Preparation method of porous polyurethane fiber
By controlling the ratio and temperature of non-solvents in the coagulation bath, and using precipitation-induced phase separation combined with atmospheric pressure drying, the problems of high energy consumption and expensive equipment in the preparation of porous polyurethane fibers were solved, and the preparation of porous polyurethane fibers with high porosity and high performance was achieved, which are suitable for lightweight and high-heat insulating textiles.
Patent Information
- Application Number
- CN202411044331.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-31
AI Technical Summary
Existing methods for preparing porous polyurethane fibers suffer from high energy consumption, long production cycles, and expensive equipment, making industrial-scale production difficult. Furthermore, these methods result in low porosity and poor performance.
Porous polyurethane fibers were prepared by using precipitation-induced phase separation combined with atmospheric pressure drying, and by controlling the non-solvent ratio and temperature in the coagulation bath to control the diffusion coefficient of phase separation kinetics.
It has achieved low-cost, green and environmentally friendly preparation of porous polyurethane fibers with high porosity and excellent performance, making them suitable for lightweight, high-heat insulation textile applications and easy to industrialize.
Smart Images

Figure CN118996664A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of textile application, and in particular relates to a method for preparing porous (homogeneous porous) polyurethane fibers, that is, a method for constructing porous polyurethane fibers through a precipitation-induced phase separation method and normal pressure drying. Background Art
[0002] Polyurethane fiber has been widely used in clothing, textiles, biomedical materials and other fields due to its high strength, low modulus, high resilience and high elongation at break.
[0003] At present, the methods for preparing porous polyurethane fibers are basically through wet spinning methods to obtain polyurethane gel fibers; the pore-making processes in the wet spinning method are different, some use freeze-drying methods to make pores, and some use precipitation-induced phase separation methods to make pores; the freeze-drying method is to obtain pores through ice crystal template sublimation, and the freeze-drying method has high energy consumption (minus 75°C) and a long cycle of 3-7 days; the precipitation-induced phase separation method uses water as a non-solvent (non-solvent of the coagulation bath), and the interaction force between the solvent and the non-solvent is large, resulting in a fast kinetic diffusion rate between the solvent and the non-solvent, resulting in a large number of large pores (50-300 micron pores) and a low porosity.
[0004] When the precipitation-induced phase separation method is adopted, due to the presence of a large number of gas-liquid and liquid-liquid interfaces inside the polyurethane gel, the gel will shrink and crack violently during the normal pressure drying process, which will eventually lead to the deterioration of fiber performance (the porosity of the porous fiber product decreases, the elongation at break decreases, and there is no thermal insulation performance), so that high-quality porous fiber products cannot be obtained. In order to solve this key technical problem, at this stage, the subsequent drying process is usually achieved by supercritical drying or freeze drying, but these methods still have some drawbacks, such as expensive equipment, harsh process conditions, long cycles, and disadvantages such as being unfavorable for large-scale production of porous fiber materials, thereby limiting the industrial production of porous polyurethane fibers. Therefore, the development of green, low-cost, and simple porous polyurethane fiber preparation technology, and the acquisition of excellent porous fiber products with adjustable pore structure are key issues to be solved at this stage. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for preparing porous (homogeneous porous) polyurethane fibers by drying at normal pressure, which is green, environmentally friendly, low-cost and simple in process.
[0006] In order to solve the above technical problems, the present invention provides a method for preparing porous (homogeneous porous) polyurethane fibers (i.e., a method for preparing porous polyurethane fibers by precipitation-induced phase separation), comprising the following steps:
[0007] S1. Preparation of polyurethane spinning solution:
[0008] Adding polyurethane masterbatch into an organic solvent and stirring until completely dissolved, the obtained polyurethane solution is used as a polyurethane spinning solution;
[0009] S2. Preparation of mixed coagulation bath:
[0010] Mixing alcohol and water, stirring evenly, and using the resulting alcohol / water mixture as a mixed coagulation bath (i.e., as a non-solvent for the mixed coagulation bath);
[0011] S3, wet spinning:
[0012] The polyurethane spinning solution obtained in step S1 enters the spinneret at a set injection speed, and then is ejected into the mixed coagulation bath obtained in step S2 for wet spinning to complete phase separation (the solvent in the polyurethane spinning solution is separated from the non-solvent in the mixed coagulation bath), thereby obtaining polyurethane gel fibers; the temperature of the mixed coagulation bath is 30 to 70° C. (preferably 35 to 65° C.);
[0013] Note: The injection speed of the polyurethane spinning solution is controlled by a microfluidic pump, and the spinneret is located in the coagulation bath. This is a conventional technology;
[0014] S4, atmospheric pressure drying
[0015] The polyurethane gel fiber obtained in step S3 is dried under normal pressure to obtain porous (homogeneous porous) polyurethane fiber.
