High-strength high-thermal-conductivity high-entropy alloy particle reinforced copper-based composite material and preparation method thereof

Through ball milling and powder mixing and discharge plasma sintering processes, FeCoCrNi high-entropy alloy particles reinforced copper-based composite materials are prepared, which solves the problems of degraded thermal conductivity of traditional copper alloys and insufficient density of high-entropy alloys, and realizes high-performance copper-based composite materials .

CN118996181APending Publication Date: 2024-11-22CHANGZHOU UNIV
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411077155.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Traditional copper alloys have reduced electrical and thermal conductivity when their strength and hardness are increased, while high-entropy alloys have insufficient density and plasticity of copper-based composite materials, which affects their processing and application.

Method used

Using ball milling powder mixing and discharge plasma sintering technology, FeCoCrNi high-entropy alloy particles with single-phase FCC structure are used as the reinforced phase, with a particle size of 45-105μm and a high-entropy alloy content of 5-20wt.%, combining ball milling and discharge plasma Sintering process, prepare high-entropy alloy particle-reinforced copper-based composite materials.

Benefits of technology

It has achieved high density, excellent strong plasticity, thermal conductivity and high conductivity, tensile strength >150MPa, elongation of fracture >10.5%, thermal conductivity >105W·m-1·K-1, and conductivity >11MS/m , density >95%, suitable for electronic equipment and power systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996181A_ABST
    Figure CN118996181A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of copper-based composite materials, and particularly discloses a high-entropy alloy reinforced copper-based composite material and a preparation method thereof. A high-entropy alloy FeCoCrNi modified copper matrix with a single FCC (fluid catalytic cracking) structure and equivalent elements is selected, the content of the high-entropy alloy in the composite material is 5wt.%-20wt.%, the high-entropy alloy is distributed in a dispersed manner, and the particle size is 45-105 microns; the tensile strength of the composite material is larger than 150 MPa, the elongation at break is larger than 10.5%, the heat conductivity coefficient is larger than 105 W.m <-1 >. K <-1 >, and the conductivity is larger than 11 MS / m. The composite material is prepared by combining a ball milling method and a spark plasma sintering method, and the obtained composite material is higher in density and mechanical property, fewer in impurities and defects, excellent in strength and plasticity, excellent in heat-conducting property and higher in electric conductivity; the material is expected to be applied to the fields of connectors, electrical switches, transformer windings and the like of various electronic devices and power systems.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of copper-based composite materials, and specifically relates to a high-entropy alloy reinforced copper-based composite material and a preparation method thereof. Background Art

[0002] As a high-performance metal-based composite material, particle-reinforced copper-based composite materials are widely used in aerospace, automotive industry, energy and electronic devices. The improvement of strength and hardness of traditional copper alloys is often accompanied by a decrease in electrical and thermal conductivity. The performance of copper-based composite materials mainly depends on the performance of the copper matrix and reinforcement and the bonding characteristics between the matrix and reinforcement, which can make up for the shortcomings of copper alloys in some aspects. Compared with traditional copper alloys, particle-reinforced copper-based composite materials have better mechanical properties and physical properties. The common particle reinforcement phases of particle-reinforced copper-based composite materials currently include ceramic particles, metallic glass, intermetallic compound particles, amorphous alloy particles, etc. There are inevitably some limitations between the traditional reinforcement phase and the metal matrix, such as poor wettability and poor interface bonding, which limit the performance improvement of the composite material. High entropy alloys have excellent properties different from traditional alloys, such as unique strength and ductility, high hardness, high temperature resistance, corrosion resistance, etc., and the natural metallic properties of high entropy alloys make them have good compatibility with metal matrices. However, not all high entropy alloys can improve the comprehensive performance of copper-based composites. For example, Wei Ting's master's thesis "Research on High Entropy Alloy Reinforced Cu-based Composites" from Xi'an University of Technology disclosed the preparation of copper-based composites reinforced with AlFeCrCoNi high entropy alloys with BCC structure by powder metallurgy. However, the density of the composites finally obtained was generally low. When the high entropy alloy content was 10%, the density reached a maximum value of 89.1%. However, as the high entropy alloy content increased further, the density tended to decrease. Furthermore, strengthening the copper-based with AlFeCrCoNi high entropy alloy with BCC structure would sharply reduce the plasticity, seriously affecting the processing and application of the composites. Summary of the invention

[0003] In order to overcome the problems existing in the above-mentioned prior art, the present invention provides a high-strength, high-thermal-conductivity, high-entropy alloy particle reinforced copper-based composite material and a preparation method thereof through ball milling powder mixing and spark plasma sintering.

