Aluminum alloy and surface treatment method thereof
Through decomposition removal treatment, two anodization and trivalent chromium salt conversion film treatment, combined with natural aging treatment, a hydrophilic corrosion-resistant conductive film layer is formed, which solves the problem of improving corrosion resistance, conductivity and wetting performance of the high-strength aluminum alloy surface. Problem, suitable for industrial applications.
Patent Information
- Application Number
- CN202411122640.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
AI Technical Summary
High-strength aluminum alloys require surface treatment before application to improve corrosion resistance and meet the needs of conductivity and wetting properties. The prior art is difficult to meet these performance requirements at the same time.
Decompression treatment, two anodization treatments and trivalent chromium salt conversion film treatment are used, combined with natural aging treatment, to form a hydrophilic corrosion-resistant conductive film layer.
It significantly improves the corrosion resistance of the anodized film of aluminum alloy, while maintaining good conductivity and wetting properties, meets the application needs of high-strength aluminum alloys in special fields, and is suitable for large-scale industrial production.
Smart Images

Figure CN118996568A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to aluminum alloy surface treatment technology, and in particular to an aluminum alloy and a surface treatment method thereof. Background Art
[0002] Aluminum alloys for aerospace such as 2024 and 7075 are widely used due to their advantages of high strength, low density and good rigidity. However, a large amount of alloying elements including copper are usually added to these high-strength aluminum alloys, which significantly reduces their corrosion resistance. Therefore, high-strength aluminum alloys must be surface treated before application to improve their resistance to atmospheric corrosion and seawater corrosion. On the other hand, when high-strength aluminum alloys are used in satellite antennas, solar panels, electronic casings and other fields, in addition to good corrosion resistance, the alloy surface is also required to have good conductivity and surface wettability to meet the special requirements of electromagnetic shielding and bonding strength.
[0003] Anodizing is the most mature and effective surface treatment method for improving the corrosion resistance of aluminum alloys in the industry. In general, the aluminum alloy anodized film has a double-layer structure, namely a thick and loose porous layer and a thin and dense barrier layer. The porous anodized film that has not been sealed has good electrical conductivity when its thickness is small (several hundred nanometers to several microns), and its porous characteristics can also give the alloy surface good bonding properties. However, there are void defects related to the selective oxidation of the second phase particles in the porous layer of the porous anodized film; when these void defects appear at the interface between the oxide film and the alloy, it will also lead to the loss of the barrier layer or the increase of defects. Therefore, the corrosion resistance of the porous anodized film that has not been sealed is very poor. Common oxide film post-treatment technologies, such as boiling water sealing, nickel salt sealing, chromate sealing, etc., can significantly improve the corrosion resistance of the oxide film, but the conductivity and surface wettability of the alloy surface will be significantly reduced after sealing, and it cannot meet the requirements of electromagnetic shielding and bonding strength. Therefore, it has become an urgent need in the industry to develop an aluminum alloy surface film technology that can simultaneously meet the requirements of conductivity, corrosion resistance and good wettability. Summary of the invention
[0004] The purpose of the present invention is to provide an aluminum alloy and a surface treatment method thereof, which can form a hydrophilic corrosion-resistant conductive film layer on the surface of the aluminum alloy and simultaneously meet the performance requirements of good conductivity, corrosion resistance and wetting of the surface of the high-strength aluminum alloy.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0006] In a first aspect, the present invention provides a method for surface treatment of an aluminum alloy, comprising the following steps:
[0007] S1, pretreatment: removing impurities from the aluminum alloy surface;
[0008] S2, first anodizing treatment: placing the pretreated aluminum alloy in an acidic aqueous solution, and performing a first constant potential anodizing treatment at a preset voltage to form an oxide film on the surface of the aluminum alloy and remove the second phase particles on the surface of the aluminum alloy;
[0009] S3, stripping treatment: immersing the aluminum alloy obtained in S2 in a stripping solution to dissolve the oxide film on the surface of the aluminum alloy;
[0010] S4, a second anodizing treatment: placing the aluminum alloy after the film stripping treatment in an acidic aqueous solution, and performing a second constant potential anodizing at a preset voltage to form a porous anodized film on the surface of the aluminum alloy;
[0011] S5, trivalent chromium salt conversion film treatment: the aluminum alloy obtained in S4 is placed in a trivalent chromium salt solution, the trivalent chromium ions in the salt solution are adsorbed by the porous anodic oxide film, and a coordination polymerization reaction is carried out with the hydroxyl groups in the oxide film, so as to form a conversion film precursor on the pore wall of the porous oxide film and on the barrier layer where the porous oxide film contacts the surface of the aluminum alloy;
[0012] S6, natural aging treatment: natural aging is carried out at room temperature to cause the conversion film precursor to undergo a dehydration reaction, generate a dense and continuous conversion film, repair the microscopic defects on the pore wall and barrier layer of the porous anodized film, and form a hydrophilic, corrosion-resistant and conductive film layer on the surface of the aluminum alloy.
[0013] Furthermore, the impurity removal treatment in S1 includes sequentially subjecting the aluminum alloy to alkaline etching, pickling and rinsing.
