorine, bromine or iodine.
[0055] In a further preferred embodiment, the tetralinol-phosphine late transition metal complex is selected from the group consisting of the following complexes:
[0056] Complex 1: Complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is methyl, and R3 is -NC5H5;
[0057] Complex 2: Complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is phenyl, and R3 is PMe3;
[0058] Complex 3: A complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 and R3 are connected to each other to form cyclooctene;
[0059] Complex 4: A complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is Cl, and R3 is -OC4H8;
[0060] Complex 5: A complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is Br, and R3 is -OC4H8;
[0061] Complex 6: A complex represented by formula (I), wherein M is Ni, R7, R9 and R 10 is H, R8 is methyl, R 11 isopropyl, R2 and R3 are connected to each other to form cyclooctene;
[0062] Complex 7: A complex represented by formula (I), wherein M is Ni, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is methyl, and R3 is -NC5H5;
[0063] Complex 8: A complex represented by formula (I), wherein M is Ni, R7, R9 and R 10is H, R8 is methyl, R 11 is isopropyl, R2 is phenyl, and R3 is PMe3;
[0064] Complex 9: A complex represented by formula (I), wherein M is Ni, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is Cl, and R3 is -OC4H8;
[0065] Complex 10: A complex represented by formula (I), wherein M is Ni, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is Br, and R3 is -OC4H8;
[0066] Complex 11: A complex represented by formula (I), wherein M is Pd, R7-R 11 is H, R2 is methyl, and R3 is -NC5H5;
[0067] Complex 12: A complex represented by formula (I), wherein M is Pd, R7-R 11 is H, R2 is Cl, and R3 is PMe3;
[0068] Complex 13: A complex represented by formula (I), wherein M is Pd, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is methyl, and R3 is -NC5H5;
[0069] Complex 14: A complex represented by formula (I), wherein M is Pd, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is Cl, and R3 is PMe3.
[0070] The second aspect of the present invention provides a method for preparing the above-mentioned tetrahydronaphthol-phosphine late transition metal complex, which comprises the following steps:
[0071] (1) reacting the compound represented by formula (II) with the compound represented by formula (III) to obtain a ligand, wherein the ligand is represented by formula (IV);
[0072] (2) reacting the ligand with an M metal compound;
[0073]
[0074] Wherein the metal M is selected from Group VIII metals, preferably nickel or palladium; R7-R 11 The definition of is the same as described above.
[0075] In the method described in the present invention, the M metal compound can be selected from nickel dimethyldipyridine (Py2NiMe2), bis(1,5-cyclooctadiene) nickel (Ni(COD)2), nickel dichlorotetrapyridine (Ni2Cl2Py4), ethylene glycol dimethyl ether nickel bromide ((DME)NiBr2), ethylene glycol dimethyl ether nickel chloride ((DME)NiCl2), dichlorobis(trimethylphosphine) nickel (NiCl2(PMe3)2), di(pyridine)bis[(trimethylsilyl)methyl]nickel (Ni(Py)2(CH2SiMe3)2), bromo(phenyl)(N,N,N',N'-tetramethyl-1,2-ethylenediamine)nickel (NiArBr(TMEDA)), dibenzyldipyridine nickel (Ni(CH2Ph)2Py2), phenyl(trimethylphosphine)nickel bromide (N iPhBr(PMe3)2, phenyl(triethylphosphine)nickel chloride (NiPhCl(PEt3)2), diphenylbis(trimethylphosphine)nickel (NiPh2(PMe3)2), dichlorobis(trimethylphosphine)nickel (NiCl2(PMe3)2), dimethyldipyridine palladium (Pd(Me)2Py2), dichlorodipyridine palladium (PdCl2Py2), di(pyridine)bis[(trimethylsilyl)methyl]palladium (Pd(Py)2(CH2SiMe3)2), dibenzyldipyridine palladium (Pd(CH2Ph)2Py2), methyl-1,5-cyclooctadiene-palladium chloride (Pd(COD)ClMe) and dimethyl(N,N,N',N'-tetramethyl-1,2-ethylenediamine)palladium ((TMEDA)PdMe2) One or more thereof.
[0076] In the method of the present invention, the reaction process of step (1) is shown in the following reaction formula.
