Modified pectin material as well as preparation method and application thereof
By adding ascorbic acid and tannin to the low methoxy pectin solution for graft copolymerization, the modified pectin material LMP-TA was obtained, which solved the problem of insufficient adhesion of pectin material and achieved continuous surface of fruits and vegetables Film formation and good fresh-preservation effects extend the shelf life of fruits and vegetables and improve quality.
Patent Information
- Application Number
- CN202411281397.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, the adhesion of pectin materials on the surface of fruits and vegetables is weak and cannot form a film continuously, affecting the antibacterial preservation effect.
By adding ascorbic acid and tannin to the low methoxy pectin solution, the modified pectin material LMP-TA is obtained through graft copolymerization, which improves its adhesion and mechanical properties, so that it can continuously form films and reduces Water vapor permeability.
It significantly extends the shelf life of fruits and vegetables, improves the quality and freshness of fruits and vegetables, and enhances the antioxidant and antibacterial properties of the materials.
Smart Images

Figure CN118994435A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fruit and vegetable preservation, and in particular to a modified pectin material and a preparation method and application thereof. Background Art
[0002] The high moisture content and high nutritional value of fruits and vegetables make them an ideal platform for microbial reproduction and survival. According to statistics, about 20%-30% of fruits and vegetables are wasted due to corruption caused by microbial reproduction. Therefore, extending the shelf life of fruits and vegetables is of great significance to reducing food waste. Bananas, as a tropical fruit with huge consumption, are rich in a variety of vitamins, minerals, phenols and other nutrients needed by the human body. However, bananas have a high respiration rate at room temperature and mature quickly. After ripening, they are prone to browning, microbial infection and oxidative damage, which shortens their shelf life. Therefore, by extending the shelf life of bananas, food waste can be effectively reduced.
[0003] Fruit wax is a lipid secreted by fruits and vegetables and attached to the epidermis. Its function is to prevent pathogens (toxic and harmful substances, bacteria, viruses, etc.) from entering the fruit and resist damage caused by environmental changes. Most fruits and vegetables have a layer of fruit wax on their surface, which makes the surface hydrophobic. At present, polysaccharide polymer materials are mostly used to coat the surface of fruits and vegetables. Although polysaccharide polymer materials have strong hydrophilicity, they have weak adhesion on the surface of fruits and vegetables and cannot form a continuous film, thus affecting the antibacterial and fresh-keeping effect of the coating.
[0004] In the prior art, CN114716579A discloses a pectin graft copolymer and its preparation method and application. By grafting coumaric acid and pectin, the ·OH generated by free radicals during the reaction process captures hydrogen atoms in the pectin, weakening the hydrogen bond force, reducing hydrophobicity, and increasing solubility. The above patent uses coumaric acid in phenolic acid and pectin for graft copolymerization. Although it can improve the solubility and antioxidant properties of the copolymer, the graft copolymerization of coumaric acid cannot improve the adhesion of the copolymer. CN111763394A discloses an antibacterial film and its preparation method and application. The antibacterial film is prepared from pectin, tannic acid, polyvinyl alcohol, etc., and has excellent antibacterial properties, good mechanical properties and water solubility. There is an interaction between tannic acid and pectin and polyvinyl alcohol. This interaction can effectively fix tannic acid in the antibacterial film, thereby ensuring that the film has stable and lasting antibacterial properties. Although the antibacterial film produced by this invention can be used for food preservation, it still cannot solve the problem that the antibacterial film has weak adhesion on the surface of fruits and vegetables and cannot form a continuous film.