[0014] Further, the acidic aqueous solution in S2 and S4 includes at least one of sulfuric acid, tartaric acid, phosphoric acid and oxalic acid.
[0015] Furthermore, the preset voltage of the first anodizing treatment in S2 is 0-3V, the reference electrode is a saturated calomel electrode, the first constant potential anodizing temperature is 20-40°C, and the first constant potential anodizing time is 3-10min.
[0016] Furthermore, the preset voltage of the second anodizing treatment in S4 is 10-40V, the reference electrode is a saturated calomel electrode, the second constant potential anodizing temperature is 20-40°C, and the second constant potential anodizing time is 15-30min.
[0017] Furthermore, the stripping solution in S3 includes a mixed aqueous solution of chromic anhydride and phosphoric acid, the stripping treatment temperature is 50-60° C., and the stripping treatment time is 30-60 min.
[0018] Furthermore, the trivalent chromium salt in S5 includes at least one of chromium sulfate, chromium chloride, and basic chromium sulfate; the concentration of the trivalent chromium salt solution is 0.0001-0.01 mol / L, and the pH of the trivalent chromium salt solution is 3-5; the trivalent chromium salt conversion film treatment temperature is 20-60°C, and the trivalent chromium salt conversion film treatment time is 5-30 min.
[0019] Furthermore, after the trivalent chromium salt conversion film treatment of S5 is completed, the aluminum alloy is rinsed in deionized water at room temperature for 1 to 2 minutes, naturally air-dried, and then subjected to the natural aging treatment of S6.
[0020] Furthermore, the natural aging treatment time in S6 is not less than 48 hours.
[0021] In a second aspect, the present invention provides an aluminum alloy obtained by the above-mentioned aluminum alloy surface treatment method, wherein a hydrophilic, corrosion-resistant, conductive film layer is formed on the surface of the aluminum alloy.
[0022] Beneficial effects of the present invention:
[0023] The present invention first removes impurities and second-phase particles on the surface of the aluminum alloy through impurity removal treatment, first anodizing treatment and stripping treatment, thereby ensuring the purity of the aluminum alloy surface, maximally eliminating the number of second-phase particles on the alloy surface, and ensuring the effective formation of the subsequent hydrophilic corrosion-resistant conductive film layer. Through the second anodizing treatment, trivalent chromium salt conversion film treatment and natural aging treatment, a hydrophilic corrosion-resistant conductive film layer is formed on the surface of the aluminum alloy, which can significantly improve the corrosion resistance of the aluminum alloy anodized film, while allowing the alloy surface to still maintain good conductivity and wettability, meeting the complex performance requirements of the surface film layer for high-strength aluminum alloys in special fields. In addition, the surface treatment method of the present invention can be carried out on a conventional aluminum alloy surface treatment production line without the need for special hardware equipment investment, reducing the production line transformation cost, and is suitable for large-scale industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 A schematic flow chart of the aluminum alloy surface treatment method of the present invention is shown.
[0025] Figure 2 A comparison chart of the copper sulfate dripping results of 2024-T351 aluminum alloy after being treated by Example 1 of the present invention and the copper sulfate dripping results after being treated by Comparative Examples 1 and 2 is shown.
[0026] Figure 3 A comparison chart of the copper sulfate dripping results of 7075-T6 aluminum alloy after being treated by Example 2 of the present invention and the copper sulfate dripping results after being treated by Comparative Example 3 is shown.
[0027] Figure 4The SEM photograph of the sample surface of 2024-T351 aluminum alloy after being treated by Example 1 of the present invention is shown.
[0028] Figure 5 The SEM photograph of the sample surface of 7075-T6 aluminum alloy after being treated by Example 2 of the present invention is shown.
[0029] Figure 6 The contact angle test result diagram of 2024-T351 aluminum alloy after being treated by Example 1 of the present invention is shown.
[0030] Figure 7 The contact angle test result diagram of 7075-T6 aluminum alloy after being treated by Example 2 of the present invention is shown. DETAILED DESCRIPTION
[0031] The following will describe the embodiments of the present invention with reference to the accompanying drawings and preferred embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be understood that the preferred embodiments are only for illustrating the present invention, not for limiting the scope of protection of the present invention.
[0032] It should be noted that the illustrations provided in the following embodiments are only schematic illustrations of the basic concept of the present invention, and thus the drawings only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.
[0033] In one embodiment, see Figure 1 As shown, the present invention provides a method for surface treatment of aluminum alloy, which comprises the following steps:
[0034] S1, pretreatment: removing impurities from the aluminum alloy surface;
[0035] S2, first anodizing treatment: placing the pretreated aluminum alloy in an acidic aqueous solution, and performing a first constant potential anodizing treatment at a preset voltage to form an oxide film on the surface of the aluminum alloy and remove the second phase particles on the surface of the aluminum alloy;
[0036] S3, stripping treatment: immersing the aluminum alloy obtained in S2 in a stripping solution to dissolve the oxide film on the surface of the aluminum alloy;
[0037] S4, a second anodizing treatment: placing the aluminum alloy after the film stripping treatment in an acidic aqueous solution, and performing a second constant potential anodizing at a preset voltage to form a porous anodized film on the surface of the aluminum alloy;
[0038] S5, trivalent chromium salt conversion film treatment: the aluminum alloy obtained in S4 is placed in a trivalent chromium salt solution, the trivalent chromium ions in the salt solution are adsorbed by the porous anodic oxide film, and a coordination polymerization reaction is carried out with the hydroxyl groups in the oxide film, so as to form a conversion film precursor on the pore wall of the porous oxide film and on the barrier layer where the porous oxide film contacts the surface of the aluminum alloy;
[0039] S6, natural aging treatment: natural aging is carried out at room temperature to cause the conversion film precursor to undergo a dehydration reaction, generate a dense and continuous conversion film, repair the microscopic defects on the pore wall and barrier layer of the porous anodized film, and form a hydrophilic, corrosion-resistant and conductive film layer on the surface of the aluminum alloy.