[0077]
[0078] Among them, R7-R 11 The definition of is the same as described above.
[0079] In the method described in the present invention, the reaction process of step (2) is shown in the following reaction formula.
[0080]
[0081] Among them, M, R2, R3, R7-R 11 The definition of is the same as described above.
[0082] In a preferred embodiment, the reaction of step (1) is carried out in the presence of a solvent; in a specific embodiment, the solvent may be diethyl ether.
[0083] In a preferred embodiment, the reaction of step (2) is carried out in the presence of a reaction solvent; in a specific embodiment, the reaction solvent may be toluene or tetrahydrofuran.
[0084] In a preferred embodiment, in step (2), the molar ratio of the M metal compound to the ligand is 1.1-1.3:1.
[0085] In a specific embodiment, the preparation process of step (1) comprises: dissolving the compound represented by formula (II) in anhydrous ether in an atmosphere of protective gas (such as nitrogen), dropping n-BuLi (n-butyl lithium) solution at -78°C, and gradually returning to room temperature after the reaction; then dropping anhydrous ether solution of the compound represented by formula (III) (ice-water bath), slowly warming to room temperature, stirring and reacting overnight. Quenching with water, extracting the organic phase with anhydrous ether, concentrating the obtained organic phase, deoxygenating by freezing cycle, adding 15mL of concentrated hydrochloric acid to react under a nitrogen atmosphere, tracking the completion of the reaction by TLC, and then adding NaHCO3 aqueous solution for neutralization, quenching with water, extracting the organic phase with anhydrous ether, drying with anhydrous MgSO4, filtering, concentrating, and column chromatography to obtain the ligand represented by formula (IV).
[0086] In a specific embodiment, the preparation process of step (2) comprises: in an atmosphere of protective gas (such as nitrogen), dissolving the ligand obtained in step (1) and the M metal compound in a reaction solvent (such as toluene, tetrahydrofuran, etc.), respectively, and then stirring and mixing the ligand solution and the M metal compound solution to react at room temperature for 8 to 10 hours, filtering, concentrating the filtrate, adding heptane for recrystallization, and obtaining the tetrahydronaphthol-phosphine post-transition metal complex of the present invention.
[0087] The third aspect of the present invention provides the use of the above-mentioned tetrahydronaphthol-phosphine late transition metal complex in olefin polymerization. Preferably, the olefin includes ethylene and an α-olefin containing a polar group.
[0088] The tetralin-phosphine late transition metal complex of the present invention can be used as a catalyst for homopolymerization or copolymerization of olefins, and is particularly suitable for homopolymerization of ethylene or copolymerization of ethylene with other alpha-olefins and olefins with polar functional groups such as hydroxyl, carboxyl, ester, etc., wherein the alpha-olefin is independently selected from one or more of propylene, butene, pentene, hexene, octene and 4-methylpentene-1; the olefin with polar functional groups is a vinyl monomer containing one or more hydroxyl, carboxyl, ester groups, and the same molecule of the vinyl monomer can contain multiple different polar groups.
[0089] In the present invention, another embodiment of the preparation method of α-olefin polymer is that (a) α-olefin and (b) (meth) acrylate monomer, vinyl monomer or allyl monomer are copolymerized in the presence of the above-mentioned tetralin-phosphine post-transition metal complex. The (meth) acrylate monomer in the present invention is of the general formula CH2=C(R 31 )CO2(R 32 ) indicates that, where R 31 It can be H or a C1-C10 hydrocarbon group, which may have a branch, a ring and / or an unsaturated bond; R 32 It may be a C1-C30 hydrocarbon group, which may have a branch, a ring and / or an unsaturated bond, and R 32 A heteroatom may be contained at any position.
[0090] When R 31 When the number of carbon atoms is 11 or more, it tends to show less polymerization activity. 31 is H or a C1-C10 hydrocarbon group. 31 is H or a C1-C5 hydrocarbon group. More preferably, R 31 It is H or methyl.
[0091] Similarly, when R 32 When the number of carbon atoms of R is greater than 30, it tends to show less polymerization activity. 32 The number of carbon atoms is 1-30, preferably 1-12, and more preferably 1-8.
