Thermal-insulation and anti-cutting aerogel fiber, thermal-insulation and anti-cutting fabric and preparation method and application of thermal-insulation and anti-cutting aerogel fiber
By using polyurethane as a binder to coat SiO2 aerogel on UHMWPE fibers, the insulation and cutting-proof aerogel fiber with a leather core structure is solved, and the problem of insufficient brittleness and insulation performance of SiO2 modified fibers is achieved, and lightness and comfort are achieved And high-performance fiber fabric.
Patent Information
- Application Number
- CN202411203002.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-29
AI Technical Summary
The existing SiO2-modified UHMWPE fabrics are prone to damage during use due to the low strength and high brittleness of silica aerogels, which are easy to damage during use, and the thermal insulation performance is degraded, and the traditional coatings make the fabric thick and uncomfortable.
Polyurethane with higher viscosity is used as a water-insoluble binder to assist SiO2 aerogel to coat ultra-high molecular weight polyethylene fibers to form thermal insulation and anti-cutting aerogel fibers with a leather core structure. Through coaxial wet spinning technology Preparation to form a uniform porous network structure to improve toughness and thermal insulation properties.
Overcome the brittleness problem of SiO2 aerogel, enhance the mechanical properties and thermal insulation properties of the fibers. The fabric is light and comfortable, and has excellent cutting and thermal insulation properties. It is suitable for high-altitude and high-risk environments.
Smart Images

Figure CN118996675A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of textile materials, and specifically relates to a thermal insulation and cut-resistant aerogel fiber with a skin-core structure modified by SiO2 aerogel, a thermal insulation and cut-resistant fabric, and a preparation method and application thereof. Background Art
[0002] Ultra-high molecular weight polyethylene fiber (UHMWPE), as a high-performance fiber made of polyethylene with a molecular weight of more than 1 million through a special spinning and high-ratio drafting process, has become a leader in industrial chemical fibers due to its excellent specific strength characteristics, especially opening up a new way for the manufacture of thin and light cut-resistant and stab-resistant gloves. However, although the current cut-resistant products on the market have made breakthroughs in cut-resistant performance, they generally ignore the comfort of wearing, resulting in problems such as heavy products, inconvenient to wear, and itchy sensations. In response to this problem, Yang Doudou and others used innovative separation weaving and transfer technology, aramid 1414 as the veil, combined with UHMWPE fiber, to successfully weave cut-resistant gloves with a cut resistance level of EN 388 standard 5, significantly improving the cut-resistant performance. However, it is worth noting that while pursuing high cut-resistant performance, the lightness and aesthetics of the gloves have not yet been systematically and comprehensively optimized.
[0003] On the other hand, hand protection equipment in high-altitude cold regions traditionally relies on heavy animal fur, which is particularly inconvenient in professional mechanical operations and delicate operations, and it is difficult to meet the operational requirements in extreme environments. The thermal insulation fabrics currently on the market are generally made of traditional filling materials such as cotton and down. Although these fabrics can provide a certain warmth effect, they lack cut resistance, and their flammable properties make them unsuitable for military and high-risk environments. Silica aerogel is a porous material with extremely low thermal conductivity and high specific surface area. Fabrics coated with silica aerogel coating on the surface of UHMWPE fabrics can enhance their cut resistance and give UHMWPE fabrics certain thermal insulation properties. At present, some products have tried to enhance the thermal insulation performance by coating silica aerogel coating on the surface of fabrics. However, due to the brittleness of aerogel itself, these coatings are often easy to break when subjected to force, causing the silica aerogel coating on the surface of the fabric to fall off, affecting the appearance and weakening the thermal insulation effect of the fabric. Although the silica-modified fabric may still have a certain cut-resistant capability due to the properties of UHMWPE itself, the comprehensive thermal insulation and cut-resistant properties of this type of fabric will be affected. Summary of the invention
[0004] The present invention is based on the inventor's discovery and understanding of the following facts and problems: In the prior art, SiO2-modified UHMWPE fabrics are easily damaged during use and their thermal insulation performance is reduced due to the low strength and high brittleness of silica aerogel.