[0040] The present invention first removes impurities and second-phase particles on the surface of the aluminum alloy through impurity removal treatment, first anodizing treatment and stripping treatment, thereby ensuring the purity of the aluminum alloy surface, maximally eliminating the number of second-phase particles on the alloy surface, and ensuring the effective formation of the subsequent hydrophilic corrosion-resistant conductive film layer. Through the second anodizing treatment, trivalent chromium salt conversion film treatment and natural aging treatment, a hydrophilic corrosion-resistant conductive film layer is formed on the surface of the aluminum alloy, which can significantly improve the corrosion resistance of the aluminum alloy anodized film, while allowing the alloy surface to still maintain good conductivity and wettability, meeting the complex performance requirements of the surface film layer for high-strength aluminum alloys in special fields. In addition, the surface treatment method of the present invention can be carried out on a conventional aluminum alloy surface treatment production line without the need for special hardware equipment investment, reducing the production line transformation cost, and is suitable for large-scale industrial applications.
[0041] In a preferred embodiment, the impurity removal treatment in S1 includes sequentially alkali etching, pickling and rinsing the aluminum alloy. This ensures that the surface of the aluminum alloy is clean, uniform and free of impurities, providing ideal substrate conditions for subsequent anodizing treatment. This will help improve the quality, uniformity and corrosion resistance of the anodized film, thereby further improving the overall performance and service life of the aluminum alloy product.
[0042] Alkali etching is mainly used to remove oil stains, natural oxide layers and some intermetallic compounds on the surface of aluminum alloys. Alkaline solutions can react chemically with these impurities to dissolve or peel them off, thereby exposing a relatively pure aluminum alloy matrix. Alkaline etching method: immerse the aluminum alloy in an alkaline solution of a certain concentration, control the appropriate temperature and time, so that impurities can be effectively removed. Subsequently, rinse off the remaining alkali solution and impurities with clean water.
[0043] The main purpose of pickling is to further remove the oxides, intermetallic compound residues and ash that may be produced during the alkaline etching process on the surface of the aluminum alloy. The acid solution can dissolve these substances, making the surface of the aluminum alloy cleaner and more uniform. Pickling method: immerse the aluminum alloy that has been alkaline etched and preliminarily cleaned in an acid solution (such as dilute sulfuric acid, concentrated nitric acid, etc.), control the appropriate concentration, temperature and time to ensure that impurities are effectively removed. After that, rinse with clean water again to remove the residual acid and impurities.
[0044] Rinsing is to thoroughly remove the residual acid and alkali solution, impurities and other pollutants that may be generated during the cleaning process on the surface of the aluminum alloy, to ensure that the surface of the aluminum alloy is clean and free of dirt, and to provide the best conditions for subsequent anodizing treatment. Rinsing method: Use clean water or deionized water to rinse the aluminum alloy several times until there is no residue on the surface. During the rinsing process, attention should be paid to controlling the water temperature and water flow rate to avoid unnecessary damage to the surface of the aluminum alloy.
[0045] In a preferred embodiment, the acidic aqueous solution in S2 and S4 includes at least one of sulfuric acid, tartaric acid, phosphoric acid and oxalic acid.
[0046] In steps S2 and S4, a suitable acidic aqueous solution formula can be selected according to specific needs and the material characteristics of the aluminum alloy. For example, sulfuric acid, tartaric acid, phosphoric acid or oxalic acid can be used alone, or they can be mixed in a certain proportion to obtain the best anodizing effect. Mixing different types of acids can make comprehensive use of their respective advantages to form an oxide film with better performance.
[0047] By selecting at least one of sulfuric acid, phosphoric acid and oxalic acid as the main component of the acidic aqueous solution, fine control and optimization of the anodizing treatment of the aluminum alloy surface can be achieved, thereby obtaining an oxide film layer with excellent performance.
[0048] In a preferred embodiment, the preset voltage of the first anodizing treatment in S2 is 0-3V, the reference electrode is a saturated calomel electrode, the first constant potential anodizing temperature is 20-40°C, and the first constant potential anodizing time is 3-10min.
[0049] The preset voltage is set to 0-3V, which is relative to the saturated calomel electrode (SCE). The selection of this voltage range is based on a deep understanding of the material properties of aluminum alloys and the kinetics of anodizing reactions. The second-phase particles commonly found in high-strength aluminum alloys usually undergo selective oxidation within this voltage range. Within this voltage range, anodizing can preferentially transform the second-phase particles near the surface of the alloy into loose and porous oxides, which are then dissolved in the subsequent stripping process, thereby further eliminating the second-phase particles on the alloy surface, reducing the oxide film defects associated with the second-phase particles during the second anodizing, and thus improving the corrosion resistance of the oxide film.