[0005] Therefore, there is an urgent need to modify pectin, a polysaccharide polymer, to obtain modified pectin materials, so as to improve its adhesion performance on the hydrophobic surface of fruits and vegetables, thereby improving the preservation effect. Summary of the invention
[0006] In view of the above-mentioned prior art, the purpose of the present invention is to provide a modified pectin material and its preparation method and application. By adding ascorbic acid and tannic acid to a low methoxyl pectin solution and mixing, and then adding a hydrogen peroxide solution, a modified pectin material LMP-TA is obtained through a graft copolymerization reaction. The present invention uses tannic acid to modify pectin to obtain an edible modified pectin material. The modified pectin material can improve the wettability of hydrophobic fruits and vegetables and achieve a good coating effect. At the same time, the modified pectin material also has good mechanical properties. When it is used as a coating material for fruit and vegetable preservation, it can continuously form a film on the surface of fruits and vegetables, reduce water vapor permeability, thereby extending the shelf life of fruits and vegetables and improving the quality of fruits and vegetables.
[0007] To achieve the above object, the present invention adopts the following technical solution:
[0008] The first aspect of the present invention provides a method for preparing a modified pectin material, comprising the following steps:
[0009] (1) dissolving low methoxy pectin in water to obtain a low methoxy pectin solution; adding ascorbic acid and tannic acid to the low methoxy pectin solution, stirring, to obtain a mixed solution; then adding a hydrogen peroxide solution to the mixed solution, reacting, to obtain a reaction product;
[0010] (2) The reaction product is dialyzed and then dried to obtain a modified pectin material.
[0011] Preferably, in step (1), in the low methoxy pectin solution, the solid-liquid ratio of low methoxy pectin to water is (0.3-0.6) g:50 mL.
[0012] Preferably, in step (1), the mass ratio of low methoxy pectin to ascorbic acid is (0.3-0.6):0.1.
[0013] Preferably, in step (1), the mass ratio of low methoxy pectin to tannic acid is 2:(1-4).
[0014] Preferably, in step (1), the stirring time is 5-15 min.
[0015] Preferably, in step (1), the concentration of the hydrogen peroxide solution is 2 mol / L.
[0016] Preferably, in step (1), the solid-liquid ratio of low-methoxy pectin to hydrogen peroxide solution is (0.3-0.6) g: 2 mL.
[0017] Preferably, in step (1), the reaction is carried out under a protective atmosphere, and the protective atmosphere is nitrogen.
[0018] Preferably, in step (1), the reaction time is 20-30 hours.
[0019] Preferably, in step (2), the dialysis operation is: placing the reaction product in deionized water for 70-75 hours.
[0020] The second aspect of the present invention provides a modified pectin material prepared by the above preparation method.
[0021] The third aspect of the present invention provides an application of a modified pectin material in preserving fruits and vegetables.
[0022] Beneficial effects of the present invention:
[0023] The present invention adds ascorbic acid and tannic acid to a low methoxyl pectin solution, mixes the mixture, then adds a hydrogen peroxide solution, and undergoes a graft copolymerization reaction to obtain a modified pectin material LMP-TA. The present invention grafts tannic acid onto pectin, utilizes the phenolic hydroxyl group in the tannic acid, improves the tensile properties of the modified pectin material, and interacts between the modified pectins, which can promote the interweaving of molecules, improve the flexibility of the modified pectin material, and reduce the water vapor penetration pressure. At the same time, due to the effect of the catechol group, the adhesion of the modified pectin material can be improved, and its adhesion performance can be increased, so that it can continuously form a film when used for fruit and vegetable preservation, thereby improving the preservation effect. The edible modified pectin material prepared by the present invention is used for fruit and vegetable preservation, which can significantly extend the shelf life of fruits and vegetables and ensure the quality of fruits and vegetables. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 : (A) FTIR image of the modified pectin material obtained in Example 3; (B) full wavelength UV image of the modified pectin material obtained in Example 3;
[0025] Figure 2 :(A) UV transmittance graph of each group of films in Test Example 2;(B) Tensile and elongation at break graph of each group of films in Test Example 2;(C) Water vapor permeability graph of each group of films in Test Example 2;
[0026] Figure 3 :(A) Adhesion strength and tensile strength diagram of each group of films in Test Example 2;(B) Dissolution time diagram of each group of films in Test Example 2;(C) Slip trace diagram of each group of films in Test Example 1;
[0027] Figure 4 :(A) Changes of bananas in each treatment group in Experimental Example 3; (B) L of bananas in each treatment group in Experimental Example 3 * Value graph;
[0028] Figure 5 : The weight loss rate change diagram of bananas in each treatment group in Experimental Example 3;
[0029] Figure 6 : The hardness change diagram of each group of bananas in Test Example 3. DETAILED DESCRIPTION
[0030] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0031] The surface of fruits and vegetables often has a layer of wax to prevent the loss of water and nutrients in fruits and vegetables. It is precisely because of the presence of this layer of wax that the peels of fruits and vegetables are mostly hydrophobic. The hydrophilic coating material has poor adhesion to the waxy hydrophobic surface of fruits and vegetables and cannot form a continuous film, which in turn affects the antibacterial and fresh-keeping effect of the coating. Pectin is a linear polysaccharide with biodegradability and biocompatibility. The coating composed only of pectin has high hydrophilicity and low adhesion, which is difficult to meet the needs of fruit preservation.