[0005] The present invention aims to solve one of the technical problems in the related art to a certain extent. To this end, the present invention proposes a SiO2 aerogel-modified UHMWPE fiber and a preparation method thereof, and develops a light and thin fiber product with good cut-resistant and heat-insulating properties.
[0006] The first purpose of the present invention is to provide a thermal insulation and cut-resistant aerogel fiber, comprising a core yarn and a sheath-core coated on the surface of the core yarn; the core yarn is UHMWPE, and the components of the sheath-core include SiO2 aerogel and a non-water-soluble binder.
[0007] Since SiO2 aerogel is not sticky, it is impossible to use it as a single component of the skin-core coated on the surface of the ultra-high molecular weight polyethylene core yarn. Therefore, it is necessary to select a viscous substance as a binder to assist SiO2 in coating the ultra-high molecular weight polyethylene core yarn. In some embodiments of the present invention, polyurethane with higher viscosity is used as a binder to successfully prepare a thermal insulation fiber with a skin-core structure. It can be seen from the SEM photos that the skin-core has a uniform porous network structure. On the one hand, the porous network structure can disperse the stress and energy when the fiber is stressed, hinder crack propagation, reduce brittleness, improve toughness, and optimize the mechanical properties of the skin-core. On the other hand, it can slow down the transfer of heat and optimize thermal insulation performance. This is one of the inventive points of the present invention. The aerogel fiber fabric prepared using this fiber overcomes the shortcomings of the traditional coating on the fabric that makes the fabric thick and uncomfortable, and also has the characteristics of being light, thin and comfortable.
[0008] Preferably, the diameter of the core yarn composed of UHMWPE is 11.1 to 13.1 μm;
[0009] Preferably, the molecular weight of UHMWPE is 1 million to 5 million, and the fineness is 800D;
[0010] Preferably, the mass ratio of SiO2 aerogel to water-insoluble binder in the skin-core component is (2-4):(4-6).
[0011] Preferably, the thickness of the skin-core is 5-10 μm;
[0012] Preferably, the non-water-soluble binder is polyurethane.
[0013] The second object of the present invention is to provide a method for preparing the above-mentioned thermal insulation and cut-resistant aerogel fiber, which specifically comprises the following steps:
[0014] Step 1, preparing SiO2 aerogel / PU spinning solution, specifically: mixing PU particles and SiO2 aerogel powder as solutes with a solvent, stirring at room temperature until the PU particles and SiO2 aerogel powder are completely dissolved to form a SiO2 aerogel / PU spinning solution.
[0015] Step 2, the SiO2 aerogel / PU spinning solution prepared in step 1 and the core yarn are coaxially wet-spinned to obtain thermal insulation and cut-resistant aerogel fibers.
[0016] One of the inventive points of the present invention is to use SiO2 aerogel for thermal insulation to directly modify UHMWPE to obtain composite fibers with thermal insulation and cut-resistant properties.
[0017] Preferably, in step 1, the mass concentration of the solute is 12% to 15%;
[0018] Preferably, in step 1, the size of the SiO2 aerogel powder is less than 100 nm;
[0019] Preferably, in step 1, the solvent is selected from N,N-dimethylformamide, butanone, cyclohexanone, acetone, ethyl acetate or toluene;
[0020] Preferably, in step 2, the speed of the injection pump to extrude the spinning solution is 100-140 ml / hr; and the coagulation bath selected for wet spinning is deionized water.
[0021] The third aspect of the present invention is to disclose a thermal insulation and cut-resistant fabric woven using the thermal insulation and cut-resistant aerogel fiber or the thermal insulation and cut-resistant aerogel fiber prepared by the above-mentioned preparation method.