[0092] In addition, as R 32 The heteroatoms optionally contained in R can be selected from oxygen, sulfur, selenium, phosphorus, nitrogen, silicon, fluorine, boron, etc. Among these heteroatoms, oxygen, silicon and fluorine are preferred, and oxygen is more preferred. 32 It is also preferred.
[0093] Further preferably, specific examples of the (meth)acrylate monomer include, but are not limited to: methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, phenyl (meth)acrylate, toluyl (meth)acrylate, The (meth)acrylate monomers may be used alone or in combination of two or more.
[0094] In a preferred embodiment, the olefin is a C2-C16 olefin; more preferably, the olefin is ethylene or an α-olefin or cycloolefin having 3 to 16 carbon atoms.
[0095] The fourth aspect of the present invention provides an olefin polymerization method, comprising carrying out an olefin polymerization reaction in the presence of the above-mentioned tetralinol-phosphine post-transition metal complex, wherein the olefin polymerization reaction can be homopolymerization or copolymerization.
[0096] In a preferred embodiment, the polymerization reaction temperature is -78°C to 200°C, more preferably -20°C to 150°C; the polymerization pressure is 0.01 to 10 MPa, more preferably 0.01 to 5 MPa.
[0097] As used herein, "polymerization pressure" refers to the ethylene pressure in the polymerization system and is expressed as an absolute pressure.
[0098] According to some embodiments of the present invention, the olefin comprises a C2-C16 olefin.
[0099] According to some embodiments of the present invention, the olefin comprises a C2-C16 α-olefin or a cyclic olefin.
[0100] According to some embodiments of the invention, the olefin comprises ethylene.
[0101] According to some embodiments of the present invention, the olefin includes ethylene and an α-olefin or a cyclic olefin containing a polar group.
[0102] According to some embodiments of the present invention, the polymerization reaction temperature may be -20°C, 50°C, 100°C or 150°C.
[0103] According to some embodiments of the present invention, the polymerization pressure may be 0.01 MPa, 0.1 MPa, 0.2 MPa, 0.5 MPa, 1 MPa or 2 MPa.
[0104] According to some embodiments of the present invention, the polymerization is carried out by olefin monomers in a solvent, and the polymerization solvent is independently selected from one or more of alkanes, aromatic hydrocarbons and halogenated hydrocarbons.
[0105] According to some specific embodiments of the present invention, the polymerization solvent is independently selected from one or more of hexane, pentane, heptane, benzene, toluene, dichloromethane, chloroform and dichloroethane, more preferably one or more of hexane, toluene and heptane.
[0106] In the present invention, alkyl refers to a straight chain alkyl, a branched alkyl or a cycloalkyl, including but not limited to: methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, tert-pentyl, neopentyl, n-hexyl, n-heptyl, n-octyl, n-decyl, cyclopropyl, cyclopentyl, cyclohexyl, 4-methylcyclohexyl, 4-ethylcyclohexyl, 4-n-propylcyclohexyl and 4-n-butylcyclohexyl.
[0107] In the present invention, examples of the aryl group include, but are not limited to, phenyl, 4-methylphenyl, 4-ethylphenyl, dimethylphenyl and vinylphenyl.
[0108] In the present invention, alkenyl refers to straight-chain alkenyl, branched-chain alkenyl or cycloalkenyl, including but not limited to vinyl, allyl and butenyl.
[0109] In the present invention, examples of the aralkyl group include, but are not limited to, phenylmethyl, phenylethyl, phenyl-n-propyl, phenyl-isopropyl, phenyl-n-butyl and phenyl-t-butyl.
[0110] In the present invention, examples of the alkylaryl group include, but are not limited to, tolyl, ethylphenyl, n-propylphenyl, isopropylphenyl, n-butylphenyl and tert-butylphenyl.
[0111] The following examples are used to further illustrate the phosphine-phenol post-transition metal complex and its preparation method and application described in the present invention. The examples are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the following examples.
[0112] The experimental methods in the following examples, unless otherwise specified, are all conventional methods in the art; the experimental materials used in the following examples, unless otherwise specified, are all commercially available.