[0032] Based on this, the present invention is inspired by the mussel adhesion strategy and introduces tannic acid into pectin materials to increase the bonding strength between the coating material and the surface of various fruits. Specifically, the present invention adds ascorbic acid and tannic acid to a low methoxyl pectin solution, mixes them, then adds a hydrogen peroxide solution, and undergoes a graft copolymerization reaction to obtain a modified pectin material LMP-TA.
[0033] Among them, tannic acid is grafted onto pectin. Since the aromatic rings and conjugated double bonds in the grafted pectin material absorb strong electromagnetic radiation in the ultraviolet range, this absorption helps to reduce potential food damage by delaying the formation of free radicals, thereby improving the ultraviolet barrier performance of the material. The addition of phenolic hydroxyl groups strengthens the interaction between molecules, thereby improving the tensile strength. At the same time, in the modified pectin material, the interaction between pectins promotes the interweaving of molecules, thereby improving the flexibility and water vapor permeability of the material. Most importantly, the introduction of catechol groups allows the catechol groups to combine with the groups on the surface of PTFE (-NH2 and -COOH), thereby generating interfacial adhesion. In addition, the introduction of tannic acid can also improve the antioxidant and antibacterial properties of the material.
[0034] Therefore, the modified pectin material prepared by the present invention can improve the wettability of hydrophobic fruits and vegetables, achieve a good coating effect, thereby extending the shelf life of fruits and vegetables and ensuring the quality of fruits and vegetables. The method of grafting polyphenol antibacterial molecules onto the matrix of the fresh-keeping material through chemical bonds of the present invention can not only exert the antioxidant and antibacterial activities of polyphenols, but also exert the strong biological adhesion properties of catechol groups, better exert its application in the field of fruit and vegetable preservation, and has a wide range of application potentials.
[0035] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.
[0036] The experimental materials used in the embodiments of the present invention are all conventional experimental materials in the art and can be purchased through commercial channels.
[0037] Low methoxyl pectin (LMP) was provided by Andre (Shandong, Dezhou), and tannic acid (TA) (purity ≥ 72%) was purchased from MacLean Biochemical Technology Co., Ltd. (Shanghai, China).
[0038] Example 1: Preparation of modified pectin material
[0039] 0.5 g of low methoxy pectin LMP was dissolved in 50 mL of water, and the mixture was stirred for 30 min to be evenly mixed to obtain a low methoxy pectin solution. 0.1 g of ascorbic acid and 1.0 g of tannic acid TA were added to the low methoxy pectin solution, and the mixture was stirred for 10 min to obtain a mixed solution. 2 mL of 2 mol / L hydrogen peroxide solution was added to the mixed solution, and the mixture was reacted for 24 h under a nitrogen atmosphere to obtain a reaction product. The reaction product was dialyzed in deionized water for 72 h and then freeze-dried to obtain a modified pectin material LMP-TA1.
