Anchoring agent for photocuring silicon-based release agent and preparation method of anchoring agent
By using anchoring agents with modified nanosilicon dioxide and other additives in photocurable silicon-based release agents, the problem of poor binding performance with substrate is solved, the curing speed and service life are improved, and the performance of the coating is enhanced .
Patent Information
- Application Number
- CN202411113455.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
AI Technical Summary
The poor bonding performance of existing photocuring silicon-based release agents and substrates leads to coat shedding and short service life, affecting industrial production efficiency.
A type of curing agent, including vinyl triacetoxysilane, gamma-(methacryloyloxy)propyl trimethoxysilane, epoxypropyl trimethoxysilane, nanosilica, thixotropy The anchoring agent of the agent, defoaming agent and surfactant was prepared by homogenizing high pressure and uniformly processing of stirring to enhance the interface bonding performance.
It significantly improves the bonding ability of the photocured release agent and the substrate, extends the service life, shortens the curing time, and increases the hardness and impact strength of the coating, reducing the layering phenomenon of the coating.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of release agent auxiliary materials, and particularly relates to an anchoring agent for a photocurable silicon-based release agent and a preparation method thereof. Background Art
[0002] Silicone oil type release agent is a widely used release agent at present. It is widely used in daily chemical products due to its simple preparation conditions, good adhesion and separation, good durability, and no need for solvents. When the release agent is coated on PET, PP, PE and other materials, its surface has poor bonding performance with silicone oil. Long-term storage will cause the release agent to fall off or even transfer to the surface of the pressure-sensitive adhesive, thereby affecting the use of the pressure-sensitive adhesive.
[0003] According to the different curing mechanisms, silicone release agents can be divided into heat addition type, condensation type, cationic polymerization type, electron beam irradiation curing type and ultraviolet light (UV) curing type. The most common silicone release agent is heat addition type, but the application scope of this type of release agent is limited. At present, ultraviolet light (UV) curing type release agents are widely used because of their light application range, low pollution and toxicity, but they often have poor bonding with the substrate, resulting in a decrease in the release force of the release paper or film during use or storage, and even the coating falling off, making the release agent ineffective. The long light curing time affects industrial production efficiency.
[0004] Therefore, the anchoring agent used for photocurable silicone-based release agent has application prospects, which can further improve the various capabilities of the photocurable silicone-based release agent and promote its popularization and use. Summary of the invention
[0005] In view of this, the purpose of the present invention is to provide an anchoring agent for a photocurable silicone-based release agent and a preparation method thereof. The anchoring agent obtained by the present invention can improve the bonding ability between the photocurable release agent and the substrate, and improve the environmental weather resistance and service life.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] In a first aspect, the present invention provides an anchoring agent for a photocurable silicone-based release agent, comprising the following raw materials in parts by weight:
[0008] 5-20 parts of curing accelerator, 80-100 parts of vinyl triacetoxy silane, 10-30 parts of γ-(methacryloyloxy)propyl trimethoxy silane, 60-80 parts of glycidoxypropyl trimethoxy silane, 0.1-2 parts of nano silicon dioxide, 0.5-2 parts of thixotropic agent, 0.5-2 parts of defoaming agent and 1-3 parts of surfactant.
[0009] Preferably, the raw materials are: 10-15 parts of a curing agent, 85-95 parts of vinyl triacetoxy silane, 15-25 parts of γ-(methacryloyloxy)propyl trimethoxy silane, 65-75 parts of glycidoxypropyl trimethoxy silane, 0.1-2 parts of nano silicon dioxide, 0.5-2 parts of a thixotropic agent, 0.5-2 parts of a defoaming agent, and 1-3 parts of a surfactant.
[0010] Preferably, the curing accelerator is prepared by mixing tetraethoxysilane, acrylate and a catalyst and reacting the mixture at 50-70° C. for 1-2 hours.