[0113] The analytical characterization instruments and test methods used in the following examples and comparative examples are as follows:
[0114] (1) Nuclear magnetic resonance instrument: Bruker DMX 300 (300 MHz), with tetramethylsilane (TMS) as internal standard;
[0115] (2) Molecular weight and molecular weight distribution PDI of polymer (PDI = Mw / Mn): measured at 150°C using PL-GPC220 chromatograph with trichlorobenzene as solvent (standard sample: PS, flow rate: 1.0 mL / min, chromatographic column: 3×PLgel 10um M1×ED-B, 300×7.5 nm);
[0116] (3) Activity measurement method: The polymer was washed with hydrochloric acid ethanol solution, vacuum dried, and the weight of the polymer was measured; the polymerization activity was calculated as follows: polymer weight (g) / metal (mol) × 60 / polymerization time (min);
[0117] (4) Analysis of the comonomer content of polymers: 1 H NMR, 13 C NMR spectrum was determined on a 400 MHz Bruker Avance 400 NMR spectrometer using a 10 mm PASEX 13 probe. The polymer sample was dissolved in 1,2,4-trichlorobenzene at 120°C for analysis and testing.
[0118] Example 1
[0119] Complex 1: Complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is methyl, and R3 is -NC5H5;
[0120] In a nitrogen atmosphere, the compound represented by formula (II) (2.32 g, 10 mmol) was dissolved in anhydrous ether (20 mL), and n-butyl lithium solution (2.7 M, 4.0 mL, 11 mmol) was added dropwise at -78 °C. The reaction gradually returned to room temperature and continued to stir for 12 h to obtain a white precipitate. Dicyclohexylphosphine chloride (10 mmol, 2.32 g) was evenly dispersed in 10 mL of anhydrous ether and added dropwise to the original reaction system under an ice-water bath. The temperature was slowly raised to room temperature and stirred. Stir overnight, quench with water, extract the organic phase with anhydrous ether, concentrate the obtained organic phase, deoxygenate by freezing cycle, add 5 mL of concentrated hydrochloric acid under nitrogen atmosphere to react for 5 h, track the reaction by TLC, neutralize with NaHCO3 aqueous solution, quench with water, extract the organic phase with anhydrous ether, dry with anhydrous MgSO4, filter, concentrate, and obtain ligand L1 by column chromatography with a yield of 31%; 1HNMR (500 MHz, CDCl3, TMS): δ11.65 (s, 0.9H), 6 .72-6.68 (m, 1H), 6.58-6.56 (m, 1H), 2.74-2.72 (t, J=5.8Hz, 2H), 2.65-2.63 (t, J=6.3Hz, 2H), 2.06- 1.96 (m, 4H), 1.86-1.68 (m, 12H), 1.45-1.13 (m, 10H); 13CNMR (126MHz, CDCl3) δ163.26, 143.18, 143.1 6, 126.63, 126.58, 125.86, 125.79, 119.39, 119.30, 104.10, 103.39, 77.28, 77.03, 76.77, 36.01, 35 .49, 29.98, 26.41, 26.31, 26.27, 26.17, 25.76, 25.27, 25.25, 24.10, 24.08, 22.78, 22.59, 22.54; 31P NMR (202MHz, CDCl3) δ60.52;
[0121] In a nitrogen atmosphere, ligand L1 (0.517 g, 1.5 mmol) and metal nickel source (Py2NiMe2) (0.366 g, 1.5 mmol) were dissolved in toluene (10 mL), and then the ligand solution was dripped into the metal nickel source solution drop by drop, stirred vigorously, and reacted at room temperature for 10 h. The brown-yellow solution was filtered, the solvent was concentrated, and frozen at -30 ° C for crystallization to obtain complex 1 with a yield of 72%, 31P NMR (202 MHz, CDCl3) δ 60.61, and elemental analysis test C 28 H 40 NNiOP: Theoretical calculation values are: C, 67.76; H, 8.12; N, 2.82; Test values are: C, 67.45; H, 8.42; N, 2.67;
[0122] A 1L stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 500mL of toluene was injected into the polymerization kettle, 5.0mg (10μmol) of complex 1 was added, and the ethylene pressure was maintained at 10atm at 50°C with vigorous stirring for 30min. The reaction was neutralized with an ethanol solution acidified with 10wt% hydrochloric acid to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.