[0040] Example 2: Preparation method of modified pectin material
[0041] 0.5 g of low methoxy pectin LMP was dissolved in 50 mL of water, and the mixture was stirred for 30 min to be evenly mixed to obtain a low methoxy pectin solution. 0.1 g of ascorbic acid and 0.67 g of tannic acid TA were added to the low methoxy pectin solution, and the mixture was stirred for 10 min to obtain a mixed solution. 2 mL of 2 mol / L hydrogen peroxide solution was added to the mixed solution, and the mixture was reacted for 24 h under a nitrogen atmosphere to obtain a reaction product. The reaction product was dialyzed in deionized water for 72 h and then freeze-dried to obtain the modified pectin material LMP-TA2.
[0042] Example 3: Preparation method of modified pectin material
[0043] 0.5 g of low methoxy pectin LMP was dissolved in 50 mL of water, and the mixture was stirred for 30 min to be evenly mixed to obtain a low methoxy pectin solution. 0.1 g of ascorbic acid and 0.5 g of tannic acid TA were added to the low methoxy pectin solution, and the mixture was stirred for 10 min to obtain a mixed solution. 2 mL of 2 mol / L hydrogen peroxide solution was added to the mixed solution, and the mixture was reacted for 24 h under a nitrogen atmosphere to obtain a reaction product. The reaction product was placed in deionized water for dialyzation for 72 h and then freeze-dried to obtain the modified pectin material LMP-TA3.
[0044] Example 4: Preparation method of modified pectin material
[0045] 0.5 g of low methoxy pectin LMP was dissolved in 50 mL of water, and the mixture was stirred for 30 min to be evenly mixed to obtain a low methoxy pectin solution. 0.1 g of ascorbic acid and 1.0 g of tannic acid TA were added to the low methoxy pectin solution, and the mixture was stirred for 10 min to obtain a mixed solution. 2 mL of 2 mol / L hydrogen peroxide solution was added to the mixed solution, and the mixture was reacted for 24 h under a nitrogen atmosphere to obtain a reaction product. The reaction product was dialyzed in deionized water for 72 h and then freeze-dried to obtain a modified pectin material LMP-TA4.
[0046] Test Example 1: Structural Characterization
[0047] The tannic acid TA, low methoxyl pectin TMP and modified pectin material LMP-TA3 in Example 3 were characterized. Figure 1 shown.
[0048] The above substances were characterized by FTIR, and the results were as follows Figure 1 Specifically, the spectra of the above substances were collected using a Nicolet iS5 FTIR spectrometer (Thermo Fisher Scientific, USA) with a scanning range of 64 times in the range of 4000-400 cm -1 .
[0049] Depend on Figure 1 (A) It can be seen that at 3550cm -1 Nearby is the absorption peak of -OH on the carboxyl group of the LMP main chain. In the LMP spectrum, 1741 cm -1 and 1618cm -1 The peaks at 1417 cm-1 and 1427 cm-2 are attributed to the C=O vibration peaks in the esterified carboxyl group (-COOR) and free carboxyl group (-COOH) of LMP, respectively. -1 The peak at 1624 cm-1 may be related to the stretching vibration of CH2OH and CH3CO. -1 ) is significantly lower, located at 1417cm -1 The peak of LMP-TA at 900 cm -1 A single peak of isolated hydrogen on the catechol benzene ring appeared, but LMP did not show an absorption peak there. This shows that tannic acid TA was successfully grafted onto the side chain of low methoxy pectin LMP.
[0050] The above three substances were also characterized by UV-Vis. The results are as follows Figure 1 Specifically, the UV-visible spectrum of the above-mentioned substance is monitored using full-wavelength UV, and the wavelength is set to 200-700nm.
[0051] Depend on Figure 1 (B) It can be seen that the modified pectin material LMP-TA has absorption peaks at 260-280nm, which corresponds to the characteristic peaks of LMP-TA grafted on the benzene ring in the main chain TA. Therefore, it can be shown that tannic acid TA is successfully grafted onto low methoxyl pectin LMP.
[0052] Test Example 2: Film Property Testing
[0053] Low methoxyl pectin LMP and the modified pectin materials obtained in Examples 1-4 were prepared into films, and the mechanical properties, water vapor permeability (WVP) and adhesion properties of the films were investigated.