[0050] The reference electrode is saturated calomel electrode (SCE). Saturated calomel electrode is a commonly used electrochemical reference electrode with stable potential and good reproducibility. In the anodization process, the use of saturated calomel electrode as a reference electrode can ensure accurate measurement and control of voltage, thereby ensuring the quality consistency of the oxide film.
[0051] The first constant potential anodizing temperature should be controlled within a certain range, and the specific value should be consistent with the second anodizing temperature, so that the two anodizing processes can be carried out on the same production line.
[0052] The time of the first constant potential anodization is set to 3 to 10 minutes. The selection of this time range depends on the type of aluminum alloy and the second phase particles on its surface. A shorter time may not completely oxidize all coarse second phase particles, while a longer time may result in an overly thick film layer, increased energy consumption, and decreased efficiency. Therefore, in actual operation, it needs to be adjusted according to specific circumstances.
[0053] In summary, by setting a reasonable preset voltage, using a stable reference electrode, and controlling the appropriate oxidation temperature and time, it can be ensured that the first anodizing treatment in S2 can quickly and effectively selectively oxidize the coarse second phase particles, and then provide a pure aluminum alloy solid solution substrate for the second anodizing through stripping treatment.
[0054] In a preferred embodiment, the preset voltage of the second anodizing treatment in S4 is 10-40V, the reference electrode is a saturated calomel electrode, the second constant potential anodizing temperature is 20-40°C, and the second constant potential anodizing time is 15-30min.
[0055] By setting a reasonable preset voltage, using a stable reference electrode, and controlling the appropriate oxidation temperature and time, it is ensured that the second anodizing treatment in S4 can obtain a porous anodized film of a preset thickness.
[0056] In a preferred embodiment, the stripping solution in S3 includes a mixed aqueous solution of chromic anhydride and phosphoric acid, the stripping treatment temperature is 50-60° C., and the stripping treatment time is 30-60 min.
[0057] The stripping solution is a mixed aqueous solution of chromic anhydride (CrO3) and phosphoric acid (H3PO4). This combination has an excellent stripping effect and can effectively dissolve and remove the oxide film on the surface of the aluminum alloy without causing corrosion damage to the aluminum alloy substrate. Chromic anhydride, as a strong oxidant, can accelerate the decomposition of the oxide film; while phosphoric acid helps to adjust the acidity and stability of the solution to ensure the smooth progress of the stripping process.
[0058] The stripping treatment temperature is set at 50-60°C. The selection of this temperature range is based on the consideration of the reactivity of the stripping solution. Higher temperatures can accelerate the chemical reaction between the stripping solution and the oxide film and improve the stripping efficiency; however, too high a temperature may also cause the stripping solution to excessively corrode the aluminum alloy substrate, affecting the effect of the subsequent second anodizing treatment. Therefore, stripping treatment within this temperature range can ensure that the oxide film is effectively removed while avoiding damage to the aluminum alloy substrate.
[0059] The stripping treatment time is set to 30 to 60 minutes. The selection of this time range depends on factors such as the thickness and uniformity of the oxide film, as well as the concentration and temperature of the stripping solution. A longer treatment time can ensure that the oxide film is fully removed, but too long a time may also cause excessive erosion of the aluminum alloy substrate by the stripping solution. Therefore, in actual operation, it is necessary to adjust according to the specific situation to find the best stripping treatment time.
[0060] In summary, by using a mixed aqueous solution of chromic anhydride and phosphoric acid as the stripping solution and performing the stripping treatment under appropriate temperature and time conditions, the oxide film layer formed during the first anodizing process can be effectively removed, providing a clean and uniform substrate for the subsequent second anodizing treatment.
[0061] In a preferred embodiment, the trivalent chromium salt in S5 includes at least one of chromium sulfate, chromium chloride, and basic chromium sulfate; the concentration of the trivalent chromium salt solution is 0.0001-0.01 mol / L, and the pH of the trivalent chromium salt solution is 3-5; the trivalent chromium salt conversion film treatment temperature is 20-60°C, and the trivalent chromium salt conversion film treatment time is 5-30 min.
[0062] Selection of trivalent chromium salts: Trivalent chromium salts include at least one of chromium sulfate (such as Cr2(SO4)3), chromium chloride (such as CrCl3), and basic chromium sulfate (such as Cr(OH)SO4). These trivalent chromium salts can react with hydroxide ions or other anions in water under appropriate conditions to form a dense conversion film with good corrosion resistance on the surface of aluminum alloy.
[0063] The concentration of the trivalent chromium salt solution is set at 0.0001-0.01 mol / L. This concentration range is selected to ensure that during the conversion film treatment process, the trivalent chromium ions can fully react with the aluminum alloy surface to form a uniform and dense conversion film. Too low a concentration may lead to incomplete formation of the conversion film, while too high a concentration may cause other impurities in the solution to have an adverse effect on the quality of the conversion film.