[0123] Example 2
[0124] Complex 1: Complex represented by formula (II), wherein M is Ni, R7-R 11 is H, R2 is methyl, and R3 is -NC5H5;
[0125] A 1L stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 500mL of hexane was injected into the polymerization kettle, 5.0mg (10μmol) of complex 1 was added, and the ethylene pressure was maintained at 10atm at 70°C with vigorous stirring for 30min. The reaction was neutralized with an ethanol solution acidified with 10wt% hydrochloric acid to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.
[0126] Example 3
[0127] Complex 1: Complex represented by formula (II), wherein M is Ni, R7-R 11 is H, R2 is methyl, and R3 is -NC5H5;
[0128] A 1L stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 500mL of hexane was injected into the polymerization kettle, 5.0mg (10μmol) of complex 1 was added, and the reaction was vigorously stirred for 30min at 100°C while maintaining an ethylene pressure of 10atm. The reaction was neutralized with an ethanol solution acidified with 10wt% hydrochloric acid to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.
[0129] Example 4
[0130] Complex 1: Complex represented by formula (II), wherein M is Ni, R7-R 11 is H, R2 is methyl, and R3 is -NC5H5;
[0131] A 100mL stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 50mL of toluene and 0.45mL (5mmol) of methyl acrylate were injected into the polymerization kettle, 5.0mg (10μmol) of complex 1 were added, and the reaction was carried out at 70°C with an ethylene pressure of 15atm for 60min with vigorous stirring. The reaction was neutralized with an ethanol solution acidified with 10wt% hydrochloric acid to obtain an ethylene-acrylate copolymer. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.
[0132] Example 5
[0133] Complex 1: Complex represented by formula (II), wherein M is Ni, R7-R 11 is H, R2 is methyl, and R3 is -NC5H5;
[0134] A 100mL stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 50mL of toluene and 0.72mL (5mmol) of butyl acrylate were injected into the polymerization kettle, 5.0mg (10μmol) of complex 1 were added, and the reaction was carried out at 70°C with an ethylene pressure of 15atm for 60min with vigorous stirring. The reaction was neutralized with an ethanol solution acidified with 10wt% hydrochloric acid to obtain an ethylene-acrylate copolymer. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.
[0135] Example 6
[0136] Complex 2: Complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is phenyl, and R3 is PMe3;
[0137] Ligand L1 was prepared according to the method of Example 1;
[0138] In a nitrogen atmosphere, ligand L1 (0.688 g, 2 mmol) and PMe3 (1 mol / L, 2 mL) were dissolved in 20 mL toluene, and a 30 mL toluene solution of a metal nickel source (Ni(COD)2) (0.550 g, 2 mmol) was added dropwise at 0°C. The reaction was carried out at room temperature for 16 h, and then heated at 50°C for 2 h. The solvent was evaporated, 5 mL toluene was added, filtered, 100 mL heptane was added, and the complex 2 was obtained by freezing and recrystallization. The yield was 66%, and the elemental analysis test was C 31 H 46 NiOP2: Theoretical calculation value: C, 67.05; H, 8.35; Test value: C, 67.31; H, 8.42;
[0139] A 1L stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 500mL of toluene was injected into the polymerization kettle, 5.55mg (10μmol) of complex 2 was added, and the reaction was carried out at 50°C with ethylene pressure maintained at 10atm with vigorous stirring for 30min. The obtained product was a C4-C24 copolymer.
[0140] Example 7
[0141] Complex 10: A complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is Br, and R3 is -OC4H8;
[0142] Ligand L1 was prepared according to the method of Example 1;
[0143] In a nitrogen atmosphere, ligand L1 (0.688 g, 2 mmol) was dissolved in tetrahydrofuran, excess NaH (0.072 g, 3 mmol) was added, and the mixture was stirred at room temperature for 10 h. NaH was filtered out, and a solution of metal nickel source (DME) NiBr2 (0.617 g, 2 mmol) in tetrahydrofuran was added dropwise. The mixture was reacted at room temperature overnight, the solvent was drained, and dichloromethane (40 mL) was added to dissolve the mixture. The filter cake was removed by filtration, the filtrate was concentrated, and heptane was added for recrystallization to obtain complex 10 with a yield of 72%. The elemental analysis test showed that the complex 10 had a yield of 72%. 26 H 40 BrNiO2P: Theoretical calculated values are: C, 56.35; H, 7.28; Test values are: C, 56.74; H, 7.41;
[0144] A 1L stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 500mL of toluene was injected into the polymerization kettle, 5.54mg (10μmol) of complex 10 was added, and the ethylene pressure was maintained at 10atm at 30°C with vigorous stirring for 30min. The reaction was neutralized with 10wt% hydrochloric acid-acidified ethanol solution to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight-average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.