[0022] The fourth aspect of the present invention discloses the application of the thermal insulation and cut-resistant aerogel fiber and the thermal insulation and cut-resistant fabric in the field of textile material technology.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The present invention provides a thermal insulation and cut-resistant fiber. By mixing SiO2 aerogel with a non-water-soluble binder and modifying UHMWPE fiber through coaxial wet spinning technology, an aerogel fiber with both cut-resistant and thermal insulation properties is obtained. The fiber has a uniform surface, and SiO2 aerogel is distributed in the skin and core to form a uniform three-dimensional porous structure. The modified UHMWPE fiber has excellent mechanical properties. When the woven fabric is actually used, on the one hand, it overcomes the brittleness of SiO2 aerogel material and is not easy to fall off. At the same time, it can give full play to the thermal insulation performance of SiO2 aerogel and effectively block the loss of heat, so that the fabric can be used in an environment with special requirements for cut-resistant and thermal insulation performance. While ensuring protection, it can also have the effect of thermal insulation and heat storage. It can be applied to various fields with high risk factors of scratches and cuts, and can also improve the safety protection of workers in high-cold working conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 A diagram showing a schematic diagram of preparing SiO2 aerogel / PU composite fibers and PU composite fibers by wet spinning according to the present invention;
[0026] Figure 2 It is a plain weave pattern plate diagram of an embodiment;
[0027] Figure 3 The SEM images of the PU composite fibers prepared in the embodiment of the present invention are as follows: (a) fiber cross section, (b) enlarged view of the skin-core part;
[0028] Figure 4 SEM images of SiO2 aerogel / PU composite fibers prepared in an embodiment of the present invention, (a) fiber cross section, (b) enlarged view of the skin-core part;
[0029] Figure 5 Elemental energy spectrum diagram of PU composite fiber prepared in the embodiment of the present invention, (a) is a photo of the selected area, (b) is a C, N, O, Si element distribution contrast photo, (c) is a C, N, O, Si element distribution energy spectrum diagram;
[0030] Figure 6 Elemental energy spectrum diagram of SiO2 aerogel / PU composite fiber prepared in an embodiment of the present invention, (a) is a photo of the selected area, (b) is a C, N, O, Si element distribution contrast photo, (c) is a C, N, O, Si element distribution energy spectrum diagram;
[0031] Figure 7 SiO2 aerogel / PU composite fiber fabric (a) and PU composite fiber fabric (b) prepared in accordance with an embodiment of the present invention;
[0032] Figure 8 PU composite fiber fabric (left) and SiO2 / PU composite fiber fabric (right), (a), (b), (c) are single-layer, 3-layer, and 5-layer fabrics respectively;
[0033] Fig. 9 Comparison of thermal insulation performance between single-layer PU composite fiber fabric (left) and single-layer SiO2 aerogel composite fiber fabric (right). The heating stage temperatures in (a), (b), (c), and (d) are 40°C, 60°C, 80°C, and 100°C, respectively.
[0034] Fig.10 Comparison of thermal insulation performance between 3-layer PU composite fiber fabric (left) and SiO2 aerogel composite fiber fabric (right). The temperatures in (a), (b), (c), and (d) are 40℃, 60℃, 80℃, and 100℃, respectively.
[0035] Fig.11 Comparison of thermal insulation performance between 5-layer PU composite fiber fabric (left) and SiO2 aerogel composite fiber fabric (right). The temperatures of the hot plate in (a), (b), (c), and (d) are 40℃, 60℃, 80℃, and 100℃, respectively.
[0036] Fig.12 Analysis of test data of thermal insulation performance of fabrics with different numbers of layers: (a) Comparison of thermal insulation performance of single-layer fabrics; (b) Comparison of thermal insulation performance of 3-layer fabrics; (c) Comparison of thermal insulation performance of 5-layer fabrics; (d) Comparison of temperature difference of fabrics with different numbers of layers;
[0037] Fig.13 The pictures of different types of gloves are as follows: (a) SiO2 aerogel / PU composite fabric gloves, (b) foamed terry gloves, (c) nitrile gloves, (d) dotted cotton gloves, (e) nylon latex gloves, and (f) spandex tire rubber gloves.