[0064] The pH of the trivalent chromium salt solution is set to 3-5. The selection of this pH range is based on the consideration of the formation mechanism of the conversion film. Under acidic conditions, trivalent chromium ions are more likely to combine with hydroxide ions or other anions on the surface of the aluminum alloy to form a stable compound and deposit on the surface to form a conversion film. At the same time, a suitable acidic environment also helps to remove oxides and other impurities on the surface of the aluminum alloy and improve the bonding strength between the conversion film and the substrate.
[0065] The treatment temperature of trivalent chromium salt conversion film is set at 20-60℃. This temperature range is selected to accelerate the formation process of the conversion film while avoiding damage to the aluminum alloy substrate caused by excessively high temperatures. Appropriate temperature can increase the diffusion rate and reaction activity of ions in the solution, thereby accelerating the formation rate of the conversion film. However, excessively high temperature will cause the formation rate of the conversion film to be lower than the dissolution rate of the oxide film, which will not only fail to improve the corrosion resistance of the oxide film, but may also reduce its corrosion resistance.
[0066] The treatment time of trivalent chromium salt conversion film is 5 to 30 minutes. The selection of this time range depends on factors such as the type, concentration, pH value and treatment temperature of the trivalent chromium salt. A longer treatment time can ensure that the conversion film is formed more completely and densely, but too long a time may also cause the conversion film to be too thick, cracked or have other adverse effects. Therefore, in actual operation, it is necessary to adjust according to the specific situation to find the best treatment time.
[0067] In a preferred embodiment, after the trivalent chromium salt conversion film treatment in S5 is completed, the aluminum alloy is rinsed in deionized water at room temperature for 1 to 2 minutes, naturally air-dried, and then subjected to natural aging treatment in S6. The excess trivalent chromium salt solution, unreacted ions, and possible impurity precipitation attached to the surface of the aluminum alloy are removed by rinsing.
[0068] Rinse time: Rinse the aluminum alloy in deionized water at room temperature for 1 to 2 minutes. This time range is selected to ensure that surface residues are fully rinsed away, while avoiding unnecessary scouring or damage to the conversion film due to excessive rinsing time. Rinse conditions: Rinsing should be carried out at room temperature, using high-quality deionized water to ensure that no additional ions or impurities are introduced into the system, thereby affecting the performance of the conversion film.
[0069] After rinsing, remove the aluminum alloy from the deionized water and allow it to air dry in a natural environment. Avoid using any external heat source or forced ventilation during this process to prevent thermal shock or mechanical damage to the conversion film. Note: During the air drying process, ensure that the aluminum alloy surface is free from contamination such as dust, grease, etc. At the same time, avoid exposing the aluminum alloy to an environment that is too humid or with rapid temperature changes, so as not to affect the drying effect and final performance of the conversion film.
[0070] In a preferred embodiment, the natural aging treatment time in S6 is not less than 48 hours.
[0071] Natural aging treatment is a process that allows materials to be placed in the natural environment for a period of time to gradually stabilize their internal structure and performance. For aluminum alloys treated with trivalent chromium salt conversion coating, natural aging treatment helps:
[0072] Eliminate internal stress: During the formation of the conversion film, a certain amount of internal stress may be generated on the surface of the aluminum alloy. Natural aging treatment can gradually release this internal stress and reduce the risk of cracking or shedding of the film due to stress concentration.
[0073] Promote chemical reactions: The chemical components in the conversion film may continue to undergo minor chemical reactions in the natural environment, such as further hydrolysis, cross-linking, etc. These reactions help to enhance the density and stability of the conversion film.
[0074] Improved microstructure: Over time, the microstructure in the conversion coating may gradually optimize, forming a more uniform and dense protective layer. This structural improvement helps improve the corrosion resistance and durability of the conversion coating.
[0075] Setting the natural aging treatment time to no less than 48 hours is based on experience gained from experiments and practical applications. This length of time is sufficient to significantly stabilize the chemical composition and microstructure of the conversion coating, thereby improving its overall performance. Of course, the actual treatment time may be adjusted depending on the specific type of trivalent chromium salt, the thickness of the conversion coating, and the required performance requirements. But in general, a longer natural aging treatment time helps to obtain a more stable and reliable conversion coating layer.
[0076] During the natural aging treatment, the aluminum alloy samples should be kept in a dry, dust-free, non-corrosive gas environment to avoid adverse effects on the conversion film caused by external factors. In addition, the temperature and humidity during the treatment process should be monitored to ensure the consistency and repeatability of the treatment conditions.
[0077] In another embodiment, the present invention provides an aluminum alloy obtained by using the aluminum alloy surface treatment method of any of the above-mentioned embodiments, wherein a hydrophilic, corrosion-resistant, conductive film layer is formed on the surface of the aluminum alloy.
[0078] The following is an explanation with reference to specific examples.
[0079] Embodiment 1, a 2024-T351 aluminum alloy surface treatment method, comprising the following steps:
[0080] S1, pretreatment: removing impurities from the surface of the aluminum alloy. Specifically, the 2024-T351 aluminum alloy is subjected to alkaline etching, pickling and rinsing in sequence.