[0145] Example 8
[0146] Complex 10: A complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is Br, and R3 is -OC4H8;
[0147] A 1L stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 500mL of hexane was injected into the polymerization kettle, 5.54mg (10μmol) of complex 10 was added, and the reaction was vigorously stirred for 30min at 80°C while maintaining an ethylene pressure of 10atm. The reaction was neutralized with an ethanol solution acidified with 10wt% hydrochloric acid to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.
[0148] Example 9
[0149] Complex 10: A complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is Br, and R3 is -OC4H8;
[0150] A 100 mL stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130° C. for 6 h, evacuated while hot and replaced with N2 gas three times, 50 mL of toluene and 0.45 mL (5 mmol) of methyl acrylate were injected into the polymerization kettle, 5.54 mg (10 μmol) of complex 10 were added, and the reaction was carried out at 70° C. while maintaining an ethylene pressure of 15 atm with vigorous stirring for 60 min. The reaction was neutralized with an ethanol solution acidified with 10 wt% hydrochloric acid to obtain an ethylene-acrylate copolymer. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.
[0151] Example 10
[0152] Complex 11: A complex represented by formula (I), wherein M is Pd, R7-R 11 is H, R2 is methyl, and R3 is -NC5H5;
[0153] Ligand L1 was prepared according to the method of Example 1;
[0154] In a nitrogen atmosphere, ligand L1 (0.688 g, 2 mmol) was dissolved in toluene (20 mL), and metal palladium source (TMEDA) PdMe2 (0.51 g, 2 mmol) was dissolved in toluene (15 mL) solution. Then, the ligand solution was dripped into the metal palladium source solution dropwise, stirred vigorously, and reacted at room temperature for 5 h. 0.6 mL of pyridine was added, and the reaction was allowed to proceed overnight. A black solution was filtered, and the solvent was removed in vacuo to obtain complex 11 with a yield of 77%. The elemental analysis test showed that C 28 H 40 NOPPd: Theoretical calculated values are: C, 61.82; H, 7.41; N, 2.57; Test values are: C, 62.03; H, 7.58; N, 2.36;
[0155] A 100 mL glass polymerization tube equipped with mechanical stirring was dried continuously at 130°C for 6 h, vacuumed while hot and replaced with N2 gas 3 times, 5.0 mL of toluene and 5.0 mL of norbornene were injected into the polymerization kettle, 5.4 mg (10 μmol) of complex 11 was added, 40 μmol of B(C6F5)3 was added, and the mixture was stirred vigorously at 60°C for 10 min. It was neutralized with an ethanol solution acidified with 10 wt% hydrochloric acid to obtain polynorbornene, and the polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.
[0156] Comparative Example 1
[0157] 10atm ethylene: A 1L stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 500mL of hexane was injected into the polymerization kettle, and then 5.0ml of methylaluminoxane (MAO) (1.53mol / l toluene solution) was added, and 10.1mg (20μmol) of complex A (Chem Cat Chem 2022, 14, e202101736) was added. The ethylene pressure was maintained at 10atm at 70°C and the reaction was vigorously stirred for 30min. The reaction was neutralized with 10wt% hydrochloric acid-acidified ethanol solution to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of weight average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.
[0158]
[0159] Comparative Example 2
[0160] A 100mL stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 50mL of toluene and 0.45mL (5mmol) of methyl acrylate were injected into the polymerization kettle, 10.1mg (10μmol) of complex A was added, and the reaction was carried out at 70°C with ethylene pressure maintained at 15atm for 60min with vigorous stirring. The reaction was neutralized with 10wt% hydrochloric acid-acidified ethanol solution to obtain ethylene-acrylate copolymer. The polymer was dried and weighed to test the polymerization activity. The test data of weight average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.