[0038] Fig.14 Depth of field diagram of the fracture morphology after the gloves were cut, (a) SiO2 aerogel / PU composite fabric gloves, (b) foamed terry gloves, (c) nitrile gloves, (d) dotted cotton gloves, (e) nylon latex gloves, (f) spandex tire rubber gloves;
[0039] Fig.15 Data analysis of cut resistance performance of different types of gloves. DETAILED DESCRIPTION
[0040] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0041] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0042] The present invention mainly adopts ultra-high molecular weight polyethylene fiber with a fineness of 800D, and uses a wet spinning machine to spin SiO2 aerogel / PU composite fibers respectively; and uses a semi-automatic sample loom to weave two types of cloth samples with a specification of 6×6 cm, and uses a testo 872 infrared thermal imager to measure the thermal insulation performance of the fabric, and compares the difference in thermal insulation performance between PU composite fiber fabric and SiO2 aerogel / PU composite fiber fabric; uses a QC-200A anti-cut glove testing machine to test the gloves woven with SiO2 aerogel / PU composite fibers prepared by the present invention and other types of labor protection gloves on the market, and compares the anti-cut performance of different types of gloves. By recording the number of cutting revolutions required for the gloves to be cut, the protective gloves with the best anti-cut performance are judged, which proves that the SiO2 aerogel / PU composite fibers prepared by the present invention have excellent anti-cut performance.
[0043] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0044] Example 1
[0045] The SiO2 aerogel / PU composite fibers and SiO2 aerogel / PU composite fiber fabrics were prepared according to the following steps:
[0046] Step 1, prepare SiO2 aerogel / PU composite fiber spinning solution: first weigh 5g PU particles and 44g N,N-dimethylformamide (DMF) solvent and add them to a reagent bottle; then weigh 3g SiO2 aerogel powder with weighing paper, slowly add the powder to the DMF solution containing PU particles (SiO2 powder is a lightweight nano solid material, and the powder must be prevented from scattering when added), and add a magnetic rotor at the same time. Stir on a magnetic stirrer at room temperature for 8h until the PU particles are completely dissolved and the SiO2 aerogel powder is evenly dispersed in the solution, so as to obtain a SiO2 aerogel / PU dispersion with a concentration of 15%. Finally, the obtained solution is placed in an ultrasonic cell crusher for ultrasonic oscillation for 10min to fully dissolve the nano-scale SiO2 aerogel powder in the solution for subsequent spinning.
[0047] Step 2, preparation of SiO2 aerogel / PU composite fiber: Use the wet spinning machine method to prepare the skin-core structure SiO2 aerogel / PU composite fiber with cross-linked skin. The small wet spinning machine was purchased from Changsha Nayi Instrument Technology Co., Ltd. The device mainly includes: an injection pump for spinning solution extrusion, a coagulation bath and a fiber drawing and collection winding device, and a customized coaxial spinning needle (18G+13G). The coagulation bath uses laboratory-made deionized water. First, insert the UHMWPE fiber with a fineness of 800D into the coaxial wet spinning needle, fix its head end on the collecting roller, and then inject an appropriate amount of spinning solution with a syringe and combine it on the injection pump. Adjust the extrusion speed of the injection pump. Generally, the speed is controlled at 120ml / hr so that the spinning solution is slowly extruded and evenly wrapped on the surface of the UHMWPE fiber to form a skin-core structure SiO2 aerogel / PU composite fiber with cross-linked skin. Finally, the fiber is collected on the collecting roller and dried at room temperature. Schematic diagram of the specific preparation process of wet spinning, such as Figure 1 shown.
[0048] Step 3, prepare SiO2 aerogel / PU composite fiber fabric: weave the SiO2 aerogel / PU composite fiber obtained in the above steps on a sample loom. First, unwind the yarn. Cut the corresponding warp SiO2 aerogel / PU composite fiber yarn into the required length according to the required length of the woven fabric, and determine the number of warp yarns according to the designed warp density and fabric width. Then warp the unwinded yarns separately, and thread the obtained regular fiber bundles according to the change law of the plain weave. Calculate the required reed number by the size of the warp density, select the appropriate reed number, thread and organize, and use a small weft tube to wind an appropriate amount of weft yarn for beating. After completing the threading step, enter the plain weave pattern card on the control panel of the sample loom. The plain weave pattern card is as shown in the figure below: Figure 2 As shown, the air compressor is turned on, and weaving is performed according to the steps of shuttle opening, weft insertion, and weft beating. The weaving process is repeated until the fabric reaches a predetermined weaving length, and finally a SiO2 aerogel / PU composite fiber fabric is obtained.