[0081] Alkali etching: After grinding, the 2024-T351 aluminum alloy sample was placed in an alkaline etching tank at a temperature of 60°C for alkaline etching treatment. The alkaline etching tank solution was a sodium hydroxide solution with a concentration of 10wt%, and the alkaline etching time was 5min. The alkaline-etched sample was rinsed with deionized water for 30s.
[0082] Pickling: Place the sample after alkaline etching and water washing in a pickling tank for pickling and deashing at room temperature. The pickling tank liquid is a 30vt% nitric acid solution, and the pickling time is 30s. Rinse the pickled sample with deionized water for 30s.
[0083] S2, first anodizing treatment: the pretreated aluminum alloy is placed in a mixed solution of 0.53M tartaric acid and 0.46M sulfuric acid, and the first constant potential anodizing is performed at a preset voltage of 1.5V (the reference electrode is a saturated calomel electrode). The temperature of the anodizing solution, i.e. the mixed solution of tartaric acid and sulfuric acid, is 37°C, and the anodizing time is 5min, so as to form an oxide film on the surface of the aluminum alloy and remove the second phase particles on the surface of the aluminum alloy.
[0084] S3, stripping treatment: The first anodized aluminum alloy sample was immersed in a mixed solution of CrO3 with a concentration of 20 g / L and H3PO4 with a concentration of 35 mL / L at a temperature of 60°C for 30 minutes to strip off the oxide film. The stripped sample was washed with deionized water and dried with cold air.
[0085] S4, second anodizing treatment: the aluminum alloy sample after the film stripping treatment is placed in a mixed solution of 0.53M tartaric acid and 0.46M sulfuric acid, and a second constant potential anodizing is performed at a preset voltage of 14V (the reference electrode is a saturated calomel electrode), the temperature of the anodizing solution, i.e., the mixed solution of tartaric acid and sulfuric acid, is 37°C, and the anodizing time is 25min, so as to form a porous anodized film on the surface of the aluminum alloy;
[0086] S5, trivalent chromium salt conversion film treatment: The aluminum alloy obtained in S4 is immersed in a trivalent chromium salt solution at a temperature of 40°C for 15 minutes, and the porous anodized film is used to absorb the trivalent chromium ions in the salt solution, and a coordination polymerization reaction occurs with the hydroxyl groups in the oxide film, forming a conversion film precursor on the pore wall of the porous oxide film and the barrier layer where the porous oxide film contacts the aluminum alloy surface. Then the treated aluminum alloy sample is rinsed in a large amount of deionized water for 1 minute.
[0087] S6, natural aging treatment: the aluminum alloy sample after the above conversion film treatment is placed in a backlit, cool laboratory atmosphere for natural aging treatment for 48 hours, so that the conversion film precursor undergoes a dehydration reaction to form a dense and continuous conversion film, repair the micro defects on the pore wall and barrier layer of the porous anodized film, and form a hydrophilic, corrosion-resistant and conductive film layer on the surface of the aluminum alloy.
[0088] Embodiment 2, a 7075-T6 aluminum alloy surface treatment method, comprising the following steps:
[0089] S1, pretreatment: removing impurities from the surface of the aluminum alloy. Specifically, 7075-T6 aluminum alloy is subjected to alkaline etching, pickling and rinsing in sequence.
[0090] Alkali etching: After grinding, the 7075-T6 aluminum alloy sample was placed in an alkaline etching tank at a temperature of 60°C for alkaline etching treatment. The alkaline etching tank solution was a sodium hydroxide solution with a concentration of 10wt%, and the alkaline etching time was 5min. The alkaline-etched sample was rinsed with deionized water for 30s.
[0091] Pickling: Place the sample after alkaline etching and water washing in a pickling tank for pickling and deashing at room temperature. The pickling tank liquid is a 30vt% nitric acid solution, and the pickling time is 30s. Rinse the pickled sample with deionized water for 30s.
[0092] S2, first anodizing treatment: the pretreated aluminum alloy is placed in a phosphoric acid solution with a concentration of 145 g / L, and the first constant potential anodizing is performed at a preset voltage of 3 V (the reference electrode is a saturated calomel electrode). The temperature of the anodizing solution, i.e., the phosphoric acid solution, is 20°C, and the anodizing time is 5 min to form an oxide film on the surface of the aluminum alloy and remove the second phase particles on the surface of the aluminum alloy.
[0093] S3, stripping treatment: The first anodized aluminum alloy sample was immersed in a mixed solution of CrO3 with a concentration of 20 g / L and H3PO4 with a concentration of 35 mL / L at a temperature of 60°C for 40 minutes to strip off the oxide film. The stripped sample was washed with deionized water and dried with cold air.