[0161] Comparative Example 3
[0162]
[0163] A 100 mL glass polymerization tube equipped with mechanical stirring was dried continuously at 130 ° C for 6 h, evacuated while hot and replaced with N2 gas three times, 5.0 mL of toluene and 5.0 mL of norbornene were injected into the polymerization kettle, 4.3 mg (8 μmol) of complex B (see Appl Organometal Chem. 2017; e4013) and 40 μmol B (C6F5) 3 were added, and the mixture was stirred vigorously at 60 ° C for 10 min. The mixture was neutralized with 10 wt% hydrochloric acid-acidified ethanol solution to obtain polynorbornene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution, polymerization activity and comonomer content of the obtained polymer are shown in Table 1.
[0164] Table 1
[0165]
[0166]
[0167] As can be seen from Table 1, the use of the tetralinol-phosphine late transition metal complex of the present invention as an olefin polymerization catalyst has higher homopolymerization / copolymerization activity under similar polymerization conditions, the molecular weight of the obtained polymer is significantly higher than that of the polymer obtained in the comparative example, and the molecular weight distribution of the obtained polymer is narrower.
[0168] The preferred embodiments of the present invention are described in detail above; however, the present invention is not limited thereto; within the technical concept of the present invention, the technical solution of the present invention may be subjected to a variety of simple modifications, including combining various technical features in any other suitable manner; these simple modifications and combinations shall also be regarded as the contents disclosed by the present invention and shall all belong to the protection scope of the present invention.
Claims
1. A tetralinol-phosphine late transition metal complex, characterized in that: Its structural formula is shown in formula (I), M is selected from Group VIII metals, R7-R 11 Each is independently selected from hydrogen, halogen, hydroxyl and substituted or unsubstituted C1-C15 hydrocarbon group, R2 and R3 are independently selected from halogen, C1-C10 hydrocarbon group, P(R4)3, NR5R6 or OR 12 R 13 , or R2 and R3 are connected to each other to form an eight-membered ring or an eight-membered ring system; Wherein R4 is selected from substituted or unsubstituted C1-C10 alkyl and substituted or unsubstituted C6-C10 aryl; R5 and R6 are each independently selected from a C1-C10 hydrocarbon group, or R5, R6 and N are connected to each other to form a five-membered ring or a six-membered ring; R 12 and R 13 Each independently selected from C1-C10 hydrocarbon group, or R 12 , R 13 Connected with O to form a five-membered ring or a six-membered ring.
2. The tetralin-phosphine late transition metal complex according to claim 1, characterized in that: M is selected from nickel or palladium.
3. The tetralin-phosphine late transition metal complex according to claim 1 or 2, characterized in that: R7-R 11 Each is independently selected from hydrogen, halogen, hydroxyl, substituted or unsubstituted C1-C15 alkyl and substituted or unsubstituted C6-C15 aryl, and the substituent is selected from halogen, hydroxyl, C1-C10 alkyl, halogenated C1-C10 alkyl, C1-C10 alkoxy or halogenated C1-C10 alkoxy; Preferably, R2 and R3 are each independently selected from halogen, C1-C8 hydrocarbon, P(R4)3, NR5R6 or OR 12 R 13 , or R2 and R3 are connected to form an eight-membered ring; wherein R4 is selected from substituted or unsubstituted C1-C10 alkyl and substituted or unsubstituted C6-C10 aryl; R5 and R6 are each independently selected from C1-C6 hydrocarbon group, or R5, R6 and N are connected to form a five-membered ring or a six-membered ring; R 12 and R 13 Each independently selected from C1-C6 hydrocarbon group, or R 12 , R 13 Connected with O to form a five-membered ring or a six-membered ring.
4. The tetralin-phosphine late transition metal complex according to any one of claims 1 to 3, characterized in that: The substituent is selected from halogen, hydroxy, C1-C6 alkyl, halogenated C1-C6 alkyl, C1-C6 alkoxy or halogenated C1-C6 alkoxy; Preferably, the C1-C6 alkyl group is selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, n-pentyl, isopentyl, n-hexyl, isohexyl or 3,3-dimethylbutyl; Preferably, the C1-C6 alkoxy group is selected from methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, n-pentoxy, isopentoxy, n-hexoxy, isohexoxy or 3,3-dimethylbutoxy; Preferably, the halogen is selected from fluorine, chlorine, bromine or iodine.