[0054] The steps of preparing the film are as follows: dissolving low methoxyl pectin LMP and modified pectin materials LMP-TA1, LMP-TA2, LMP-TA3, LMP-TA4 prepared in Examples 1-4 in deionized water respectively, stirring at room temperature for 20 minutes, and preparing 4 wt% pectin coating liquid LMP and 4 wt% modified pectin coating liquids LMP-TA1, LMP-TA2, LMP-TA3, LMP-TA4 respectively;
[0055] Then take 20 mL of the above coating liquids LMP-TA1, LMP-TA2, LMP-TA3, LMP-TA4 and LMP, respectively, place them on polytetrafluoroethylene molds, and dry them at room temperature to obtain modified pectin films LMP-TA1, LMP-TA2, LMP-TA3, LMP-TA4 and pectin film LMP, respectively.
[0056] 1. UV transmittance
[0057] The specific steps are as follows: the prepared modified pectin films LMP-TA1, LMP-TA2, LMP-TA3, LMP-TA4 and pectin film LMP are cut into rectangles of 60 nm × 15 nm and placed in a quartz dish. The transmittance of the above films is detected in the wavelength range of 200-800 nm using a full-wavelength UV-visible spectrophotometer (Shimadzu, UV-2700, Japan). The results are as follows: Figure 2 shown.
[0058] Depend on Figure 2 (A) It can be seen that the UV transmittance of the modified pectin material in the range of 200-400nm decreased from 43.97% to nearly 0, which shows that TA grafting improves the UV blocking performance. This is due to the aromatic rings and conjugated double bonds in the grafted LMP absorbing strong electromagnetic radiation in the UV range, and this absorption helps to mitigate potential food damage by delaying the formation of free radicals.
[0059] 2. Mechanical properties
[0060] The specific steps are as follows: the mechanical properties of modified pectin films LMP-TA1, LMP-TA2, LMP-TA3, LMP-TA4 and pectin film LMP were tested by an automatic tensile testing machine (Labthink Instruments Co. Ltd, Jinan, China), the mechanical properties including tensile strength (TS, MPa) and elongation at break (EAB, %). During the test, the original clamping distance was 40 mm and the clamping speed was 1 mm / s. The results are as follows: Figure 2 shown.
[0061] Tensile strength TS and elongation at break EAB are key factors in reflecting film performance. Figure 2 It can be seen that the tensile strength of the film LMP made of pectin alone is only 10.90MPa, while the tensile strength of the modified pectin LMP-TA prepared by the present invention is 15.43-24.00MPa. At the same time, the elongation at break of the film made of pectin LMP alone is 9.47%, while the elongations at break of the modified pectins LMP-TA1, LMP-TA2, LMP-TA3, and LMP-TA4 prepared by the present invention are 12.47%, 14.00%, 15.53%, and 16.23%, respectively. It can be seen that the present invention can significantly improve the tensile properties and flexibility of the film by grafting tannic acid on pectin.
[0062] After grafting tannic acid onto pectin, the addition of phenolic hydroxyl groups strengthens the interaction between molecules, thereby improving the tensile strength. After being modified with tannic acid, the interaction between pectins after modification promotes the interweaving of molecules, thereby improving the flexibility of the film.
[0063] 3. Water Vapor Permeability (WVP)
[0064] The specific steps are as follows: the modified pectin films LMP-TA1, LMP-TA2, LMP-TA3, LMP-TA4 and pectin film LMP were cut into circles with a diameter of 80 nm, and then the WVP of the films was measured using a PERME W3 / 031WVP detector.
[0065] The WVP test conditions are: 53% RH and 23°C, preheating time is 1h, weighing interval is 5min, and the results are as follows: Figure 2 shown.