[0004] In order to achieve the purpose of the present invention, the technical solution adopted is as follows:

[0005] The present invention first provides a high entropy alloy particle reinforced copper-based composite material, wherein the high entropy alloy component is FeCoCrNi, which is a single FCC structure high entropy alloy, and the atomic proportions are: Fe25%, Co25%, Cr25%, Ni25%; the high entropy alloy content in the composite material is 5wt.% to 20wt.%, and the remainder is a pure copper matrix;

[0006] In the composite material, high entropy alloy particles are dispersed and have a particle size of 45 to 105 μm;

[0007] The composite material has a tensile strength of >150 MPa, a breaking elongation of >10.5%, and a thermal conductivity of >105 W·m -1 ·K -1 , conductivity>11MS / m.

[0008] The present invention also provides a method for preparing the high entropy alloy particle reinforced copper-based composite material, comprising the following steps:

[0009] Weighing powder: select commercial pure copper matrix powder with a particle size of 30-40 μm; FCC structure FeCoCrNi high entropy alloy powder prepared by gas atomization with a particle size of 45-105 μm, and the content of FeCoCrNi high entropy alloy powder is 5%-20% of the total mass of the composite powder;

[0010] Ball milling powder mixing: FeCoCrNi high entropy alloy powder and pure copper matrix powder are placed in a stainless steel ball mill, stainless steel ball milling balls are added, anhydrous ethanol is added as a process control agent, vacuum is evacuated, Ar is introduced as a protective gas, and a high-energy planetary ball mill is used for ball milling powder mixing; the ball-to-material ratio is set to 5-10:1, argon is filled into the stainless steel ball mill when the vacuum degree is lower than 0.1Pa, the ball mill speed is set to 240-300r / min, and the effective ball milling time is 6-10h;

[0011] Drying of composite powder: After ball milling, the stainless steel ball mill is vacuumed, and the residual composite powder on the wall of the mill is washed with anhydrous ethanol. The stainless steel ball mill is placed in a high-temperature blast drying oven for drying, and the composite powder is obtained by sieving the powder;

[0012] Pre-pressing: Weigh a certain amount of composite powder, put it into a hot isostatic pressing graphite mold with carbon paper around it, and pre-press it with a manual hydraulic press;

[0013] Sintering: After the composite powder is pre-pressed and formed, it is placed in the furnace chamber of the spark plasma sintering system together with the graphite mold. Symmetrical graphite gaskets are placed between the mold and the upper and lower electrodes, and carbon paper is placed between the electrodes and the graphite gaskets. The system is evacuated, the sintering pressure is controlled at 40-60MPa, the sintering temperature is 750℃-950℃, the temperature is increased by 50℃ per minute, the holding time is 6-10min, and the furnace is cooled;

[0014] Demolding: The sintering program is terminated, the composite material is sintered and formed, the current and voltage are turned off, the system is vacuumed, the graphite mold is taken out, and a manual hydraulic press is used for demolding. The carbon paper residue on the surface of the composite material is polished with coarse sandpaper to obtain a high-entropy alloy particle-reinforced copper-based composite material.

[0015] In the above preparation method, the present invention uses FeCoCrNi high entropy alloy particles with a mass content of 5wt.% to 20wt.% single-phase FCC structure to reinforce the copper matrix, and at the same time combines the material particle size, ball milling mixing process, and the advantages of faster heating rate and more uniform heating temperature of the sample in the coordinated discharge plasma sintering process. The prepared FeCoCrNi high entropy alloy particle reinforced copper-based composite material has higher density and mechanical properties, fewer impurities and defects, and stronger controllability of process parameters. The final composite material has excellent strong plasticity, thermal conductivity and high electrical conductivity (tensile strength>150MPa, elongation at break>10.5%, thermal conductivity>105W·m -1 ·K -1 , conductivity>11MS / m, density>95%), and is expected to be used in various electronic equipment and power system connectors, electrical switches, transformer windings and other related fields.

[0016] As a preferred embodiment of the preparation method of the present invention, the FeCoCrNi high entropy alloy powder accounts for 5% to 10% of the total mass of the composite powder, and the sintering temperature is 950° C. It is further preferred that the FeCoCrNi high entropy alloy powder accounts for 10% of the total mass of the composite powder.

[0017] As a preferred embodiment of the preparation method of the present invention, the composite powder is placed in a high-temperature blast drying oven after ball milling, the temperature is set at 50° C., and the drying process lasts for 8 to 12 hours.

[0018] As a preferred embodiment of the preparation method of the present invention, the powder pre-pressing pressure ranges from 5 to 10 Pa, and the holding time is from 10 to 15 min.

[0019] As a preferred embodiment of the preparation method of the present invention, the high entropy alloy particle reinforced copper-based composite material has a density of >98%, a tensile strength of >150 MPa, an elongation at break of >11%, and a thermal conductivity of >110 W·m -1 ·K -1 , conductivity>13MS / m.

[0020] Compared with the prior art, the present invention also has the following technical advantages:

[0021] (1) The present invention uses FeCoCrNi high entropy alloy particles with a single-phase FCC structure, whose natural metallic properties enable them to have a good combination with the copper matrix to form an interface diffusion layer.