[0016] As an improvement to the preparation method of the present invention: the mass fraction of the polyurethane masterbatch in the polyurethane solution is 5 to 30% (preferably 10 to 30%).
[0017] As a further improvement of the preparation method of the present invention:
[0018] In step S1, the organic solvent is at least any one of the following: dimethylformamide, dimethylacetamide, dimethyl sulfoxide, that is, one or more of dimethylformamide, dimethylacetamide and dimethyl sulfoxide;
[0019] In step S2, the alcohol is at least any one of the following: ethanol, isopropanol, tert-butanol, and the mass concentration of the alcohol in the alcohol / water mixture is 10% to 90% (preferably 30 to 60%).
[0020] As a further improvement of the preparation method of the present invention:
[0021] In step S1, the stirring is performed mechanically at 25-80°C (preferably 30-70°C).
[0022] As a further improvement of the preparation method of the present invention:
[0023] In step S3, the diameter of the wet spinning head is 200-800 μm (preferably 300-700 μm).
[0024] As a further improvement of the preparation method of the present invention:
[0025] In step S3, under the flow rate control of the microfluidic pump, the polyurethane spinning solution enters the spinneret at a push injection rate of 1-10 mL / min (preferably 1.5-5 ml / min), and the collection rate is 20-100 m / min (preferably 10-50 m / min).
[0026] As a further improvement of the preparation method of the present invention:
[0027] In step S4, the atmospheric pressure drying treatment is drying at 40-100° C. for 1-5 h (preferably drying at 50-80° C. for 2-4.5 h).
[0028] As a further improvement of the preparation method of the present invention:
[0029] Polyurethane is thermoplastic polyurethane.
[0030] As a further improvement of the preparation method of the present invention:
[0031] A polyurethane solution with a polyurethane mass fraction of 10% is used as a polyurethane spinning solution;
[0032] A 60% ethanol / water mixture was used as the mixed coagulation bath, and the temperature of the mixed coagulation bath was 65°C.
[0033] The wet spinning of the present invention adopts the precipitation-induced phase separation method to prepare pores; that is, the present invention provides a preparation method for constructing porous polyurethane fibers by atmospheric pressure drying and precipitation-induced phase separation. The present invention is based on wet spinning technology, and the phase separation kinetic diffusion coefficient is regulated by adjusting the non-solvent ratio in the coagulation bath, and porous polyurethane fibers with high elasticity and high thermal insulation properties are prepared after atmospheric pressure drying and shaping. The preparation method of the present invention is simple and easy to implement, convenient for industrial production, and the prepared product has good thermal insulation performance. The homogenized pore structure and high porosity inside the porous polyurethane fiber give the fiber lightness, providing potential applications for thin and light and high thermal insulation textiles, and the method is simple and easy to implement, easy to control, low cost, green and environmentally friendly, and convenient for industrial production.
[0034] The beneficial effects of the present invention are:
[0035] 1. The present invention selects a non-solvent (ethanol / water mixed solution) with low interaction between the solvent and the non-solvent, regulates the kinetic diffusion coefficient in the phase separation process, reduces the generation of macropores, and increases the porosity, thereby constructing a porous (homogeneous porous) polyurethane fiber. The method of the present invention has a short cycle (5-12 hours) and low energy consumption (drying in normal pressure environment).
[0036] 2. The present invention strengthens the porous network structure of polyurethane and resists capillary stress by regulating the coagulation bath temperature.
[0037] 3. The present invention obtains a uniform pore structure by changing the non-solvent ratio and non-solvent temperature in precipitation-induced phase separation.
