Melt direct spinning antimony-free polyester fiber and preparation method thereof
By adding antibacterial agents and antistatic modifiers to the melt spinning process of polyester fibers, the problem of the surface of polyester fibers being easily adhered to bacteria and lack of moisture absorption ability, and its excellent antibacterial and antistatic properties are achieved. Improves the fracture toughness and hygroscopicity of the fibers.
Patent Information
- Application Number
- CN202411246623.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-06
AI Technical Summary
Existing polyester fibers lack antibacterial function, and their surfaces are easily adhered to by bacteria, lack of moisture absorption and are prone to static electricity, resulting in difficult production processes and discomfort in use.
Antibacterial agents are prepared by adding antibacterial agents and antistatic modifiers during direct spinning of melt, using 2-pyridinyl alcohol and decyl bromide to synthesize antibacterial intermediates, and grafting with chitosan; using γ-methyl Acryloyloxypropyltrimethoxysilane modified graphene oxide copolymerized with methacryloyloxyethyltrimethylammonium chloride to prepare antistatic modifiers, and esterification reactions combined with titanium catalysts to prepare excellent preparation Antimony-free polyester fiber with antibacterial and antistatic properties.
It imparts excellent fracture toughness, hygroscopicity and antistatic properties to polyester fibers, significantly improves its antibacterial properties, and enhances its hygroscopicity and mechanical properties.
Smart Images

Figure BDA0005030960860000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyester fibers, and in particular relates to a melt-spun antimony-free polyester fiber and a preparation method thereof. Background Art
[0002] Polyester fiber is a synthetic fiber obtained by spinning polyester formed by the polycondensation of organic dibasic acid and diol, referred to as PET fiber. Due to its excellent modulus, strength, elasticity, shape retention and heat resistance, polyester fiber has become one of the most widely used and consumed chemical fiber varieties, accounting for more than 50% of the total textile fiber, and is commonly used in home furnishings, clothing, industrial textiles and other fields.
[0003] At present, the production methods of polyester fibers include chip spinning and melt spinning. The chip spinning process mainly produces fibers by drying polyester chips, heating the screw and then melt-extruding them into a spinning box. Early polyester fiber production mostly adopted this method, but chip spinning technology has the disadvantages of high energy consumption, long process and unstable product quality. In recent years, chip spinning has gradually been replaced by melt spinning. The melt spinning process has the advantages of economies of scale and low cost and has become the main process route for polyester fiber production.
[0004] The polyester fiber prepared by the prior art does not have antibacterial function, and its loose and porous surface is easily attached by external bacteria and microorganisms, and the bacteria will grow and multiply rapidly under nutritional conditions such as human sweat. In addition, the macromolecules of polyester fiber are connected to each other by covalent bonds, and cannot be ionized, nor can they transfer electrons and ions. Moreover, its molecular groups have low polarity and poor hydrophilicity, resulting in insufficient moisture absorption capacity and easy generation of static electricity. Static electricity not only causes difficulties in the production process of polyester fiber, causing the fabrics to entangle with each other and absorb dust, but also causes the fiber fabrics to entangle with the human body, causing discomfort. Summary of the invention
[0005] In order to solve the deficiencies mentioned in the above background technology, the purpose of the present invention is to provide a melt-spun antimony-free polyester fiber and a preparation method thereof. By adding antibacterial agents and antistatic modifiers, the polyester fiber is endowed with excellent fracture toughness, good hygroscopicity and antistatic properties, and at the same time has excellent antibacterial properties.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] A method for preparing melt-spun antimony-free polyester fiber is prepared by the following method: using terephthalic acid and ethylene glycol in a molar ratio of 1:1.3-1.6 as reaction raw materials, adding an antibacterial agent, an antistatic modifier and a titanium catalyst, undergoing an esterification reaction and a pre-polycondensation process, and then undergoing a final polycondensation reaction and a spinning process to prepare the melt-spun antimony-free polyester fiber; the mass of the antibacterial agent is 1-4% of the mass of the terephthalic acid, and the mass of the antistatic modifier is 0.5-2% of the mass of the terephthalic acid;
[0008] The antibacterial agent is prepared by synthesizing an antibacterial intermediate using 2-pyridinemethanol and decyl bromide, grafting the antibacterial intermediate with chitosan using isophorone diisocyanate as a linker, and further grafting p-hydroxybenzoic acid; the antistatic modifier is prepared by modifying graphene oxide using γ-methacryloxypropyltrimethoxysilane, and then copolymerizing with methacryloxyethyltrimethylammonium chloride and methoxypolyethylene glycol acrylate.
[0009] Preferably, the titanium-based catalyst is one or more combinations of titanium glycol, titanate, and nano-titanium dioxide.