[0022] (2) The present invention adopts a method combining ball milling and spark plasma sintering, which has a simple preparation method, low preparation cost, high raw material utilization rate, and various sample shapes, and is suitable for large-scale industrial production.

[0023] The present invention prepares a new type of metal-based composite material, which provides a new idea for developing a metal-based composite material with strong plasticity matching and maintaining good physical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:

[0025] Figure 1 It is a process flow chart of the present invention.

[0026] Figure 2 This is the SEM image of the 5wt.% FeCoCrNi / Cu composite material prepared in Example 1.

[0027] Figure 3 This is the engineering stress-strain curve of the 5wt.% FeCoCrNi / Cu composite material prepared in Example 1, with a tensile strength of 152 MPa and an elongation at break of 28%.

[0028] Figure 4 This is the SEM image of the 10wt.% FeCoCrNi / Cu composite material prepared in Example 2.

[0029] Figure 5 This is the engineering stress-strain curve of the 10wt.% FeCoCrNi / Cu composite material prepared in Example 2, with a tensile strength of 252MPa and an elongation at break of 30%.

[0030] Figure 6 This is the SEM image of the 20wt.% FeCoCrNi / Cu composite material prepared in Example 3.

[0031] Figure 7 The engineering stress-strain curve of the 20wt.% FeCoCrNi / Cu composite material prepared in Example 3 has a tensile strength of 276MPa and an elongation at break of 11%.

[0032] Figure 8 This is the SEM image of the 10wt.% FeCoCrNi / Cu composite material prepared in Example 4.

[0033] Fig. 9 The engineering stress-strain curve of the FeCoCrNi / Cu composite material prepared in Example 5 shows a tensile strength of 238 MPa and an elongation at break of 10.6%.

[0034] Fig.10 The engineering stress-strain curve of the FeCoCrNi / Cu composite material prepared in Example 6 shows that the tensile strength is 196 MPa and the elongation at break is 7.8%.

[0035] Fig.11 The hardness distribution diagram of the matrix, interface and reinforcement phase of the FeCoCrNi / Cu composite material prepared in Examples 1 to 3, the hardness increases from the matrix to the reinforcement phase.

[0036] Fig.12 The thermal conductivity and electrical conductivity comparison diagram of the FeCoCrNi / Cu composite material prepared in Examples 1 to 3. The thermal conductivity of the composite material is > 110 W·m -1 ·K -1 , conductivity>13MS / m. DETAILED DESCRIPTION

[0037] In order to further understand the purpose, content and advantages of the present invention, the specific embodiments of the present invention are now described in detail as follows, but it is not limited to the following examples, and it is freely matched according to actual conditions. The endpoints and any values ​​of the scope disclosed in this article are not limited to the precise scope and value. For numerical ranges, between the endpoint values ​​of each scope, between the endpoint values ​​of each scope and a separate point value, and between separate point values, one or more new numerical ranges can be combined with each other, and these numerical ranges should be considered as specifically disclosed in this article.

[0038] The raw materials used in the embodiments of the present invention: FeCoCrNi high entropy alloy powder and pure Cu powder (99.9%) are all from Jirui Metal Materials (Shandong) Co., Ltd.

[0039] The instruments used in the embodiments of the present invention are as follows: the ball mill is a QM-QX-2L planetary ball mill produced by Changsha Miqi Technology Co., Ltd., and the sintering instrument is a Labox-325 spark plasma sintering furnace produced by Japan Si Li Co., Ltd.

[0040] The hardness test method in the following examples is: use HXD-1000TMC Vickers hardness tester to measure the hardness of the composite matrix, interface and reinforcement phase, set the load to 50gf, and the full load time to 15s. The hardness test sample is a disc with a diameter of 12.7mm and a height of 2.5mm.

[0041] The tensile performance parameter testing method in the following embodiments is as follows: the tensile test is carried out on a WDW-200 universal testing machine, and the tensile strain rate is set to 2×10 -4 / s. The dimensions of the tensile specimen were rectangular dog-bone specimens with a gauge length of 6.5 mm, a thickness of 1.2 mm, and a width of 2 mm.

[0042] The test conditions of the electrical conductivity in the following examples are: using a Seebeck coefficient measuring instrument, the electrical conductivity of the composite material is measured according to the four-probe method at room temperature 25° C. The thermal conductivity test sample is a disc with a diameter of 12.7 mm and a height of 2.5 mm.

[0043] The test conditions of the electrical conductivity in the following examples are: using a high-temperature laser thermal conductivity meter to measure the thermal diffusion coefficient (D) of the composite material at room temperature 25°C, measuring the sample specific heat capacity (Cp) by the comparison method in the laser thermal conductivity meter analysis software, measuring the sample geometric density (ρ) by the Archimedean drainage method, and using the formula k = D·ρ·Cp to calculate the thermal conductivity of the composite material. The conductivity test sample is a disc with a diameter of 12.7 mm and a height of 2.5 mm.