[0094] S4, second anodizing treatment: placing the aluminum alloy sample after the film stripping treatment in a phosphoric acid solution with a concentration of 145 g / L, and performing a second constant potential anodizing at a preset voltage of 38 V (the reference electrode is a saturated calomel electrode), the temperature of the anodizing solution, i.e., the phosphoric acid solution, is 20° C., and the anodizing time is 30 min, so as to form a porous anodized film on the surface of the aluminum alloy;
[0095] S5, trivalent chromium salt conversion film treatment: The aluminum alloy obtained in S4 is immersed in a trivalent chromium salt solution at a temperature of 40°C for 10 minutes, and the porous anodized film is used to absorb the trivalent chromium ions in the salt solution, and a coordination polymerization reaction occurs with the hydroxyl groups in the oxide film, forming a conversion film precursor on the pore wall of the porous oxide film and the barrier layer where the porous oxide film contacts the aluminum alloy surface. Then the treated aluminum alloy sample is rinsed in a large amount of deionized water for 1 minute.
[0096] S6, natural aging treatment: the aluminum alloy sample after the above conversion film treatment is placed in a backlit, cool laboratory atmosphere for natural aging treatment for 48 hours, so that the conversion film precursor undergoes a dehydration reaction to form a dense and continuous conversion film, repair the micro defects on the pore wall and barrier layer of the porous anodized film, and form a hydrophilic, corrosion-resistant and conductive film layer on the surface of the aluminum alloy.
[0097] Comparative Example 1, a 2024-T351 aluminum alloy surface treatment method, which is different from Example 1 in that it does not include S5 trivalent chromium salt conversion film treatment and S6 natural aging treatment.
[0098] Comparative Example 2, a 2024-T351 aluminum alloy surface treatment method, which is different from Example 1 in that it does not include the S2 first anodizing treatment and the S3 stripping treatment.
[0099] Comparative Example 3, a 7075-T6 aluminum alloy surface treatment method, which is different from Example 2 in that it does not include S5 trivalent chromium salt conversion film treatment and S6 natural aging treatment.
[0100] The aluminum alloy samples prepared in Example 1, Example 2 and Comparative Examples 1 to 3 were tested and analyzed, specifically including:
[0101] 1. Copper sulfate spot test: Prepare a copper sulfate spot solution with a concentration of 41g / L copper sulfate, 35g / L sodium chloride, and 20ml / L concentrated hydrochloric acid. Apply the copper sulfate spot solution to the treated sample and observe the time when the red corrosion point appears at room temperature of 26°C. The corrosion resistance of the sample film layer is judged by the time when the red corrosion point appears. The longer the waiting time for the red corrosion point to appear, the better the corrosion resistance of the film layer.
[0102] Figure 2The copper sulfate dripping results of 2024-T351 aluminum alloy after being treated by Example 1 of the present invention are compared with the copper sulfate dripping results of Comparative Example 1 and Comparative Example 2. Figure 2 It can be seen that after the aluminum alloy sample treated in Example 1, a small amount of red rust spots appeared after 26 minutes of dripping, the aluminum alloy sample treated in Comparative Example 1 showed a large area of red rust spots in 10 minutes, and the aluminum alloy sample treated in Comparative Example 2 showed red rust spots in 16 minutes, and a large area of red rust spots in 24 minutes. By comparing Example 1 and Comparative Example 1, it can be seen that the trivalent chromium conversion film treatment and the subsequent natural aging treatment can greatly improve the corrosion resistance of the film layer; by comparing Example 1 and Comparative Example 2, it can be seen that the corrosion resistance of the final film layer can also be significantly improved after two anodizing.
[0103] Figure 3 The copper sulfate dripping result of the aluminum alloy sample of 7075-T6 aluminum alloy treated by Example 2 of the present invention and the copper sulfate dripping result of the aluminum alloy sample treated by Comparative Example 3 is compared. Figure 3 It can be seen that the aluminum alloy sample treated in Example 2 has obvious red rust spots after 300s of dripping, and the aluminum alloy sample treated in Comparative Example 3 has large-area rust spots after 120s of dripping. By comparing Example 2 and Comparative Example 3, it can be seen that the trivalent chromium conversion film treatment and the subsequent natural aging treatment can improve the corrosion resistance of the film layer to a certain extent; by comparing Example 1 and Example 2, it can be seen that tartaric acid-sulfuric acid anodization has better corrosion resistance than phosphoric acid anodization.
[0104] 2. Morphology observation: The surface morphology of the anodic oxide film on the surface of the 2024-T351 aluminum alloy treated in Example 1 and the 27075-T6 aluminum alloy treated in Example 2 was observed by field emission scanning electron microscopy. The results are as follows: Figure 4 , Figure 5 As shown. Figure 4 and Figure 5 It can be seen that after the treatment in Example 1 and Example 2, the oxide film on the surface of the aluminum alloy is flat and uniform, and its unique nano-pores are still clearly visible, indicating that after two anodizing treatments, the influence of the second phase particles on the oxide film is weakened, and the uniform growth of the film layer is promoted, while the subsequent trivalent chromium conversion film treatment and natural aging treatment do not change the porous structure of the anodized film. Figure 2 , Figure 3 The results of the spot test and Figure 4 , Figure 5 From the analysis of the film surface morphology, it can be seen that Example 1 and Example 2 retain the porous structure of the anodized film while improving the corrosion resistance of the alloy, which is beneficial to improving the surface wettability and electrical conductivity (see contact angle test and resistance test for details).