[0010] Preferably, the method for preparing the antibacterial agent comprises the following steps:
[0011] A. Take 2-pyridinemethanol and decyl bromide in a reactor, add 1,4-dioxane solvent, place at 95-110° C. and stir to react for 42-48 hours. After the reaction is completed, the antibacterial intermediate is prepared by rotary evaporation, washing, suction filtration and drying;
[0012] B. Put isophorone diisocyanate in a reactor, add anhydrous butyl acetate solvent and dibutyltin dilaurate catalyst, raise the temperature to 35-45° C., add the antibacterial intermediate and stir to react for 5-6 hours to prepare an isocyanate antibacterial intermediate;
[0013] C. Dispersing chitosan in methanol-water solution to obtain chitosan solution, dissolving benzaldehyde in methanol and adding it to the chitosan solution, adjusting the pH value of the system to 4.5-5, heating to 45-55° C. to react for 3-5 hours, and filtering after the reaction, washing and drying to prepare N-benzylidene chitosan;
[0014] D. Dissolve N-benzylidene chitosan in acetone, raise the temperature to 50-70°C, add dibutyltin dilaurate catalyst, mix the isocyanate antibacterial intermediate with acetone evenly, and then add it to the reaction system to react for 8-11 hours. Dissolve the obtained product in a mixture of hydrochloric acid and ethanol, react for 20-24 hours, and after the reaction is completed, filter, wash, and dry to prepare modified chitosan;
[0015] E. Take the modified chitosan and dissolve it in deionized water to obtain a mixed solution. Take p-hydroxybenzoic acid and dissolve it in methanol. Add 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide. After stirring and mixing, add them to the mixed solution. Place it at 30-40°C to react for 20-24 hours. After the reaction is completed, dialyze and dry to prepare an antibacterial agent.
[0016] Preferably, the mass ratio of the 2-pyridinemethanol, decyl bromide and isophorone diisocyanate is 1:3.8-4.4:1.4-1.8.
[0017] Preferably, the preparation method of the antistatic modifier comprises the following steps:
[0018] (1) taking graphene oxide in anhydrous ethanol, dispersing it in a water bath by ultrasonication, adding γ-methacryloxypropyltrimethoxysilane, and reacting it under reflux at 105-120° C. for 10-12 hours in a nitrogen atmosphere, and filtering, washing, and drying after the reaction is completed to prepare modified graphene oxide;
[0019] (2) The modified graphene oxide was ultrasonically dispersed in anhydrous ethanol, and methacryloyloxyethyl trimethylammonium chloride and methoxy polyethylene glycol acrylate were added in a nitrogen atmosphere, and stirred to mix evenly at room temperature, and then azobisisobutyronitrile was added, and the temperature was raised to 70-80°C for reaction for 6-7h. After the reaction was completed, the temperature was lowered to room temperature, and the antistatic modifier was prepared by precipitation and drying.
[0020] Preferably, in step (2), the mass ratio of methacryloyloxyethyltrimethylammonium chloride, modified graphene oxide and methoxy polyethylene glycol acrylate is 7.5-9.2:0.5-1:4-5.
[0021] Preferably, the method specifically comprises the following steps:
[0022] S1, mixing ethylene glycol (70-75% of the total amount of ethylene glycol) and terephthalic acid uniformly to obtain a mixed slurry;
[0023] S2, mixing 15-20% of the total amount of ethylene glycol and a titanium catalyst to obtain a catalyst liquid;
[0024] S3, taking the antibacterial agent, the antistatic modifier and the remaining ethylene glycol and mixing them evenly to obtain an additive suspension;
[0025] S4, after mixing the mixed slurry and the catalyst liquid, a first esterification reaction is carried out at a temperature of 230-250° C. and a reaction time of 1-3 hours. When the esterification rate of the antimony-free polyester polymerization reaches 85-90%, the additive suspension is added to carry out a second esterification reaction at a temperature of 230-250° C. and a reaction time of 0.5-1 hour to obtain an esterified product;
[0026] S5, pressing the esterification product into a pre-condensation reactor, drawing a low vacuum to discharge excess ethylene glycol, and performing pre-condensation to obtain a pre-condensation product;
[0027] S6, pressing the pre-polycondensation product into a final polycondensation kettle, and further evacuating the polycondensation to obtain a melt;
[0028] S7. The melt is subjected to a spinning process to prepare melt-spun antimony-free polyester fibers.
[0029] Preferably, the vacuum degree of the pre-polycondensation is 1-100 KPa, the temperature is 250-265°C, and the reaction time is 0.5-1h; the vacuum degree of the final polycondensation reactor is 30-80 Pa, the final polycondensation temperature is 260-280°C, and the reaction time is 0.8-3h.