[0044] In the embodiments of the present invention, the preparation method of the high entropy alloy particle reinforced copper-based composite material comprises the following steps:

[0045] Weighing powder: commercial pure copper matrix powder with a particle size of 30-40 μm; FCC structure FeCoCrNi high entropy alloy powder prepared by gas atomization, the atomic proportion of the high entropy alloy powder is: Fe25%, Co25%, Cr25%, Ni25%, the particle size is 45-105 μm, and the content of FeCoCrNi high entropy alloy powder is 5%-20% of the total mass of the composite powder;

[0046] Ball milling powder mixing: FeCoCrNi high entropy alloy powder and pure copper matrix powder are placed in a stainless steel ball mill, stainless steel ball milling balls are added, anhydrous ethanol is added as a process control agent, vacuum is evacuated, Ar is introduced as a protective gas, and a high-energy planetary ball mill is used for ball milling powder mixing; the ball-to-material ratio is set to 5-10:1, argon is filled into the stainless steel ball mill when the vacuum degree is lower than 0.1Pa, the ball mill speed is set to 240-300r / min, and the effective ball milling time is 6-10h;

[0047] Drying of composite powder: After ball milling, the stainless steel ball mill is vacuumed, and the residual composite powder on the wall of the mill is washed with anhydrous ethanol. The stainless steel ball mill is placed in a high-temperature blast drying oven for drying, and the composite powder is obtained by sieving the powder;

[0048] Pre-pressing: Weigh a certain amount of composite powder, put it into a hot isostatic pressing graphite mold with carbon paper around it, and pre-press it with a manual hydraulic press;

[0049] Sintering: After the composite powder is pre-pressed and formed, it is placed in the furnace chamber of the spark plasma sintering system together with the graphite mold. Symmetrical graphite gaskets are placed between the mold and the upper and lower electrodes, and carbon paper is placed between the electrodes and the graphite gaskets. The system is evacuated and the sintering pressure is controlled at 40-60 MPa (in different experiments, the pressure change within this range has basically no effect on the product performance). The sintering temperature is 750℃-950℃, the temperature is increased by 50℃ per minute, the holding time is 6-10min, and the furnace is cooled;

[0050] Demolding: The sintering program is terminated, the composite material is sintered and formed, the current and voltage are turned off, the system is vacuumed, the graphite mold is taken out, and a manual hydraulic press is used for demolding. The carbon paper residue on the surface of the composite material is polished with coarse sandpaper to obtain a high-entropy alloy particle-reinforced copper-based composite material.

[0051] In the above embodiment method, FeCoCrNi high entropy alloy particles with the same single-phase FCC structure as pure copper are selected as the reinforcing phase, and the copper-based composite material is prepared by ball milling combined with spark plasma sintering. By controlling the mass fraction of high entropy alloy particles, the mechanical properties of the composite material are improved, and the electrical and thermal conductivity of the copper matrix is ​​retained to a certain extent. The prepared FeCoCrNi high entropy alloy particle reinforced copper-based composite material has a tensile strength of >150MPa, an elongation at break of >10.5%, and a thermal conductivity of >105W·m -1 ·K -1 , conductivity>11MS / m, density>95%.

[0052] The present invention is further described in detail below in conjunction with specific embodiments:

[0053] Example 1

[0054] Weighing powder: commercial pure copper powder with a particle size of 30 μm; FeCoCrNi high entropy alloy powder with a particle size of 60 μm, and a reinforcing phase mass fraction of 5 wt.%.

[0055] Ball milling mixed powder: FeCoCrNi high entropy alloy powder and pure copper matrix powder are placed in a stainless steel ball mill according to the preset mass fraction, stainless steel ball milling balls (6 mm) are added, the ball-to-material ratio is 5:1, ethanol is added as a process control agent, the vacuum is evacuated to less than 0.1 Pa, Ar is introduced as a protective gas, the ball mill speed is 240 r / min, and the effective ball milling time is 6 h.

[0056] Composite powder drying: After ball milling, the stainless steel ball mill is vacuumed, and the residual composite powder on the wall of the mill is washed with a small amount of alcohol. The stainless steel ball mill is placed in a high-temperature blast drying oven for drying. The drying temperature is set to 50°C and the drying time is 12 hours. The composite powder is obtained by sieving the powder.

[0057] Prepressing: Weigh an appropriate amount of composite powder and put it into a hot isostatic pressing graphite mold padded with carbon paper on all sides. Use a manual hydraulic press to prepress the powder. The prepressing pressure is controlled to be 10 MPa and the prepressing time is 10 min.