[0011] Preferably, the particle size of the nano silicon dioxide is 10-50 nm. By adopting the above technical solution, the nano silicon dioxide has good dispersibility in the photocuring system, can effectively enhance the hardness of the photocuring film, improve the hardness, impact strength, wear resistance and other properties of the photocuring coating, and the modified nano silicon dioxide has good compatibility with the base material and migrates to the film surface, which helps to improve the interface bonding performance between the photocuring layer and the substrate.
[0012] Preferably, the thixotropic agent is hydrogenated castor oil or hydroxyethyl cellulose. By adopting the above technical solution, hydrogenated castor oil and hydroxyethyl cellulose can help the release agent to form a uniform coating on the mold surface by forming a three-dimensional network structure, and at the same time maintain stability when removing the mold to prevent the coating from cracking or falling off; and it is helpful to mix the anchoring agent and the release agent, and it is not easy to have side effects such as stratification.
[0013] Preferably, the defoamer is a mineral oil defoamer, a silicone defoamer or a polyether defoamer.
[0014] Preferably, the surfactant is an aminosilane coupling agent or a silane coupling agent.
[0015] In a second aspect, the present invention provides a method for preparing the above-mentioned anchoring agent for photocurable silicone-based release agent, comprising the following steps:
[0016] 1) weighing the raw materials according to the weight parts;
[0017] 2) mixing and modifying nano-silicon dioxide with a surfactant to obtain modified nano-silicon dioxide;
[0018] 3) mixing a curing agent, vinyl triacetoxysilane, γ-(methacryloyloxy)propyl trimethoxysilane, and glycidoxypropyl trimethoxysilane, and homogenizing under high pressure to obtain a mixed solution;
[0019] 4) The mixed solution, thixotropic agent and defoaming agent are mixed and added with stirring while the modified nano-silicon dioxide is mixed evenly to obtain an anchoring agent for the photocurable silicon-based release agent.
[0020] Preferably, the pressure of high pressure homogenization in step 3) is 10-15 MPa, and the homogenization time is 5-10 min.
[0021] Preferably, the stirring rate in step 4) is 200-300 rpm.
[0022] Beneficial technical effects:
[0023] 1. The anchoring agent prepared by the present invention can improve the bonding ability between the light-curing release agent and the substrate, and improve the environmental weather resistance and service life.
[0024] 2. The anchoring agent prepared by the present invention further improves the curing speed of the light-curing release agent, and can be applied to a variety of light-curing release agents, has no adverse reactions, is not easy to delaminate, and has a wide range of applications.
[0025] 3. The preparation method of the anchoring agent of the present invention is simple, and the mixing effect can be improved by high-pressure homogenization, which greatly reduces the time for stirring and mixing. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.
[0028] Example 1
[0029] This embodiment provides an anchoring agent for a photocurable silicone-based release agent, comprising the following preparation steps:
[0030] 1) tetraethoxysilane, acrylate and stannous octoate catalyst are mixed and reacted at 50° C. for 1 hour to obtain a curing agent;
[0031] 2) Weigh 5 parts of curing agent, 80 parts of vinyl triacetoxysilane, 10 parts of γ-(methacryloyloxy)propyl trimethoxysilane, 60 parts of glycidoxypropyl trimethoxysilane, 0.1 parts of nano-silicon dioxide, 0.5 parts of hydrogenated castor oil, 0.5 parts of polydimethylsiloxane, and 1 part of aminosilane coupling agent by weight;
[0032] 3) mixing the nano-silica and the aminosilane coupling agent for 20 minutes to obtain modified nano-silica;
[0033] 4) mixing the curing agent, vinyl triacetoxysilane, γ-(methacryloyloxy)propyl trimethoxysilane and glycidoxypropyl trimethoxysilane, and homogenizing for 5 minutes at a pressure of 10 MPa to obtain a mixed solution;
[0034] 5) The mixed solution, hydrogenated castor oil and polydimethylsiloxane are mixed and stirred at a rate of 200 rpm while adding modified nano-silicon dioxide to mix evenly to obtain an anchoring agent for a photocurable silicone-based release agent.