[0030] Preferably, the parameters of the spinning process are set as: spinning temperature 270-295°C, side blowing cooling temperature 25-30°C, side blowing wind speed 0.2-0.4 m / s, spinning speed 2800-3500 m / min, and draft ratio 3.0-4.0.
[0031] A melt-spun antimony-free polyester fiber is prepared by the above-mentioned preparation method.
[0032] Beneficial effects of the present invention:
[0033] The invention utilizes 2-pyridinemethanol and decyl bromide to synthesize an antibacterial intermediate, and then utilizes the hydroxyl group on the surface of the antibacterial intermediate to react with the isocyanate group directly connected to the cyclohexane in the isophorone diisocyanate molecule to synthesize the isocyanate-treated antibacterial intermediate. In addition, chitosan and benzaldehyde form an N-benzylidene chitosan Schiff base to protect the amino group on the chitosan molecule, and then further react with the isocyanate-treated antibacterial intermediate to make the isocyanate group react with the hydroxyl group on the surface of the N-benzylidene chitosan, so that the antibacterial intermediate containing a quaternary ammonium salt structure is grafted on the surface of the chitosan to prepare the modified chitosan, and in addition, the amino group in the modified chitosan structure is subjected to an amidation reaction with the carboxyl group in the p-hydroxybenzoic acid structure to prepare the antibacterial agent. The quaternary ammonium salt group and phenolic structure in the antibacterial agent molecule synergize with chitosan to achieve antibacterial effect, giving the polyester fiber excellent antibacterial effect. At the same time, the multiple amide and carbamate groups generated by the reaction are hydrophilic groups with strong polarity, which enhances the moisture absorption capacity of the polyester fiber.
[0034] The invention uses γ-methacryloxypropyltrimethoxysilane to modify graphene oxide, so that the graphene oxide is grafted with a double bond structure, and then copolymerized with methacryloxyethyltrimethylammonium chloride and methoxy polyethylene glycol acrylate to prepare an antistatic modifier. The graphene oxide has excellent mechanical properties, methacryloxyethyltrimethylammonium chloride is used as the main body of the antistatic agent, and methoxy polyethylene glycol acrylate is introduced into the molecular chain of the copolymer as a hydrophilic component to enhance the hygroscopic property of the copolymer. The addition of the antistatic modifier can give the polyester fiber excellent breaking strength, breaking elongation, hygroscopicity and antistatic property. DETAILED DESCRIPTION
[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] Embodiment 1 A method for preparing an antibacterial agent comprises the following steps:
[0037] A. Take 2.74g 2-pyridinemethanol and 11.06g decyl bromide in a reactor, add 50mL 1,4-dioxane solvent, place at 105°C and stir for 42h. After the reaction is completed, the antibacterial intermediate is prepared by rotary evaporation, washing, suction filtration and drying;
[0038] B. Take 3.85g of isophorone diisocyanate in a reactor, add 40mL of anhydrous butyl acetate solvent and 0.02g of dibutyltin dilaurate catalyst, raise the temperature to 40°C, add the antibacterial intermediate and stir to react for 6h to prepare an isocyanate antibacterial intermediate;
[0039] C. Take 2g of chitosan and disperse it in 50% methanol-water solution to obtain a chitosan solution. Take 7.9g of benzaldehyde and dissolve it in 20mL of methanol and add it to the chitosan solution. Adjust the pH value of the system to 4.5, heat it to 50°C and react for 4h. After the reaction is completed, filter it with suction, wash it, and dry it to prepare N-benzylidene chitosan.
[0040] D. Take 2g of N-benzylidene chitosan and dissolve it in 100mL of acetone, heat it to 65°C, add 0.02g of dibutyltin dilaurate catalyst, take 5g of isocyanate antibacterial intermediate and mix it evenly with 20mL of acetone, then add it to the reaction system to react for 10h, dissolve the obtained product in 0.5mol / L hydrochloric acid / ethanol solution, react for 24h, filter after the reaction is completed, wash and dry to prepare modified chitosan;
[0041] E. Take 2g of modified chitosan and dissolve it in 60mL of deionized water to obtain a mixed solution. Take 0.9g of p-hydroxybenzoic acid and dissolve it in 50mL of methanol. Add 1.2g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and 0.7g of N-hydroxysuccinimide. Stir and mix them and add them to the mixed solution. Place it at 30°C to react for 24h. After the reaction is completed, dialyze and dry to prepare an antibacterial agent.