[0058] Sintering: Place the graphite mold filled with composite powder in the furnace chamber of the spark plasma sintering system. Symmetrical graphite gaskets are placed between the mold and the upper and lower electrodes, and carbon paper is placed between the electrodes and the graphite gaskets. The system is vacuumed and the sintering program is set according to the preset sintering process. The current and voltage are set, the sintering temperature is 950℃, the sintering pressure is 50MPa, the heating rate is 50℃ / min, the holding time is 10min, and the furnace is cooled.

[0059] Demolding: The sintering program is terminated, the composite material is sintered and formed, the current and voltage are turned off, the system is vacuumed, the graphite mold is taken out, and a manual hydraulic press is used for demolding. The carbon paper residue on the surface of the composite material is polished with coarse sandpaper to obtain a high-entropy alloy particle-reinforced copper-based composite material.

[0060] Morphology and performance analysis: Scanning electron microscope was used to observe the surface morphology of the composite material, Archimedes drainage method was used to measure the density of the composite material and calculate its density, microhardness tester and universal testing machine were used to test the mechanical properties of the composite material, and high temperature laser thermal conductivity meter and Seebeck coefficient measuring instrument were used to measure the thermal conductivity and electrical conductivity of the composite material. The density of the prepared composite material is 98.4%, the tensile strength is 152MPa, the elongation at break is 28%, and the thermal conductivity is 143.15W·m -1 ·K -1 , the conductivity is 13.16MS / m.

[0061] Example 2

[0062] Weighing powder: commercial pure copper powder with a particle size of 30 μm; FeCoCrNi high entropy alloy powder with a particle size of 60 μm and a reinforcing phase mass fraction of 10 wt.%.

[0063] Ball milling mixed powder: FeCoCrNi high entropy alloy powder and pure copper matrix powder are placed in a stainless steel ball mill according to the preset mass fraction, stainless steel ball milling balls (6 mm) are added, the ball-to-material ratio is 5:1, ethanol is added as a process control agent, the vacuum is evacuated to less than 0.1 Pa, Ar is introduced as a protective gas, the ball mill speed is 240 r / min, and the effective ball milling time is 6 h.

[0064] Composite powder drying: After ball milling, the stainless steel ball mill is vacuumed, and the residual composite powder on the wall of the mill is washed with a small amount of alcohol. The stainless steel ball mill is placed in a high-temperature blast drying oven for drying. The drying temperature is set to 50°C and the drying time is 12 hours. The composite powder is obtained by sieving the powder.

[0065] Prepressing: Weigh an appropriate amount of composite powder and put it into a hot isostatic pressing graphite mold padded with carbon paper on all sides. Use a manual hydraulic press to prepress the powder. The prepressing pressure is controlled to be 10 MPa and the prepressing time is 10 min.

[0066] Sintering: Place the graphite mold filled with composite powder in the furnace chamber of the spark plasma sintering system. Symmetrical graphite gaskets are placed between the mold and the upper and lower electrodes, and carbon paper is placed between the electrodes and the graphite gaskets. The system is vacuumed and the sintering program is set according to the preset sintering process. The current and voltage are set, the sintering temperature is 950℃, the sintering pressure is 50MPa, the heating rate is 50℃ / min, the holding time is 10min, and the furnace is cooled.

[0067] Demolding: The sintering program is terminated, the composite material is sintered and formed, the current and voltage are turned off, the system is vacuumed, the graphite mold is taken out, and a manual hydraulic press is used for demolding. The carbon paper residue on the surface of the composite material is polished with coarse sandpaper to obtain a high-entropy alloy particle-reinforced copper-based composite material.

[0068] Morphology and performance analysis: Scanning electron microscope was used to observe the surface morphology of the composite material, Archimedes drainage method was used to measure the density of the composite material and calculate its density, microhardness tester and universal testing machine were used to test the mechanical properties of the composite material, and high temperature laser thermal conductivity meter and Seebeck coefficient measuring instrument were used to measure the thermal conductivity and electrical conductivity of the composite material. The density of the prepared composite material is 99.1%, the tensile strength is 252MPa, the elongation at break is 30%, and the thermal conductivity is 149.19W·m -1 ·K -1 , the conductivity is 23.31MS / m.

[0069] Example 3

[0070] Weighing powder: commercial pure copper powder with a particle size of 30 μm; FeCoCrNi high entropy alloy powder with a particle size of 60 μm and a reinforcing phase mass fraction of 20 wt.%.

[0071] Ball milling mixed powder: FeCoCrNi high entropy alloy powder and pure copper matrix powder are placed in a stainless steel ball mill according to the preset mass fraction, stainless steel ball milling balls (6 mm) are added, the ball-to-material ratio is 5:1, ethanol is added as a process control agent, the vacuum is evacuated to less than 0.1 Pa, Ar is introduced as a protective gas, the ball mill speed is 240 r / min, and the effective ball milling time is 6 h.