[0035] Example 2
[0036] This embodiment provides an anchoring agent for a photocurable silicone-based release agent, comprising the following preparation steps:
[0037] 1) tetraethoxysilane, acrylate and stannous octoate catalyst are mixed and reacted at 70° C. for 2 h to obtain a curing agent;
[0038] 2) Weighing by weight 20 parts of a curing agent, 100 parts of vinyl triacetoxysilane, 30 parts of γ-(methacryloyloxy)propyl trimethoxysilane, 80 parts of glycidoxypropyl trimethoxysilane, 2 parts of nano-silica, 2 parts of hydrogenated castor oil, 2 parts of polydimethylsiloxane, and 3 parts of an aminosilane coupling agent;
[0039] 3) mixing the nano-silica and the aminosilane coupling agent for 40 minutes to obtain modified nano-silica;
[0040] 4) mixing the curing agent, vinyl triacetoxysilane, γ-(methacryloyloxy)propyl trimethoxysilane and glycidoxypropyl trimethoxysilane, and homogenizing for 10 minutes at a pressure of 15 MPa to obtain a mixed solution;
[0041] 5) The mixed solution, hydrogenated castor oil and polydimethylsiloxane were mixed and stirred at a rate of 300 rpm while adding modified nano-silicon dioxide to mix evenly to obtain an anchoring agent for the photocurable silicone-based release agent.
[0042] Example 3
[0043] This embodiment provides an anchoring agent for a photocurable silicone-based release agent, comprising the following preparation steps:
[0044] 1) tetraethoxysilane, acrylate and stannous octoate catalyst are mixed and reacted at 60° C. for 1.5 h to obtain a curing agent;
[0045] 2) Weigh 10 parts of a curing agent, 90 parts of vinyl triacetoxysilane, 20 parts of γ-(methacryloyloxy)propyl trimethoxysilane, 70 parts of glycidoxypropyl trimethoxysilane, 1 part of nano-silicon dioxide, 1 part of hydrogenated castor oil, 1 part of polyoxypropylene glycidyl ether, and 2 parts of a silane coupling agent by weight;
[0046] 3) mixing the nano-silica and the silane coupling agent for 30 minutes to obtain modified nano-silica;
[0047] 4) mixing the curing agent, vinyl triacetoxysilane, γ-(methacryloyloxy)propyl trimethoxysilane and glycidoxypropyl trimethoxysilane, and homogenizing for 7 minutes at a pressure of 12 MPa to obtain a mixed solution;
[0048] 5) The mixed solution, hydrogenated castor oil and polyoxypropylene epoxyethylene glycerol ether are mixed at a rate of 250 rpm and the modified nano-silicon dioxide is added and mixed evenly to obtain an anchoring agent for a photocurable silicone-based release agent.
[0049] Example 4
[0050] This embodiment provides an anchoring agent for a photocurable silicone-based release agent, comprising the following preparation steps:
[0051] 1) tetraethoxysilane, acrylate and stannous octoate catalyst are mixed and reacted at 60° C. for 1.5 h to obtain a curing agent;
[0052] 2) Weigh 10 parts of a curing agent, 85 parts of vinyl triacetoxysilane, 15 parts of γ-(methacryloyloxy)propyl trimethoxysilane, 65 parts of glycidoxypropyl trimethoxysilane, 0.1 parts of nano-silicon dioxide, 0.5 parts of hydroxyethyl cellulose, 0.5 parts of polyoxypropylene glycidyl ether, and 1 part of a silane coupling agent by weight;
[0053] 3) mixing the nano-silica and the silane coupling agent for 30 minutes to obtain modified nano-silica;
[0054] 4) mixing the curing agent, vinyl triacetoxysilane, γ-(methacryloyloxy)propyl trimethoxysilane and glycidoxypropyl trimethoxysilane, and homogenizing for 7 minutes at a pressure of 12 MPa to obtain a mixed solution;
[0055] 5) The mixed solution, hydroxyethyl cellulose and polyoxypropylene ethylene glycol ether are mixed and stirred at a rate of 250 rpm while adding the modified nano-silicon dioxide to mix evenly to obtain an anchoring agent for the photocurable silicone-based release agent.