[0038] In summary, the present invention provides a preparation method and application of porous polyurethane fibers constructed by precipitation-induced phase separation, based on wet spinning technology, by regulating the kinetic diffusion coefficient in the phase separation process, regulating the pores in the solidification process of the fiber in the wet spinning process, and preparing porous (homogeneous porous) polyurethane fibers with high elasticity and high thermal insulation properties by normal pressure drying. The preparation method is simple and easy to implement, easy to regulate, low in cost, green and environmentally friendly, and convenient for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] The specific implementation modes of the present invention are further described in detail below with reference to the accompanying drawings.
[0040] Figure 1 The cross-sectional electron micrograph of the porous polyurethane fiber prepared in Example 1-4;
[0041] Figure 1 In: a to d correspond to Examples 1 to 4 respectively;
[0042] Figure 2 The stress-strain curves of the porous polyurethane fibers prepared in Examples 1 to 4;
[0043] Figure 3 It is a temperature rise curve diagram of Example 1-4 under a heating environment of 35°C. DETAILED DESCRIPTION
[0044] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto:
[0045] The polyurethane masterbatch is 1180A10 model purchased from BASF (China) Co., Ltd., Germany, with a particle size of 2 cm and a specific gravity of polyurethane: 1.11 g / cm 3 , tensile modulus: 12.4MPa, flexural modulus: 17.2MPa. It is thermoplastic polyurethane.
[0046] Example 1: A method for preparing porous polyurethane fibers by precipitation-induced phase separation, comprising the following steps:
[0047] (1) At 30-70° C., 5 g of polyurethane masterbatch was added to 45 g of N,N-dimethylformamide and stirred until the polyurethane masterbatch was completely dissolved to obtain a polyurethane solution with a polyurethane mass fraction of 10%, which was used as the polyurethane spinning solution.
[0048] (2) adding 150 g of ethanol to 350 g of water, stirring at 35° C. for 1 h, to obtain a 30% ethanol / water mixture as a mixed coagulation bath (i.e., as a non-solvent for the mixed coagulation bath);
[0049] (3) Wet spinning:
[0050] Under the flow rate control of the microfluidic pump, the polyurethane spinning solution enters the spinneret at a push injection rate of 1.5 mL / min, and then is ejected into the mixed coagulation bath obtained in step 2) for wet spinning to complete phase separation (the solvent in the polyurethane spinning solution is separated from the non-solvent in the mixed coagulation bath), thereby obtaining polyurethane gel fibers;
[0051] The spinneret diameter is 400 μm (i.e., the fiber diameter formed is 400 μm); the collection rate is 20 m / min; the temperature of the mixing coagulation bath is set to 35°C;
[0052] (4) The phase-separated polyurethane gel fibers were dried at 50° C. under normal pressure for 2 h to obtain porous polyurethane fibers.
[0053] Example 2: A method for preparing porous polyurethane fibers by precipitation-induced phase separation.
[0054] The following changes are made relative to Example 1:
[0055] (2) adding 200 g of ethanol to 300 g of water and stirring at 45° C. for 1 h to obtain a 40% ethanol / water mixture as a mixed coagulation bath;
[0056] In step (3): setting the temperature of the mixed coagulation bath to 45°C;
[0057] The rest is the same as Example 1.
[0058] Example 3: A method for preparing porous polyurethane fibers by precipitation-induced phase separation.
[0059] The following changes are made relative to Example 1:
[0060] (2) Add 250 g of ethanol to 250 g of water, stir at 55° C. for 1 h, and obtain a 50% ethanol / water mixture as a mixed coagulation bath;
[0061] In step (3): setting the temperature of the mixed coagulation bath to 55°C;
[0062] The rest is the same as Example 1.
[0063] Example 4: A method for preparing homogeneous porous polyurethane fibers by precipitation-induced phase separation.
[0064] The following changes are made relative to Example 1:
[0065] (2) adding 300 g of ethanol to 200 g of water and stirring at 65° C. for 1 h to obtain a 60% ethanol / water mixture as a mixed coagulation bath;
[0066] In step (3): setting the temperature of the mixed coagulation bath to 65°C;
[0067] The rest is the same as Example 1.