[0105] 3. Contact angle test: The surface contact angle test was performed on the aluminum alloy samples of Example 1 and Example 2, and the results were as follows: Figure 6 and Figure 7 As shown. Figure 6 and Figure 7 It can be seen from the analysis that the water contact angles of the 2024-T351 aluminum alloy surface treated in Example 1 and the 7075-T6 aluminum alloy surface treated in Example 2 are both much smaller than 90°, indicating that the alloy surfaces treated in Example 1 and Example 2 have good surface wetting properties.
[0106] 4. Surface resistance test: The surface resistance of the aluminum alloy samples obtained in Example 1, Example 2, Comparative Example 1, Comparative Example 2, and Comparative Example 3 were tested using a DC resistance tester. The results are shown in Table 1. From the analysis results, it can be seen that the surface resistance of all samples is less than 100 mΩ, and their surfaces have good conductive properties.
[0107] Table 1 Surface resistance test results of different samples
[0108] Group Embodiment 1 Comparative Example 1 Comparative Example 2 Embodiment 2 Comparative Example 3 Resistance (mΩ) 79.97 76.01 76.53 56.70 52.49
[0109] In summary, the aluminum alloy surface treatment method described in the present invention can form a hydrophilic, corrosion-resistant and conductive film layer on the aluminum alloy surface, which can significantly improve the corrosion resistance of the aluminum alloy anodized film, while allowing the alloy surface to still maintain good conductivity and wettability, thereby meeting the complex performance requirements of the surface film layer for high-strength aluminum alloys in special fields.
[0110] The above embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Any equivalent substitution or change made by a person skilled in the art based on the present invention is within the protection scope of the present invention.
Claims
1. A method for treating the surface of an aluminum alloy, characterized in that: The steps include: S1, pretreatment: removing impurities from the aluminum alloy surface; S2, first anodizing treatment: placing the pretreated aluminum alloy in an acidic aqueous solution, and performing a first constant potential anodizing treatment at a preset voltage to form an oxide film on the surface of the aluminum alloy and remove the second phase particles on the surface of the aluminum alloy; S3, stripping treatment: immersing the aluminum alloy obtained in S2 in a stripping solution to dissolve the oxide film on the surface of the aluminum alloy; S4, a second anodizing treatment: placing the aluminum alloy after the film stripping treatment in an acidic aqueous solution, and performing a second constant potential anodizing at a preset voltage to form a porous anodized film on the surface of the aluminum alloy; S5, trivalent chromium salt conversion film treatment: the aluminum alloy obtained in S4 is placed in a trivalent chromium salt solution, the trivalent chromium ions in the salt solution are adsorbed by the porous anodic oxide film, and a coordination polymerization reaction is carried out with the hydroxyl groups in the oxide film, so as to form a conversion film precursor on the pore wall of the porous oxide film and on the barrier layer where the porous oxide film contacts the surface of the aluminum alloy; S6, natural aging treatment: natural aging is carried out at room temperature to cause the conversion film precursor to undergo a dehydration reaction, generate a dense and continuous conversion film, repair the microscopic defects on the pore wall and barrier layer of the porous anodized film, and form a hydrophilic, corrosion-resistant and conductive film layer on the surface of the aluminum alloy.
2. The aluminum alloy surface treatment method according to claim 1, characterized in that: The impurity removal treatment in S1 includes sequentially subjecting the aluminum alloy to alkaline etching, pickling and rinsing.
3. The aluminum alloy surface treatment method according to claim 1, characterized in that: The acidic aqueous solution in S2 and S4 includes at least one of sulfuric acid, tartaric acid, phosphoric acid and oxalic acid.
4. The aluminum alloy surface treatment method according to claim 1, characterized in that: The preset voltage of the first anodizing treatment in S2 is 0~3V, the reference electrode is a saturated calomel electrode, the first constant potential anodizing temperature is 20~40℃, and the first constant potential anodizing time is 3~10min.
5. The aluminum alloy surface treatment method according to claim 1, characterized in that: The preset voltage of the second anodizing treatment in S4 is 10-40 V, the reference electrode is a saturated calomel electrode, the second constant potential anodizing temperature is 20-40° C., and the second constant potential anodizing time is 15-30 min.
6. The aluminum alloy surface treatment method according to claim 1, characterized in that: The stripping solution in S3 includes a mixed aqueous solution of chromic anhydride and phosphoric acid, the stripping treatment temperature is 50-60°C, and the stripping treatment time is 30-60 minutes.
7. The aluminum alloy surface treatment method according to claim 1, characterized in that: The trivalent chromium salt in S5 includes at least one of chromium sulfate, chromium chloride, and basic chromium sulfate; The concentration of the trivalent chromium salt solution is 0.0001-0.01 mol / L, and the pH of the trivalent chromium salt solution is 3-5; The treatment temperature of trivalent chromium salt conversion film is 20~60℃, and the treatment time of trivalent chromium salt conversion film is 5~30min.
8. The aluminum alloy surface treatment method according to claim 1, characterized in that: After the trivalent chromium salt conversion film treatment of S5 is completed, the aluminum alloy is rinsed in deionized water at room temperature for 1 to 2 minutes, naturally air-dried, and then subjected to the natural aging treatment of S6.
9. The aluminum alloy surface treatment method according to claim 1, characterized in that: The natural aging treatment time in S6 is not less than 48h.