[0066] The water exchange between the product and the external environment directly affects the shelf life of the product. Generally, packaging materials should minimize water transfer to protect the food from moisture. Figure 2 It can be seen that the film made of pectin LMP alone has the highest WVP value of 2.015×10 -12g / cm·s·Pa, which is due to the large number of hydroxyl groups in pectin LMP, resulting in the weakest water vapor barrier performance. In contrast, the WVP value of the modified pectin LMP-TA prepared in the present invention is 1.567-1.160×10 -12 g / cm·s·Pa, compared with the film made of pectin LMP alone, its WVP value is reduced by 22.23%-42.43%. It can be seen that the grafting treatment of pectin with tannic acid enhances the interaction between molecules and makes the molecules more compact, thereby reducing the water vapor permeability of the film.
[0067] 4. Adhesion performance
[0068] The pull-out test method was used to measure the adhesive strength of the modified pectin films LMP-TA1, LMP-TA2, LMP-TA3, LMP-TA4, and pectin film LMP. The specific steps are:
[0069] (1) 4 wt % modified pectin coating liquid LMP-TA1, LMP-TA2, LMP-TA3, LMP-TA4 and 4 wt % pectin coating liquid LMP were coated on two 10 cm × 2.5 cm PTFE plates respectively, ensuring that the contact area was 2.5 cm × 2.5 cm. The two PTFE plates were overlapped and dried at 50° C. for 6 h. Then, the tensile strength TS and the maximum tensile force MF were tested respectively. The results are shown in FIG. Figure 3 shown.
[0070] (2) 4 wt % modified pectin coating liquids LMP-TA1, LMP-TA2, LMP-TA3, LMP-TA4 and 4 wt % pectin coating liquid LMP were dyed red with 0.1 wt % Allura Red to facilitate subsequent experiments to observe their adhesion ability.
[0071] (3) 1 mL of modified pectin coating liquid LMP-TA1, LMP-TA2, LMP-TA3, LMP-TA4 and pectin coating liquid LMP were respectively dropped on a glass plate (76×26 mm) and spread on the entire plate, and then dried naturally at 25°C for 24 hours. The dried glass plate containing pectin coating materials was placed in 150 mL of deionized water, and the dissolution of the two edible pectin coatings on the glass plate was observed. The absorbance of allura red in deionized water was measured and recorded at certain time intervals, and the adhesion ability curves of LMP and LMP-TA on the glass plate were drawn. The results are shown in FIG. Figure 3 shown.
[0072] (4) Take another 1 mL of the dyed modified pectin coating liquid LMP-TA1, LMP-TA2, LMP-TA3, LMP-TA4 and pectin coating liquid LMP and drop them on a polytetrafluoroethylene (PTFE) plate. Then tilt the plate 45° to allow the pectin to slide along the plate. Observe and record the residual amount of coating material in the flow channel and on the plate at 10 s, 30 s and 60 s, respectively. The results are shown in the figure. Figure 3 shown.
[0073] The present invention uses PTFE to simulate the surface of a food substrate, and performs tensile force tests on low methoxyl pectin LMP and the modified pectin LMP-TA prepared in Examples 1-4. Figure 3 (A) It can be seen that the adhesion of pectin LMP alone is poor, and its MF value is low, which is 7.37N. In contrast, the LMP-TA film prepared by the present invention shows a higher MF value, and LMP-TA1, LMP-TA2, LMP-TA3, and LMP-TA4 are 12.2N, 15.4N, 19.6N, and 20.1N, respectively. It can be seen that the present invention can significantly improve the adhesion of the material by grafting pectin with tannic acid TA. This is because the catechol groups and the groups on the surface of PTFE (-NH2 and -COOH) combine with each other, thereby generating interfacial adhesion. In addition, the higher the degree of grafting, the greater the maximum tensile force reflected, and the better the adhesion performance, which shows that the catechol group has a direct relationship with the adhesion performance. The adhesion results of the dyed LMP and LMP-TA on the PTFE plate are shown in Figure 2. Figure 3 As shown by Figure 3 (C) It can be seen that after the same volume of coating liquid slides on the PTFE plate, the residual amount of LMP-TA on the flow mark is higher and the sliding speed is slower, indicating that TA-grafted pectin has better adhesion on the hydrophobic interface. Figure 3 (B) It can be seen that different coating solutions have different solubility in water, among which LMP-DA4 has the slowest dissolution rate in water. In summary, the adhesion ability of LMP on the hydrophobic interface is significantly improved after DA grafting.