[0068] Experiment 1: The cross section of the porous polyurethane fibers prepared in Examples 1 to 4 was analyzed; the electron microscope images thereof are shown in FIG. Figure 1 ,according to Figure 1 , it can be known that: Example 1 ( Figure 1 a) A large number of finger-like pores and large cellular pores are generated. As the ethanol content in the coagulation bath increases, the large pores gradually decrease; when the ethanol content is 60% (Example 4, Figure 1 d), there are no macropores inside the fiber, the pore structure is uniform, and homogeneous porous polyurethane fibers are obtained.
[0069] Experiment 2: The porous polyurethane fibers prepared in Examples 1 to 4 were tested according to GB / T 3923.1-2013, and the stress-strain curves thereof are shown in FIG. Figure 2 ,according to Figure 2 It can be seen that: as the macropores inside the porous polyurethane fiber decrease, the fiber elongation at break increases, and the homogeneous porous fiber of Example 4 exhibits the highest elongation at break of 2865%.
[0070] Experiment 3: The porous polyurethane fibers prepared in Examples 1 to 4 were heated at 35°C. The heating curve is shown in FIG. Figure 3 ,according to Figure 3 It can be seen that the temperature differences of the porous polyurethane fibers prepared in Examples 1 to 4 are 3.48, 3.59, 3.71 and 3.85°C, respectively, and the homogeneous porous polyurethane fibers prepared in Example 4 have the highest thermal insulation performance.
[0071] The performance comparison of the above-mentioned embodiments 1 to 4 is shown in Table 1 below:
[0072] Table 1. Statistics of thermal insulation and stress-strain properties of porous polyurethane fibers
[0073]
[0074] Example 5-1: The "dimethylformamide" in Example 4 is replaced by "dimethylacetamide", the dosage remains unchanged, and the rest is the same.
[0075] Example 5-2: The "dimethylformamide" in Example 4 is replaced by "dimethyl sulfoxide", the dosage remains unchanged, and the rest is the same.
[0076] Example 6-1: In Example 4, "ethanol" is replaced with "isopropanol", and the amount used remains unchanged, and the rest is the same.
[0077] Example 6-2: The "ethanol" in Example 4 is replaced with "tert-butyl alcohol", the dosage remains unchanged, and the rest is the same.
[0078] Example 7-1. Replace the "5 g polyurethane masterbatch and 45 g N,N-dimethylformamide" in Example 4 with "2.5 g polyurethane masterbatch and 47.5 g N,N-dimethylformamide" to obtain a polyurethane solution with a mass fraction of 5%; the rest are the same.
[0079] Example 7-2: Change the "5 g polyurethane masterbatch and 45 g N,N-dimethylformamide" in Example 4 to "15 g polyurethane masterbatch and 35 g N,N-dimethylformamide" to obtain a polyurethane solution with a mass fraction of 30%; the rest are the same.
[0080] Example 8-1: Change "the urethane solution enters the spinneret at a push injection rate of 1.5 mL / min" in Example 4 to "the urethane solution enters the spinneret at a push injection rate of 2 mL / min"; the rest are the same.
[0081] Example 8-2: Change "the urethane solution enters the spinneret at a push injection rate of 1.5 mL / min" in Example 4 to "the urethane solution enters the spinneret at a push injection rate of 3 mL / min"; the rest are the same.
[0082] Example 8-3: Change "the urethane solution enters the spinneret at a push injection rate of 1.5 mL / min" in Example 4 to "the urethane solution enters the spinneret at a push injection rate of 5 mL / min"; the rest are the same.
[0083] Example 9-1: Change the "collection rate 20 m / min" in Example 4 to "collection rate 10 m / min"; the rest are the same.
[0084] Example 9-2: Change the "collection rate 20 m / min" in Example 4 to "collection rate 30 m / min"; the rest are the same.
[0085] Example 9-3: Change the "collection rate 20 m / min" in Example 4 to "collection rate 50 m / min"; the rest are the same.