[0072] Composite powder drying: After ball milling, the stainless steel ball mill is vacuumed, and the residual composite powder on the wall of the mill is washed with a small amount of alcohol. The stainless steel ball mill is placed in a high-temperature blast drying oven for drying. The drying temperature is set to 50°C and the drying time is 12 hours. The composite powder is obtained by sieving the powder.

[0073] Prepressing: Weigh an appropriate amount of composite powder and put it into a hot isostatic pressing graphite mold padded with carbon paper on all sides. Use a manual hydraulic press to prepress the powder. The prepressing pressure is controlled to be 10 MPa and the prepressing time is 10 min.

[0074] Sintering: Place the graphite mold filled with composite powder in the furnace chamber of the spark plasma sintering system. Symmetrical graphite gaskets are placed between the mold and the upper and lower electrodes, and carbon paper is placed between the electrodes and the graphite gaskets. The system is vacuumed and the sintering program is set according to the preset sintering process. The current and voltage are set, the sintering temperature is 950℃, the sintering pressure is 50MPa, the heating rate is 50℃ / min, the holding time is 10min, and the furnace is cooled.

[0075] Demolding: The sintering program is terminated, the composite material is sintered and formed, the current and voltage are turned off, the system is vacuumed, the graphite mold is taken out, and a manual hydraulic press is used for demolding. The carbon paper residue on the surface of the composite material is polished with coarse sandpaper to obtain a high-entropy alloy particle-reinforced copper-based composite material.

[0076] Morphology and performance analysis: Scanning electron microscope was used to observe the surface morphology of the composite material, Archimedes drainage method was used to measure the density of the composite material and calculate its density, microhardness tester and universal testing machine were used to test the mechanical properties of the composite material, and high temperature laser thermal conductivity meter and Seebeck coefficient measuring instrument were used to measure the thermal conductivity and electrical conductivity of the composite material. The density of the prepared composite material is 98.6%, the tensile strength is 276MPa, the elongation at break is 11%, and the thermal conductivity is 110.33W·m -1 ·K -1 , the conductivity is 13.58MS / m.

[0077] Example 4

[0078] Weighing powder: commercial pure copper powder with a particle size of 30 μm; FeCoCrNi high entropy alloy powder with a particle size of 140 μm and a reinforcing phase mass fraction of 10 wt.%.

[0079] Ball milling mixed powder: FeCoCrNi high entropy alloy powder and pure copper matrix powder are placed in a stainless steel ball mill according to the preset mass fraction, stainless steel ball milling balls (6 mm) are added, the ball-to-material ratio is 5:1, ethanol is added as a process control agent, the vacuum is evacuated to less than 0.1 Pa, Ar is introduced as a protective gas, the ball mill speed is 240 r / min, and the effective ball milling time is 6 h.

[0080] Composite powder drying: After ball milling, the stainless steel ball mill is vacuumed, and the residual composite powder on the wall of the mill is washed with a small amount of alcohol. The stainless steel ball mill is placed in a high-temperature blast drying oven for drying. The drying temperature is set to 50°C and the drying time is 12 hours. The composite powder is obtained by sieving the powder.

[0081] Prepressing: Weigh an appropriate amount of composite powder and put it into a hot isostatic pressing graphite mold padded with carbon paper on all sides. Use a manual hydraulic press to prepress the powder. The prepressing pressure is controlled to be 10 MPa and the prepressing time is 10 min.

[0082] Sintering: Place the graphite mold filled with composite powder in the furnace chamber of the spark plasma sintering system. Symmetrical graphite gaskets are placed between the mold and the upper and lower electrodes, and carbon paper is placed between the electrodes and the graphite gaskets. The system is vacuumed and the sintering program is set according to the preset sintering process. The current and voltage are set, the sintering temperature is 950℃, the sintering pressure is 50MPa, the heating rate is 50℃ / min, the holding time is 10min, and the furnace is cooled.

[0083] Demolding: The sintering program is terminated, the composite material is sintered and formed, the current and voltage are turned off, the system is vacuumed, the graphite mold is taken out, and a manual hydraulic press is used for demolding. The carbon paper residue on the surface of the composite material is polished with coarse sandpaper to obtain a high-entropy alloy particle-reinforced copper-based composite material.

[0084] Morphology and performance analysis: The density of the composite material measured by the Archimedes drainage method and its density was 96.33%. The density of the composite material in Example 4 was much lower than that in Example 2. The decrease in density was related to the selection of high-entropy alloy particles with larger particle size. High-entropy alloy particles with larger particle size occupied more volume in the composite material, and the gaps between the particles would also increase accordingly. During the sintering process, these gaps were difficult to completely eliminate, resulting in a decrease in the density of the material.

[0085] Example 5

[0086] Weighing powder: commercial pure copper powder with a particle size of 30 μm; FeCoCrNi high entropy alloy powder with a particle size of 60 μm and a reinforcing phase mass fraction of 10 wt.%.