[0042] Embodiment 2 A method for preparing an antistatic modifier comprises the following steps:
[0043] (1) 0.2 g of graphene oxide was dissolved in 20 mL of anhydrous ethanol, and ultrasonically dispersed in a water bath, 3 g of γ-methacryloxypropyltrimethoxysilane was added, and the mixture was refluxed at 110° C. for 12 h in a nitrogen atmosphere. After the reaction was completed, the mixture was filtered, washed, and dried to prepare modified graphene oxide;
[0044] (2) Take 0.8 g of modified graphene oxide and ultrasonically disperse it in 150 mL of anhydrous ethanol. In a nitrogen atmosphere, add 8.2 g of methacryloyloxyethyl trimethylammonium chloride and 4.7 g of methoxy polyethylene glycol acrylate, stir and mix evenly at room temperature, then add azobisisobutyronitrile, raise the temperature to 70-80 ° C to react for 6-7 hours, cool to room temperature after the reaction is completed, precipitate and dry to prepare an antistatic modifier.
[0045] Embodiment 3 A method for preparing a melt-spun antimony-free polyester fiber comprises the following steps:
[0046] S1, ethylene glycol (75% of the total amount of ethylene glycol) and terephthalic acid are uniformly mixed to obtain a mixed slurry, wherein the molar ratio of the total amount of ethylene glycol to terephthalic acid is 1.5:1;
[0047] S2, ethylene glycol (15% of the total amount of ethylene glycol) and nano-titanium dioxide are mixed evenly to obtain a catalyst liquid, wherein the amount of nano-titanium dioxide used is 250ppm of the total mass of terephthalic acid;
[0048] S3, taking 1% by weight of terephthalic acid and the antibacterial agent prepared in Example 1, 0.5% by weight of terephthalic acid and the antistatic modifier prepared in Example 2, and the remaining ethylene glycol, and mixing them evenly to obtain an additive suspension;
[0049] S4, after mixing the mixed slurry and the catalyst liquid, a first esterification reaction is carried out at a temperature of 230° C. and a reaction time of 1.5 h. When the polymerization esterification rate of the antimony-free polyester reaches 85%, the additive suspension is added to carry out a second esterification reaction at a temperature of 240° C. and a reaction time of 1 h to obtain an esterified product;
[0050] S5, press the esterification product into a pre-condensation reactor, draw a low vacuum to discharge the excess ethylene glycol, and carry out pre-condensation at a temperature of 250° C. for a reaction time of 1 h to obtain a pre-condensation product;
[0051] S6, press the pre-polycondensation product into the final polycondensation kettle at a temperature of 270°C and a reaction time of 1.5h, and further perform high vacuum polycondensation to obtain a melt;
[0052] S7. The melt is subjected to a spinning process to obtain melt-spun antimony-free polyester fiber, with a spinning temperature of 290° C., a side-blowing cooling temperature of 25° C., a side-blowing wind speed of 0.3 m / s, a spinning speed of 3000 m / min, and a draft ratio of 3.5.
[0053] Embodiment 4 A method for preparing a melt-spun antimony-free polyester fiber comprises the following steps:
[0054] S1. Ethylene glycol (75% of the total amount of ethylene glycol) and terephthalic acid are uniformly mixed to obtain a mixed slurry, wherein the molar ratio of the total amount of ethylene glycol to terephthalic acid is 1.5:1;
[0055] S2, 15% of the total amount of ethylene glycol and nano-titanium dioxide are mixed evenly to obtain a catalyst liquid, wherein the amount of nano-titanium dioxide used is 250ppm of the total mass of terephthalic acid;
[0056] S3, taking 2% by weight of terephthalic acid prepared in Example 1, the antistatic modifier prepared in Example 2 with 1% by weight of terephthalic acid, and the remaining ethylene glycol, and mixing them evenly to obtain an additive suspension;
[0057] S4, after mixing the mixed slurry and the catalyst liquid, a first esterification reaction is carried out at a temperature of 230° C. and a reaction time of 1.5 h. When the polymerization esterification rate of the antimony-free polyester reaches 85%, the additive suspension is added to carry out a second esterification reaction at a temperature of 240° C. and a reaction time of 1 h to obtain an esterified product;
[0058] S5, press the esterification product into a pre-condensation reactor, draw a low vacuum to discharge the excess ethylene glycol, and carry out pre-condensation at a temperature of 250° C. for a reaction time of 1 h to obtain a pre-condensation product;
[0059] S6, press the pre-polycondensation product into the final polycondensation kettle at a temperature of 270°C and a reaction time of 1.5h, and further perform high vacuum polycondensation to obtain a melt;
[0060] S7. The melt is subjected to a spinning process to obtain melt-spun antimony-free polyester fiber, with a spinning temperature of 290° C., a side-blowing cooling temperature of 25° C., a side-blowing wind speed of 0.3 m / s, a spinning speed of 3000 m / min, and a draft ratio of 3.5.