[0086] The above-mentioned Examples 5-1 to 9-3 were tested according to the above experimental method, and the performance comparison of each example is shown in Table 1 below:
[0087] Table 2. Statistics of thermal insulation and stress-strain properties of porous polyurethane fibers
[0088]
[0089] Comparative Example 1-1: The "60% ethanol / water mixture" in Example 4 was changed to "90% ethanol / water mixture", and the rest was the same as Example 4.
[0090] Comparative Example 1-2: The "60% ethanol / water mixture" in Example 4 is changed to "20% ethanol / water mixture", and the rest is the same as Example 4.
[0091] Comparative Example 2-1: The "temperature of the mixed coagulation bath" in Example 4 was changed from 65°C to 75°C, and the rest was the same as Example 4.
[0092] Comparative Example 2-2: The "temperature of the mixed coagulation bath" in Example 4 was changed from 65°C to 25°C, and the rest was the same as Example 4.
[0093] All the comparative examples were tested according to the above experimental method, and the performance comparison with Example 4 is shown in Table 3 below:
[0094] Table 3. Statistics of thermal insulation and stress-strain properties of porous polyurethane fibers
[0095]
[0096] Finally, it should be noted that the above examples are only some specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and there are many variations. All variations that can be directly derived or associated with the content disclosed by a person skilled in the art should be considered as the protection scope of the present invention.
Claims
1. A method for preparing porous polyurethane fiber, characterized in that The following steps are involved: S1. Preparation of polyurethane spinning solution: Adding polyurethane masterbatch into an organic solvent and stirring until completely dissolved, the obtained polyurethane solution is used as a polyurethane spinning solution; S2. Preparation of mixed coagulation bath: mixing alcohol with water, and using the resulting alcohol / water mixture as a mixed coagulation bath; S3, wet spinning: The polyurethane spinning solution obtained in step S1 enters the spinneret at a set injection speed, and then is ejected into the mixed coagulation bath obtained in step S2 for wet spinning to complete phase separation, thereby obtaining polyurethane gel fibers; the temperature of the mixed coagulation bath is 30-70° C.; S4, atmospheric pressure drying The polyurethane gel fiber obtained in step S3 is dried under normal pressure to obtain porous polyurethane fiber.
2. The method for preparing porous polyurethane fiber according to claim 1, characterized in that: The mass fraction of the polyurethane masterbatch in the polyurethane solution is 5-30%.
3. The method for preparing porous polyurethane fiber according to claim 2, characterized in that: In step S1, the organic solvent is at least any one of the following: dimethylformamide, dimethylacetamide, dimethyl sulfoxide; In step S2, the alcohol is at least any one of the following: ethanol, isopropanol, tert-butanol, and the mass concentration of the alcohol in the alcohol / water mixture is 10% to 90%.
4. The method for preparing porous polyurethane fiber according to claim 3, characterized in that: In step S1, the stirring is performed mechanically at 25-80°C.
5. The method for preparing porous polyurethane fiber according to claim 4, characterized in that: In step S3, the diameter of the wet spinning head is 200-800 μm.
6. The method for preparing porous polyurethane fiber according to claim 5, characterized in that: In step S3, the injection speed is 1-10 ml / min, and the collection rate is 20-100 m / min.
7. The method for preparing porous polyurethane fiber according to any one of claims 1 to 6, characterized in that: In step S4, the atmospheric pressure drying treatment is drying at 40-100° C. for 1-5 hours.
8. The method for preparing porous polyurethane fiber according to any one of claims 1 to 7, characterized in that: Polyurethane is thermoplastic polyurethane.
9. The method for preparing porous polyurethane fiber according to any one of claims 1 to 8, characterized in that: A polyurethane solution with a polyurethane mass fraction of 10% is used as a polyurethane spinning solution; A 60% ethanol / water mixture was used as a mixed coagulation bath, and the temperature of the mixed coagulation bath was 65°C.
Citation Information
Patent Citations
Method for improving strength and strain of polyurethane fibers
CN110230117A
Polyurethane / chitosan composite porous fiber and spinning method thereof
CN116732646A
Hollow aerogel fiber and preparation method thereof at normal temperature and normal pressure
CN118127654A
Method of manufacturing polymeric porous hollow fiber membrane
JP2012176409A
Cited By
Superfine aerogel fiber as well as preparation method and application thereof
CN119932733A