[0056] Example 5
[0057] This embodiment provides an anchoring agent for a photocurable silicone-based release agent, comprising the following preparation steps:
[0058] 1) tetraethoxysilane, acrylate and stannous octoate catalyst are mixed and reacted at 60° C. for 1.5 h to obtain a curing agent;
[0059] 2) Weigh 15 parts of a curing agent, 95 parts of vinyl triacetoxysilane, 25 parts of γ-(methacryloyloxy)propyl trimethoxysilane, 75 parts of glycidoxypropyl trimethoxysilane, 2 parts of nano-silicon dioxide, 2 parts of hydroxyethyl cellulose, 2 parts of polyoxypropylene glycidyl ether, and 3 parts of a silane coupling agent by weight;
[0060] 3) mixing the nano-silica and the silane coupling agent for 30 minutes to obtain modified nano-silica;
[0061] 4) mixing the curing agent, vinyl triacetoxysilane, γ-(methacryloyloxy)propyl trimethoxysilane and glycidoxypropyl trimethoxysilane, and homogenizing for 7 minutes at a pressure of 12 MPa to obtain a mixed solution;
[0062] 5) The mixed solution, hydroxyethyl cellulose and polyoxypropylene ethylene glycol ether are mixed and stirred at a rate of 250 rpm while adding the modified nano-silicon dioxide to mix evenly to obtain an anchoring agent for the photocurable silicone-based release agent.
[0063] Comparative Example 1
[0064] The preparation steps of this comparative example are the same as those of Example 1, except that the raw materials do not contain a curing accelerator.
[0065] Comparative Example 2
[0066] The preparation steps of this comparative example are the same as those of Example 1, except that the raw materials do not contain a thixotropic agent.
[0067] Comparative Example 3
[0068] The preparation steps of this comparative example are the same as those of Example 1, except that the raw materials do not contain nano-silicon dioxide.
[0069] Comparative Example 4
[0070] The preparation steps of this comparative example are the same as those of Example 1, except that high-pressure homogenization is not used in the step, and mechanical stirring is used for 3 hours.
[0071] Experimental Example 1
[0072] Preparation of release agent: 10 parts of amino silicone oil, 10 parts of methyl silicone oil, 5 parts of ethylene-methyl acrylate-glycidyl methacrylate, 8 parts of reactive diluent, 0.1 parts of antioxidant, 0.5 parts of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 20 parts of solvent, and 2 parts of anchoring agent;
[0073] The anchoring agent is obtained from Examples 1-5 and Comparative Examples 1-4. The release agents are numbered as Examples 1-5 and Comparative Examples 1-4 according to the source of the anchoring agent, and the group without anchoring agent is the blank group. The release agent prepared above is coated on a PET film with a thickness of 50 μm, and the coating thickness is controlled to be 600 nm. The film is cured by UV lamp irradiation to obtain a release film.
[0074] Performance testing:
[0075] Curing time;
[0076] Peel test: Refer to GB / T 25256-2010 for room temperature peel force test: 25.4mm wide MY2G standard test tape is attached to the test surface of the release material to make a test specimen, and a 2kg standard pressure roller is used to reciprocate and roll the test specimen for 3 times, and the test specimen is left to stand for 20 minutes. The release material is fixed, and the standard test tape is stretched with a tensile machine at a peeling angle of 180° and a peeling speed of 300mm / min to measure the room temperature peel force;
[0077] The release film was aged at 75°C for 10 h and then subjected to a peeling test using the same method.