[0061] Embodiment 5 A method for preparing a melt-spun antimony-free polyester fiber comprises the following steps:
[0062] S1. Ethylene glycol (75% of the total amount of ethylene glycol) and terephthalic acid are uniformly mixed to obtain a mixed slurry, wherein the molar ratio of the total amount of ethylene glycol to terephthalic acid is 1.5:1;
[0063] S2, 15% of the total amount of ethylene glycol and nano-titanium dioxide are mixed evenly to obtain a catalyst liquid, wherein the amount of nano-titanium dioxide used is 250ppm of the total mass of terephthalic acid;
[0064] S3, taking 4% by weight of terephthalic acid prepared in Example 1, the antistatic modifier prepared in Example 2 and 2% by weight of terephthalic acid, and mixing them evenly with the remaining ethylene glycol to obtain an additive suspension;
[0065] S4, after mixing the mixed slurry and the catalyst liquid, a first esterification reaction is carried out at a temperature of 230° C. and a reaction time of 1.5 h. When the polymerization esterification rate of the antimony-free polyester reaches 85%, the additive suspension is added to carry out a second esterification reaction at a temperature of 240° C. and a reaction time of 1 h to obtain an esterified product;
[0066] S5, press the esterification product into a pre-condensation reactor, draw a low vacuum to discharge the excess ethylene glycol, and carry out pre-condensation at a temperature of 250° C. for a reaction time of 1 h to obtain a pre-condensation product;
[0067] S6, press the pre-polycondensation product into the final polycondensation kettle at a temperature of 270°C and a reaction time of 1.5h, and further perform high vacuum polycondensation to obtain a melt;
[0068] S7. The melt is subjected to a spinning process to obtain melt-spun antimony-free polyester fiber, with a spinning temperature of 290° C., a side-blowing cooling temperature of 25° C., a side-blowing wind speed of 0.3 m / s, a spinning speed of 3000 m / min, and a draft ratio of 3.5.
[0069] Comparative Example 1 A method for preparing an antibacterial agent comprises the following steps:
[0070] A. Take 2-pyridinemethanol and decyl bromide in a reactor, add 1,4-dioxane solvent, place at 95-110° C. and stir to react for 42-48 hours. After the reaction is completed, the antibacterial intermediate is prepared by rotary evaporation, washing, suction filtration and drying;
[0071] B. Put isophorone diisocyanate in a reactor, add anhydrous butyl acetate solvent and dibutyltin dilaurate catalyst, raise the temperature to 35-45° C., add the antibacterial intermediate and stir to react for 5-6 hours to prepare an isocyanate antibacterial intermediate;
[0072] C. Dispersing chitosan in methanol-water solution to obtain chitosan solution, dissolving benzaldehyde in methanol and adding it to the chitosan solution, adjusting the pH value of the system to 4.5-5, heating to 45-55° C. to react for 3-5 hours, and filtering after the reaction, washing and drying to prepare N-benzylidene chitosan;
[0073] D. Dissolve N-benzylidene chitosan in acetone, raise the temperature to 50-70°C, add dibutyltin dilaurate catalyst, mix the isocyanate antibacterial intermediate with acetone evenly, and add it to the reaction system to react for 8-11 hours. Dissolve the obtained product in a mixture of hydrochloric acid and ethanol, react for 20-24 hours, and after the reaction is completed, filter, wash and dry to prepare the antibacterial agent.
[0074] Comparative Example 2 A method for preparing a melt-spun antimony-free polyester fiber comprises the following steps:
[0075] S1. Ethylene glycol (75% of the total amount of ethylene glycol) and terephthalic acid are uniformly mixed to obtain a mixed slurry, wherein the molar ratio of the total amount of ethylene glycol to terephthalic acid is 1.5:1;
[0076] S2, 15% of the total amount of ethylene glycol and nano-titanium dioxide are mixed evenly to obtain a catalyst liquid, wherein the amount of nano-titanium dioxide used is 250ppm of the total mass of terephthalic acid;
[0077] S3, taking 4% by weight of terephthalic acid prepared in comparative example 1, 2% by weight of terephthalic acid prepared in example 2, and the remaining ethylene glycol, and mixing them evenly to obtain an additive suspension;
[0078] S4, after mixing the mixed slurry and the catalyst liquid, a first esterification reaction is carried out at a temperature of 230° C. and a reaction time of 1.5 h. When the polymerization esterification rate of the antimony-free polyester reaches 85%, the additive suspension is added to carry out a second esterification reaction at a temperature of 240° C. and a reaction time of 1 h to obtain an esterified product;
[0079] S5, press the esterification product into a pre-condensation reactor, draw a low vacuum to discharge the excess ethylene glycol, and carry out pre-condensation at a temperature of 250° C. for a reaction time of 1 h to obtain a pre-condensation product;
[0080] S6, press the pre-polycondensation product into the final polycondensation kettle at a temperature of 270°C and a reaction time of 1.5h, and further perform high vacuum polycondensation to obtain a melt;
[0081] S7. The melt is subjected to a spinning process to obtain melt-spun antimony-free polyester fiber, with a spinning temperature of 290° C., a side-blowing cooling temperature of 25° C., a side-blowing wind speed of 0.3 m / s, a spinning speed of 3000 m / min, and a draft ratio of 3.5.