[0074] Test Example 2: Banana preservation experiment
[0075] This experiment set up four treatment groups, using different coating materials to carry out banana preservation experiments, and tested the weight loss rate, color and hardness of bananas during the experiment to study the preservation effect of different coating materials. The specific steps are:
[0076] Twelve fresh bananas were randomly divided into four groups, namely treatment groups 1 to 4, and the bananas in each treatment group were coated by dipping. Specifically, the bananas in each treatment group were completely immersed in different coating solutions for 5 seconds, taken out and placed on a tray for storage.
[0077] Among them, the bananas in each treatment group were stored for a total of 7 days. During the storage, the temperature was maintained at 25°C and the humidity was 75% to ensure consistent management of the bananas in each treatment group during storage. The weight, color, and hardness of each group of bananas were measured every day, and photos were taken to record the changes in the appearance of the bananas during storage.
[0078] The details of each treatment group are as follows:
[0079] Treatment group 1: control group, distilled water was used as the coating solution in this treatment group;
[0080] Treatment group 2: LMP group, this treatment group only uses low methoxyl pectin LMP as a coating material, and mixes the coating material with water to obtain a 1wt% coating solution LMP;
[0081] Treatment group 3: LMP / TA group, in this treatment group, a mixture of low methoxyl pectin LMP and tannic acid in a mass ratio of 1:1 was used as a coating material, and the coating material was mixed with water to obtain a 1wt% coating solution LMP / TA;
[0082] Treatment group 4: LMP-TA group. This treatment group used the modified pectin material LMP-TA3 prepared in Example 3 as a coating material, and mixed the coating material with water to obtain a 1 wt% coating solution LMP-TA.
[0083] 1. Weight loss rate
[0084] Weigh and record the weight of bananas at a fixed time every day, and calculate the weight loss rate of bananas. The results are as follows Figure 5 As shown. Among them, the calculation formula of weight loss rate (%) is:
[0085]
[0086] Where W0 is the initial weight of the banana, W x is the weight of bananas stored at different times.
[0087] Weight loss rate is an important indicator for evaluating the post-harvest quality of fruits. Bananas are typical respiratory climacteric fruits. During storage, due to their own cellular respiration and transpiration, the water inside them is consumed and migrates and diffuses to the outside, resulting in changes in quality.
[0088] pass Figure 5It can be seen that the cnotrol group is used as a blank control, and the banana is directly exposed to the environment, and the weight loss rate decreases the most. After storage for 7 days, the weight loss rate of the banana is 7.1% after the modified pectin material LMP-TA is used for smearing treatment, and the weight loss rate of the banana is 10.1% after the banana is smeared with LMP / TA obtained by physical mixing of low methoxy pectin LMP and tannic acid TA. After the banana is smeared with only low methoxy pectin LMP, the weight loss rate of the banana is 13.2%. It can be seen that the present invention uses tannic acid to graft pectin, which can significantly reduce the weight loss rate of bananas compared to the simple compounding of the two. Therefore, the modified pectin continuously forms a film to reduce the weight loss rate of bananas during storage by improving its adhesion performance on the hydrophobic surface of fruits and vegetables.
[0089] 2. Color
[0090] The color of bananas was observed using a CR 400 colorimeter (Konica Minolta, Japan). The color of each banana was measured every day, and the color analysis of bananas in each treatment group was calculated. The results are shown in Figure 4 As shown. Among them, the color analysis (L * ) is calculated by the following formula;
[0091]
[0092] Where ΔL is the difference between the measured darkness and the initial darkness, Δa is the difference between the measured redness and the initial redness, and Δb is the difference between the measured yellowness and the initial yellowness.