[0087] Ball milling mixed powder: FeCoCrNi high entropy alloy powder and pure copper matrix powder are placed in a stainless steel ball mill according to the preset mass fraction, stainless steel ball milling balls (6 mm) are added, the ball-to-material ratio is 5:1, ethanol is added as a process control agent, the vacuum is evacuated to less than 0.1 Pa, Ar is introduced as a protective gas, the ball mill speed is 240 r / min, and the effective ball milling time is 6 h.

[0088] Composite powder drying: After ball milling, the stainless steel ball mill is vacuumed, and the residual composite powder on the wall of the mill is washed with a small amount of alcohol. The stainless steel ball mill is placed in a high-temperature blast drying oven for drying. The drying temperature is set to 50°C and the drying time is 12 hours. The composite powder is obtained by sieving the powder.

[0089] Prepressing: Weigh an appropriate amount of composite powder and put it into a hot isostatic pressing graphite mold padded with carbon paper on all sides. Use a manual hydraulic press to prepress the powder. The prepressing pressure is controlled to be 10 MPa and the prepressing time is 10 min.

[0090] Sintering: Place the graphite mold filled with composite powder in the furnace chamber of the spark plasma sintering system. Symmetrical graphite gaskets are placed between the mold and the upper and lower electrodes, and carbon paper is placed between the electrodes and the graphite gaskets. The system is vacuumed and the sintering program is set according to the preset sintering process. The current and voltage are set, the sintering temperature is 750℃, the sintering pressure is 50MPa, the heating rate is 50℃ / min, the holding time is 10min, and the furnace is cooled.

[0091] Demolding: The sintering program is terminated, the composite material is sintered and formed, the current and voltage are turned off, the system is vacuumed, the graphite mold is taken out, and a manual hydraulic press is used for demolding. The carbon paper residue on the surface of the composite material is polished with coarse sandpaper to obtain a high-entropy alloy particle-reinforced copper-based composite material.

[0092] Morphology and performance analysis: Archimedes drainage method was used to measure the density of the composite material and calculate its density. A universal testing machine was used to test the mechanical properties of the composite material. A high-temperature laser thermal conductivity meter and Seebeck coefficient measuring instrument were used to measure the thermal and electrical conductivity of the composite material. The density of the prepared composite material was 95.20%, the tensile strength was 238MPa, the elongation at break was 10.6%, and the thermal conductivity was 106.20W·m -1 ·K -1 , the conductivity is 11.58MS / m.

[0093] Example 6

[0094] Weighing powder: commercial pure copper powder with a particle size of 30 μm; FeCoCrNi high entropy alloy powder with a particle size of 60 μm and a reinforcing phase mass fraction of 40 wt.%.

[0095] Ball milling mixed powder: FeCoCrNi high entropy alloy powder and pure copper matrix powder are placed in a stainless steel ball mill according to the preset mass fraction, stainless steel ball milling balls (6 mm) are added, the ball-to-material ratio is 5:1, ethanol is added as a process control agent, the vacuum is evacuated to less than 0.1 Pa, Ar is introduced as a protective gas, the ball mill speed is 240 r / min, and the effective ball milling time is 6 h.

[0096] Composite powder drying: After ball milling, the stainless steel ball mill is vacuumed, and the residual composite powder on the wall of the mill is washed with a small amount of alcohol. The stainless steel ball mill is placed in a high-temperature blast drying oven for drying. The drying temperature is set to 50°C and the drying time is 12 hours. The composite powder is obtained by sieving the powder.

[0097] Prepressing: Weigh an appropriate amount of composite powder and put it into a hot isostatic pressing graphite mold padded with carbon paper on all sides. Use a manual hydraulic press to prepress the powder. The prepressing pressure is controlled to be 10 MPa and the prepressing time is 10 min.

[0098] Sintering: Place the graphite mold filled with composite powder in the furnace chamber of the spark plasma sintering system. Symmetrical graphite gaskets are placed between the mold and the upper and lower electrodes, and carbon paper is placed between the electrodes and the graphite gaskets. The system is vacuumed and the sintering program is set according to the preset sintering process. The current and voltage are set, the sintering temperature is 950℃, the sintering pressure is 50MPa, the heating rate is 50℃ / min, the holding time is 10min, and the furnace is cooled.

[0099] Demolding: The sintering program is terminated, the composite material is sintered and formed, the current and voltage are turned off, the system is vacuumed, the graphite mold is taken out, and a manual hydraulic press is used for demolding. The carbon paper residue on the surface of the composite material is polished with coarse sandpaper to obtain a high-entropy alloy particle-reinforced copper-based composite material.