[0082] Comparative Example 3 A method for preparing a melt-spun antimony-free polyester fiber comprises the following steps:
[0083] S1. Ethylene glycol (75% of the total amount of ethylene glycol) and terephthalic acid are uniformly mixed to obtain a mixed slurry, wherein the molar ratio of the total amount of ethylene glycol to terephthalic acid is 1.5:1;
[0084] S2, 15% of the total amount of ethylene glycol and nano-titanium dioxide are mixed evenly to obtain a catalyst liquid, wherein the amount of nano-titanium dioxide used is 250ppm of the total mass of terephthalic acid;
[0085] S3, taking 4% chitosan by weight of terephthalic acid, 2% by weight of terephthalic acid, the antistatic modifier prepared in Example 2, and the remaining ethylene glycol, and mixing them evenly to obtain an additive suspension;
[0086] S4, after mixing the mixed slurry and the catalyst liquid, a first esterification reaction is carried out at a temperature of 230° C. and a reaction time of 1.5 h. When the polymerization esterification rate of the antimony-free polyester reaches 85%, the additive suspension is added to carry out a second esterification reaction at a temperature of 240° C. and a reaction time of 1 h to obtain an esterified product;
[0087] S5, press the esterification product into a pre-condensation reactor, draw a low vacuum to discharge the excess ethylene glycol, and carry out pre-condensation at a temperature of 250° C. for a reaction time of 1 h to obtain a pre-condensation product;
[0088] S6, press the pre-polycondensation product into the final polycondensation kettle at a temperature of 270°C and a reaction time of 1.5h, and further perform high vacuum polycondensation to obtain a melt;
[0089] S7. The melt is subjected to a spinning process to obtain melt-spun antimony-free polyester fiber, with a spinning temperature of 290° C., a side-blowing cooling temperature of 25° C., a side-blowing wind speed of 0.3 m / s, a spinning speed of 3000 m / min, and a draft ratio of 3.5.
[0090] Comparative Example 4 A method for preparing a melt-spun antimony-free polyester fiber comprises the following steps:
[0091] S1. Ethylene glycol (75% of the total amount of ethylene glycol) and terephthalic acid are uniformly mixed to obtain a mixed slurry, wherein the molar ratio of the total amount of ethylene glycol to terephthalic acid is 1.5:1;
[0092] S2, 15% of the total amount of ethylene glycol and nano-titanium dioxide are mixed evenly to obtain a catalyst liquid, wherein the amount of nano-titanium dioxide used is 250ppm of the total mass of terephthalic acid;
[0093] S3, taking 4% by weight of terephthalic acid and mixing the antibacterial agent prepared in Example 1 with the remaining ethylene glycol to obtain an additive suspension;
[0094] S4, after mixing the mixed slurry and the catalyst liquid, a first esterification reaction is carried out at a temperature of 230° C. and a reaction time of 1.5 h. When the polymerization esterification rate of the antimony-free polyester reaches 85%, the additive suspension is added to carry out a second esterification reaction at a temperature of 240° C. and a reaction time of 1 h to obtain an esterified product;
[0095] S5, press the esterification product into a pre-condensation reactor, draw a low vacuum to discharge excess ethylene glycol, and perform pre-condensation at a temperature of 250° C. for a reaction time of 1 h to obtain a pre-condensation product;
[0096] S6, press the pre-polycondensation product into the final polycondensation kettle at a temperature of 270°C and a reaction time of 1.5h, and further evacuate the high vacuum polycondensation to obtain a melt;
[0097] S7. The melt is subjected to a spinning process to obtain melt-spun antimony-free polyester fiber, with a spinning temperature of 290° C., a side-blowing cooling temperature of 25° C., a side-blowing wind speed of 0.3 m / s, a spinning speed of 3000 m / min, and a draft ratio of 3.5.