[0078] Residual Adhesion Test: Refer to GB / T 25256-2010 for residual adhesion test. Stick the standard tape peeled off in the peeling force test on the steel plate again, roll it back and forth 3 times with a 2kg standard roller, and peel it 180° at a speed of 300mm / min using a tensile testing machine to obtain the test value L1. Stick a new MY2G standard test tape that has not been in contact with the release material on the steel plate, roll it back and forth 3 times with a 2kg standard roller, place it in an environment with room temperature of 23℃ and relative humidity of 50% for 20 minutes, peel it 180° at 300mm / min, and record the value L0. Residual Adhesion = L1 / L0×100%.
[0079] Table 1 Performance test
[0080]
[0081]
[0082] According to Table 1, it can be explained that the anchoring agent obtained in Examples 1-5 of the present application can significantly improve the bonding force between the release film and the substrate, reduce the light curing time, have anti-aging ability and environmental tolerance, and improve the stripping ability.
[0083] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. An anchoring agent for a photocurable silicone-based release agent, characterized in that: The invention comprises the following raw materials in parts by weight: 5-20 parts of curing accelerator, 80-100 parts of vinyl triacetoxy silane, 10-30 parts of γ-(methacryloyloxy)propyl trimethoxy silane, 60-80 parts of glycidoxypropyl trimethoxy silane, 0.1-2 parts of nano silicon dioxide, 0.5-2 parts of thixotropic agent, 0.5-2 parts of defoaming agent and 1-3 parts of surfactant.
2. The anchoring agent for photocurable silicone-based release agent according to claim 1, characterized in that: The raw materials are: 10-15 parts of a curing accelerator, 85-95 parts of vinyl triacetoxy silane, 10-30 parts of gamma-(methacryloyloxy)propyl trimethoxy silane, 60-80 parts of glycidoxypropyl trimethoxy silane, 0.1-2 parts of nano silicon dioxide, 0.5-2 parts of a thixotropic agent, 0.5-2 parts of a defoaming agent, and 1-3 parts of a surfactant.
3. The anchoring agent for photocurable silicone-based release agent according to claim 1, characterized in that: The preparation method of the curing accelerator is as follows: tetraethoxysilane, acrylate and a catalyst are mixed and reacted at 50-70° C. for 1-2 hours to obtain the curing accelerator.
4. The anchoring agent for photocurable silicone-based release agent according to claim 1, characterized in that: The particle size of the nano silicon dioxide is 10-50nm.
5. The anchoring agent for photocurable silicone-based release agent according to claim 1, characterized in that: The thixotropic agent is hydrogenated castor oil or hydroxyethyl cellulose.
6. The anchoring agent for photocurable silicone-based release agent according to claim 1, characterized in that: The defoamer is a mineral oil defoamer, an organosilicon defoamer or a polyether defoamer.
7. The anchoring agent for photocurable silicone-based release agent according to claim 1, characterized in that: The surfactant is an aminosilane coupling agent or a silane coupling agent.
8. The method for preparing an anchoring agent for a photocurable silicone-based release agent according to claim 1, characterized in that: The following steps are involved: 1) weighing the raw materials according to the weight parts; 2) mixing and modifying nano-silicon dioxide with a surfactant to obtain modified nano-silicon dioxide; 3) mixing a curing agent, vinyl triacetoxysilane, γ-(methacryloyloxy)propyl trimethoxysilane, and glycidoxypropyl trimethoxysilane, and homogenizing under high pressure to obtain a mixed solution; 4) The mixed solution, thixotropic agent and defoaming agent are mixed and added with modified nano-silicon dioxide while stirring, and the mixture is evenly mixed to obtain an anchoring agent for the photocurable silicon-based release agent.
9. The preparation method according to claim 8, characterized in that: The pressure of the high pressure homogenization in step 3) is 10-15 MPa, and the homogenization time is 5-10 min.
10. The preparation method according to claim 8, characterized in that: The stirring rate in step 4) is 200-300 rpm.
Citation Information
Cited By
Emulsion type release agent and preparation method thereof
CN120648379A