5. The tetralin-phosphine late transition metal complex according to any one of claims 1 to 4, characterized in that: It is selected from the group consisting of the following complexes, Complex 1: Complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is methyl, and R3 is -NC5H5; Complex 2: Complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is phenyl, and R3 is PMe3; Complex 3: A complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 and R3 are connected to each other to form cyclooctene; Complex 4: A complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is Cl, and R3 is -OC4H8; Complex 5: A complex represented by formula (I), wherein M is Ni, R7-R 11 is H, R2 is Br, and R3 is -OC4H8; Complex 6: A complex represented by formula (I), wherein M is Ni, R7, R9 and R 10 is H, R8 is methyl, R 11 isopropyl, R2 and R3 are connected to each other to form cyclooctene; Complex 7: A complex represented by formula (I), wherein M is Ni, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is methyl, and R3 is -NC5H5; Complex 8: A complex represented by formula (I), wherein M is Ni, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is phenyl, and R3 is PMe3; Complex 9: A complex represented by formula (I), wherein M is Ni, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is Cl, and R3 is -OC4H8; Complex 10: The complex represented by formula (I), wherein M is Ni, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is Br, and R3 is -OC4H8; Complex 11: A complex represented by formula (I), wherein M is Pd, R7-R 11 is H, R2 is methyl, and R3 is -NC5H5; Complex 12: A complex represented by formula (I), wherein M is Pd, R7-R 11 is H, R2 is Cl, and R3 is PMe3; Complex 13: A complex represented by formula (I), wherein M is Pd, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is methyl, and R3 is -NC5H5; Complex 14: A complex represented by formula (I), wherein M is Pd, R7, R9 and R 10 is H, R8 is methyl, R 11 is isopropyl, R2 is Cl, and R3 is PMe3.
6. A method for preparing the tetralin-phosphine late transition metal complex according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: (1) reacting the compound represented by formula (II) with the compound represented by formula (III) to obtain a ligand; (2) reacting the ligand with an M metal compound; Wherein the metal M is selected from Group VIII metals, preferably nickel or palladium; R7-R 11 The definition is the same as that of claim 1.
7. The method according to claim 6, characterized in that The M metal compound is selected from one or more of dimethyldipyridinium nickel, bis(1,5-cyclooctadiene)nickel, dichlorotetrapyridinium nickel, ethylene glycol dimethyl ether nickel bromide, ethylene glycol dimethyl ether nickel chloride, dichlorobis(trimethylphosphine)nickel, bis(pyridine)bis[(trimethylsilyl)methyl]nickel, bromo(phenyl)(N,N,N',N'-tetramethyl-1,2-ethylenediamine)nickel, dibenzyldipyridinium nickel, phenyl(trimethylphosphine)nickel bromide, phenyl(triethylphosphine)nickel chloride, diphenylbis(trimethylphosphine)nickel, dichlorobis(trimethylphosphine)nickel, dimethyldipyridinium palladium, dichlorodipyridinium palladium, bis(pyridine)bis[(trimethylsilyl)methyl]palladium, dibenzyldipyridinium palladium, methyl-1,5-cyclooctadiene-palladium chloride and dimethyl(N,N,N',N'-tetramethyl-1,2-ethylenediamine)palladium.
8. The method according to claim 6 or 7, characterized in that: The reaction of step (2) is carried out in the presence of a reaction solvent, which is toluene or tetrahydrofuran.
9. Use of the tetralinol-phosphine late transition metal complex according to any one of claims 1 to 5 in olefin polymerization.
10. An olefin polymerization method, characterized in that: The method comprises carrying out an olefin polymerization reaction in the presence of the tetrahydronaphthol-phosphine late transition metal complex as described in any one of claims 1 to 5; Preferably, the polymerization reaction temperature is -78°C to 200°C, more preferably -20°C to 150°C; The polymerization pressure is 0.01 to 10 MPa, more preferably 0.01 to 5 MPa.
Citation Information
Cited By
5,6,7,8-tetrahydro-1-naphthol-phosphine post-transition metal complexes, preparation method therefor, and use thereof
EP4671259A1