[0098] Performance Testing
[0099] The polyester fibers prepared in Examples 3-5 and Comparative Examples 2-4 were subjected to performance tests: the mechanical properties of the fibers were tested in accordance with GB / T14337-2022; the antibacterial properties were tested in accordance with GB / T 20944.3-2008; 50 g of the polyester fibers were rinsed with ethanol twice and dried in an oven to constant weight, with the mass recorded as M0, and then immersed in a beaker filled with deionized water, allowed to stand for 48 hours, taken out, placed on a 100-mesh standard sieve, allowed to stand for 30 minutes until no liquid droplets were dropped, and then weighed, with the mass recorded as M1, and a water absorption test was performed. The water absorption was calculated according to the following formula: Water absorption = (M1-M0) / M0×100%, and the data results are shown in Table 1.
[0100] Table 1 Test results of sample performance
[0101]
[0102] It can be seen from the data in Table 1 that the polyester fibers prepared in Examples 3-5 of the present invention are not easy to break, have good hygroscopicity and antistatic properties, and also have excellent antibacterial properties. The antibacterial agent added in Comparative Example 2 does not contain a phenolic structure, and only chitosan is added as an antibacterial agent in Comparative Example 3. The antibacterial properties of Comparative Examples 2-3 are significantly lower than those of Examples 3-5, indicating that both the phenolic structure and the quaternary ammonium salt group can have a synergistic antibacterial effect with chitosan, and the hygroscopicity and antistatic properties of Comparative Examples 2-3 are slightly worse than those of Examples 3-5. The reason is that the isocyanate-treated antibacterial intermediate reacts with N-benzylidene chitosan to generate a carbamate group, and the modified chitosan reacts with p-hydroxybenzoic acid to generate an amide group. The amide group and the carbamate group are hydrophilic groups with strong polarity, which enhance the hygroscopicity and antistatic properties of the polyester fiber. No antistatic modifier is added in Comparative Example 4, and the breaking strength, elongation at break, and water absorption are lower than those of Examples 3-5, and the volume resistivity is increased compared with Examples 3-5, indicating that the addition of an antistatic modifier can improve the mechanical properties, hygroscopicity and antistatic properties of the polyester fiber.
[0103] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0104] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A method for preparing melt-spun antimony-free polyester fiber, characterized in that: The method is prepared by the following method: using terephthalic acid and ethylene glycol in a molar ratio of 1:1.3-1.6 as reaction raw materials, adding an antibacterial agent, an antistatic modifier and a titanium catalyst, undergoing an esterification reaction and a pre-polycondensation process, and then undergoing a final polycondensation reaction and a spinning process to prepare a melt-spun antimony-free polyester fiber; the mass of the antibacterial agent is 1-4% of the mass of the terephthalic acid, and the mass of the antistatic modifier is 0.5-2% of the mass of the terephthalic acid; The antibacterial agent is prepared by synthesizing an antibacterial intermediate using 2-pyridinemethanol and decyl bromide, grafting the antibacterial intermediate with chitosan using isophorone diisocyanate as a linker, and further grafting p-hydroxybenzoic acid; the antistatic modifier is prepared by modifying graphene oxide using γ-methacryloxypropyltrimethoxysilane, and then copolymerizing with methacryloxyethyltrimethylammonium chloride and methoxypolyethylene glycol acrylate.
2. The method for preparing melt-spun antimony-free polyester fiber according to claim 1, characterized in that: The titanium catalyst is one or more combinations of titanium glycol, titanate, and nano titanium dioxide.
3. The method for preparing melt-spun antimony-free polyester fiber according to claim 1, characterized in that: The preparation method of the antibacterial agent comprises the following steps: A. Take 2-pyridinemethanol and decyl bromide in a reactor, add 1,4-dioxane solvent, place at 95-110° C. and stir to react for 42-48 hours. After the reaction is completed, the antibacterial intermediate is prepared by rotary evaporation, washing, suction filtration and drying; B. Put isophorone diisocyanate in a reactor, add anhydrous butyl acetate solvent and dibutyltin dilaurate catalyst, raise the temperature to 35-45° C., add the antibacterial intermediate and stir to react for 5-6 hours to prepare an isocyanate antibacterial intermediate; C. Dispersing chitosan in methanol-water solution to obtain chitosan solution, dissolving benzaldehyde in methanol and adding it to the chitosan solution, adjusting the pH value of the system to 4.5-5, heating to 45-55° C. to react for 3-5 hours, and filtering after the reaction, washing and drying to prepare N-benzylidene chitosan; D. Dissolve N-benzylidene chitosan in acetone, raise the temperature to 50-70°C, add dibutyltin dilaurate catalyst, mix the isocyanate antibacterial intermediate with acetone evenly, and then add it to the reaction system to react for 8-11 hours. Dissolve the obtained product in a mixture of hydrochloric acid and ethanol, react for 20-24 hours, and after the reaction is completed, filter, wash, and dry to prepare modified chitosan; E. Take the modified chitosan and dissolve it in deionized water to obtain a mixed solution. Take p-hydroxybenzoic acid and dissolve it in methanol. Add 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide. After stirring and mixing, add them to the mixed solution. Place it at 30-40°C to react for 20-24 hours. After the reaction is completed, dialyze and dry to prepare an antibacterial agent.