[0093] Fresh fruits are likely to change color once harvested due to pigment degradation. The color of fruits during storage is an important factor in determining consumer purchasing preferences. Figure 4 (A) It can be seen that the control group had mold on the surface on the third day, which is a typical pathological manifestation of bananas after harvest. In contrast, the LMP-TA coating group had no obvious surface damage. Figure 4 (B) It can be seen that during storage, LMP-TA group * The value decreased from 78.11±0.73 to 71.88±0.60, a decrease of only 7.97%, while the LMP and LMP / TA groups and the control group showed significant decreases, respectively. It can be seen that LMP-TA is effective in maintaining fruit color due to its improved control of banana respiration rate, enzymatic and oxidative reactions.
[0094] 3. Hardness
[0095] The hardness of bananas was measured using a texture device (TA-XT plus, Godalming, UK). The test speed was 1 mm / s, the puncture displacement was 10 mm, and the center of the banana was used as the measurement point for three measurements. The average value was taken. Figure 6 shown.
[0096] The maintenance of fruit hardness mainly depends on the primary cell wall composed of cellulose, pectin and hemicellulose. During the ripening process of the fruit, the peel tissue and cell wall components, intracellular substances and cell structures of the banana dissolve or depolymerize, causing the fruit to soften and the hardness to decrease. When these structures degenerate, the long chain of pectin compounds in bananas shortens, increasing the activity of pectinesterase and polygalacturonase. The activities of these enzymes are usually triggered by O2 and CO2. Therefore, the coating needs to have good barrier properties.
[0097] Depend on Figure 6 It can be seen that after 1 day of storage, the hardness of the bananas was 51g when the modified pectin material was used for preservation treatment. After 7 days of storage, the hardness was 35g, and the hardness decreased by 31.4%. After the LMP / TA material was used for preservation treatment, the hardness of the bananas decreased by 38.3%. The hardness of the bananas only using the LMP material for preservation treatment decreased by 45.7%, and the hardness of the bananas in the blank control group decreased by 59.1%. It can be seen that the present invention can significantly delay the aging process of bananas by using tannic acid grafted pectin as a coating, which is conducive to improving the shelf life of bananas.
[0098] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A method for preparing a modified pectin material, characterized in that: The steps include: (1) dissolving low methoxy pectin in water to obtain a low methoxy pectin solution; adding ascorbic acid and tannic acid to the low methoxy pectin solution, stirring, and obtaining a mixed solution; Then, adding hydrogen peroxide solution to the mixed solution for reaction to obtain a reaction product; (2) The reaction product is dialyzed and then dried to obtain a modified pectin material.
2. The method for preparing the modified pectin material according to claim 1, characterized in that: In step (1), the solid-liquid ratio of low-methoxy pectin to water is (0.3-0.6) g:50 mL.
3. The method for preparing the modified pectin material according to claim 1, characterized in that: In step (1), the mass ratio of low methoxy pectin to ascorbic acid is (0.3-0.6):0.
1.
4. The method for preparing the modified pectin material according to claim 1, characterized in that: In step (1), the mass ratio of low methoxy pectin to tannic acid is 2:(1-4).
5. The method for preparing the modified pectin material according to claim 1, characterized in that: In step (1), the solid-liquid ratio of low-methoxy pectin to hydrogen peroxide solution is (0.3-0.6) g: 2 mL; and the concentration of the hydrogen peroxide solution is 2 mol / L.
6. The method for preparing the modified pectin material according to claim 1, characterized in that: In step (1), the stirring time is 5-15 min, the reaction is carried out under a protective atmosphere of nitrogen, and the reaction time is 20-30 h.
7. The method for preparing the modified pectin material according to claim 1, characterized in that: In step (2), the dialysis operation is: placing the reaction product in deionized water for 70-75 hours.
8. The modified pectin material prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the modified pectin material according to claim 8 in preserving fruits and vegetables.
Citation Information
Cited By
Fresh-keeping coating film as well as preparation method and application thereof
CN119498402A
A fresh-keeping coating film, preparation method and application thereof
CN119498402B