[0100] Morphology and performance analysis: When the mass fraction of high entropy alloy particles reaches 40%, the local agglomeration of the reinforcement phase particles becomes more serious, and the inhomogeneity increases, resulting in local stress concentration in the composite material. The mechanical properties of the composite material decrease, with a tensile strength of 196MPa and an elongation at break of 7.8%.

[0101] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.

[0102] The above is only a preferred specific implementation of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field within the technical scope disclosed by the present invention, according to the technical solution and its concept of the present invention, shall be covered within the protection scope of the present invention. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

Claims

1. A method for preparing a high entropy alloy particle reinforced copper-based composite material, It is characterized in that The steps include: Weighing powder: pure copper matrix powder with a particle size of 30-40 μm; FCC structure FeCoCrNi high entropy alloy powder prepared by gas atomization, the atomic proportion of the high entropy alloy powder is: Fe25%, Co25%, Cr25%, Ni25%, the particle size is 45-105 μm, and the content of FeCoCrNi high entropy alloy powder is 5%-20% of the total mass of the composite powder; Ball milling powder mixing: FeCoCrNi high entropy alloy powder and pure copper matrix powder are placed in a stainless steel ball mill, stainless steel ball milling balls are added, anhydrous ethanol is added as a process control agent, vacuum is evacuated, Ar is introduced as a protective gas, and a high-energy planetary ball mill is used for ball milling powder mixing; the ball-to-material ratio is set to 5-10:1, argon is filled into the stainless steel ball mill when the vacuum degree is lower than 0.1Pa, the ball mill speed is set to 240-300r / min, and the effective ball milling time is 6-10h; Drying of composite powder: After ball milling, the stainless steel ball mill is vacuumed, and the residual composite powder on the wall of the mill is washed with anhydrous ethanol. The stainless steel ball mill is placed in a high-temperature blast drying oven for drying, and the composite powder is obtained by sieving the powder; Pre-pressing: Weigh a certain amount of composite powder, put it into a hot isostatic pressing graphite mold with carbon paper around it, and pre-press it with a manual hydraulic press; Sintering: After the composite powder is pre-pressed and formed, it is placed in the furnace chamber of the spark plasma sintering system together with the graphite mold. Symmetrical graphite gaskets are placed between the mold and the upper and lower electrodes, and carbon paper is placed between the electrodes and the graphite gaskets. The system is evacuated, the sintering pressure is controlled at 40-60MPa, the sintering temperature is 750℃-950℃, the temperature is increased by 50℃ per minute, the holding time is 6-10min, and the furnace is cooled; Demolding: The sintering program is terminated, the composite material is sintered and formed, the current and voltage are turned off, the system is vacuumed, the graphite mold is taken out, and a manual hydraulic press is used for demolding. The carbon paper residue on the surface of the composite material is polished with coarse sandpaper to obtain a high-entropy alloy particle-reinforced copper-based composite material.

2. The method for preparing the high entropy alloy particle reinforced copper-based composite material according to claim 1, Features: The FeCoCrNi high entropy alloy powder accounts for 5% to 10% of the total mass of the composite powder, and the sintering temperature is 950°C.

3. The method for preparing the high entropy alloy particle reinforced copper-based composite material according to claim 1, Features: The FeCoCrNi high entropy alloy powder accounts for 10% of the total mass of the composite powder, and the sintering temperature is 950°C.

4. The method for preparing the high entropy alloy particle reinforced copper-based composite material according to claim 1, Features: After ball milling, the composite powder is placed in a high-temperature forced air drying oven with a set temperature of 50° C. The drying process lasts for 8 to 12 hours.

5. The preparation method according to claim 1, Features: The powder pre-pressing pressure ranges from 5 to 10 Pa, and the holding time is 10 to 15 minutes.

6. A high entropy alloy particle reinforced copper-based composite material, Features: Prepared according to the method according to any one of claims 1 to 5, in the composite material, high entropy alloy particles are dispersedly distributed and have a particle size of 45 to 105 μm.

7. The high entropy alloy particle reinforced copper-based composite material according to claim 6, Features: The composite material has a tensile strength of >150 MPa, a breaking elongation of >10.5%, and a thermal conductivity of >105 W·m -1 ·K -1 , conductivity>11MS / m, density>95%.

8. The high entropy alloy particle reinforced copper-based composite material according to claim 6, Features: The composite material has a tensile strength of >150 MPa, a breaking elongation of >11%, and a thermal conductivity of >110 W·m -1 ·K -1 , conductivity>13MS / m, density>98%.

Citation Information

Cited By

  • High-entropy alloy particle reinforced copper-based contact material and preparation method and application thereof

    CN119685645A

  • High-entropy alloy particle reinforced copper-based contact material, preparation method and application thereof

    CN119685645B

  • High-entropy particle reinforced heat-resistant copper alloy and preparation method and application thereof

    CN120738514A

  • WMoTaNb-Cu composite material and preparation method thereof

    CN121065562A