4. The method for preparing melt-spun antimony-free polyester fiber according to claim 3, characterized in that: The mass ratio of the 2-pyridinemethanol, decyl bromide and isophorone diisocyanate is 1:3.8-4.4:1.4-1.
8.
5. The method for preparing melt-spun antimony-free polyester fiber according to claim 1, characterized in that: The preparation method of the antistatic modifier comprises the following steps: (1) taking graphene oxide in anhydrous ethanol, dispersing it in a water bath by ultrasonication, adding γ-methacryloxypropyltrimethoxysilane, and reacting it under reflux at 105-120° C. for 10-12 hours in a nitrogen atmosphere, and filtering, washing, and drying after the reaction is completed to prepare modified graphene oxide; (2) The modified graphene oxide was ultrasonically dispersed in anhydrous ethanol, and methacryloyloxyethyl trimethylammonium chloride and methoxy polyethylene glycol acrylate were added in a nitrogen atmosphere, and stirred to mix evenly at room temperature, and then azobisisobutyronitrile was added, and the temperature was raised to 70-80°C for reaction for 6-7h. After the reaction was completed, the temperature was lowered to room temperature, and the antistatic modifier was prepared by precipitation and drying.
6. The method for preparing melt-spun antimony-free polyester fiber according to claim 5, characterized in that: In the step (2), the mass ratio of methacryloyloxyethyl trimethylammonium chloride, modified graphene oxide and methoxy polyethylene glycol acrylate is 7.5-9.2:0.5-1:4-5.
7. The method for preparing melt-spun antimony-free polyester fiber according to claim 1, characterized in that: The method specifically comprises the following steps: S1, mixing ethylene glycol (70-75% of the total amount of ethylene glycol) and terephthalic acid uniformly to obtain a mixed slurry; S2, mixing 15-20% of the total amount of ethylene glycol and a titanium catalyst to obtain a catalyst liquid; S3, taking the antibacterial agent, the antistatic modifier and the remaining ethylene glycol and mixing them evenly to obtain an additive suspension; S4, after mixing the mixed slurry and the catalyst liquid, a first esterification reaction is carried out at a temperature of 230-250° C. and a reaction time of 1-3 hours. When the esterification rate of the antimony-free polyester polymerization reaches 85-90%, the additive suspension is added to carry out a second esterification reaction at a temperature of 230-250° C. and a reaction time of 0.5-1 hour to obtain an esterified product; S5, pressing the esterification product into a pre-condensation reactor, drawing a low vacuum to discharge excess ethylene glycol, and performing pre-condensation to obtain a pre-condensation product; S6, pressing the pre-polycondensation product into a final polycondensation kettle, and further evacuating the polycondensation to obtain a melt; S7. The melt is subjected to a spinning process to prepare melt-spun antimony-free polyester fibers.
8. The method for preparing melt-spun antimony-free polyester fiber according to claim 7, characterized in that: The vacuum degree of the pre-polycondensation is 1-100 KPa, the temperature is 250-265° C., and the reaction time is 0.5-1 h; the vacuum degree of the final polycondensation kettle is 30-80 Pa, the final polycondensation temperature is 260-280° C., and the reaction time is 0.8-3 h.
9. The method for preparing melt-spun antimony-free polyester fiber according to claim 7, characterized in that: The parameters of the spinning process are set as follows: spinning temperature 270-295° C., side blowing cooling temperature 25-30° C., side blowing wind speed 0.2-0.4 m / s, spinning speed 2800-3500 m / min, and draft ratio 3.0-4.
0.
10. A melt-spun antimony-free polyester fiber, characterized in that: Prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
A production method of hydrophilic moisture-transmitting polyester staple fibers used for direct spinning
CN105586659A
Preparation method of antimony-free antibacterial easy-to-dye copolyester and preparation method of fiber
CN118344574A
Antimony-free antibacterial deodorizing moisture-conducting polyester master batch, preparation method thereof and preparation method of fiber
CN118344713A
Preparation method for antimicrobial knitted fabric
WO2022143004A1
Manufacturing method for antimicrobial and Anti-yellowing zno antimony-free polyester fibers
WO2024008053A1
Cited By
Flame-retardant and high-strength polyester fiber and preparation method thereof
CN120967540A