[0049] Example 2
[0050] The SiO2 aerogel / PU composite fibers and SiO2 aerogel / PU composite fiber fabrics were prepared according to the following steps:
[0051] Step 1, prepare SiO2 aerogel / PU composite fiber spinning solution: first weigh 4g PU particles and 44g butanone as solvent and add them to a reagent bottle; then weigh 2g SiO2 aerogel powder with weighing paper, slowly add the powder to the PU-butanone solution containing PU particles (SiO2 powder is a lightweight nano solid material, and the powder must be prevented from scattering when added), and add a magnetic rotor at the same time. Stir on a magnetic stirrer at room temperature for 8h until the PU particles are completely dissolved and the SiO2 aerogel powder is evenly dispersed in the solution, so as to obtain a SiO2 aerogel / PU dispersion with a concentration of 12%. Finally, the obtained solution is placed in an ultrasonic cell crusher for ultrasonic oscillation for 10min to fully dissolve the nano-scale SiO2 aerogel powder in the solution for subsequent spinning.
[0052] Step 2, the step of preparing SiO2 aerogel / PU composite fiber is the same as step 2 of Example 1.
[0053] Step 3, the step of preparing SiO2 aerogel / PU composite fiber fabric is the same as step 3 of Example 1, to obtain SiO2 aerogel / PU composite fiber fabric.
[0054] Example 3
[0055] The SiO2 aerogel / PU composite fibers and SiO2 aerogel / PU composite fiber fabrics were prepared according to the following steps:
[0056] Step 1, prepare SiO2 aerogel / PU composite fiber spinning solution: first weigh 6g PU particles and 61.43g toluene as a solvent and add them to a reagent bottle; then weigh 4g SiO2 aerogel powder with weighing paper, slowly add the powder to the PU-toluene solution containing PU particles, and add a magnetic rotor at the same time, stir on a magnetic stirrer at room temperature for 8h until the PU particles are completely dissolved and the SiO2 aerogel powder is evenly dispersed in the solution, thus obtaining a SiO2 aerogel / PU dispersion with a concentration of 14%, and finally place the obtained solution into an ultrasonic cell crusher for ultrasonic oscillation for 10min to fully dissolve the nano-scale SiO2 aerogel powder in the solution for subsequent spinning.
[0057] Step 2, the step of preparing SiO2 aerogel / PU composite fiber is the same as step 2 of Example 1.
[0058] Step 3, the step of preparing SiO2 aerogel / PU composite fiber fabric is the same as step 3 of Example 1, to obtain SiO2 aerogel / PU composite fiber fabric.
[0059] Comparative Example 1
[0060] The PU composite fibers and PU composite fabrics were prepared according to the following steps:
[0061] Step 1, prepare PU composite fiber spinning solution: weigh 5g PU particles and 28g N,N-dimethylformamide (DMF) solution and add them into a reagent bottle; stir with a magnetic stirrer at room temperature for 8h until the PU particles are completely dissolved, and a transparent pure PU dispersion with a concentration of 15% can be obtained for subsequent spinning.
[0062] Step 2, the step of preparing PU composite fiber is the same as step 2 of Example 1.
[0063] Step 3, the step of preparing the PU composite fabric is the same as step 3 of Example 1, to obtain the PU composite fabric.
[0064] The performance comparison involved in the following tests all used the SiO2 aerogel / PU composite fiber prepared in Example 1 and the PU composite fiber prepared in Comparative Example 1.
[0065] Test Example 1
[0066] Scanning electron microscope characterization: 3 cm SiO2 aerogel / PU composite fiber and PU composite fiber were cut and immersed in liquid nitrogen for quick freezing, and then the cut fiber was quickly cut from the middle with a blade to obtain the complete cross section of the fiber. The cut fiber was glued to the side of the sample stage with conductive glue to observe the complete cross-sectional morphology, and then it was sprayed with gold. The sample stage was placed in a scanning electron microscope (SEM), and under the condition of an acceleration voltage of 10-20 kV, it was observed and photographed according to the required requirements, magnification, and desired cross section.
[0067] The microstructure of pure PU fiber and SiO2 aerogel / PU composite fiber was observed by SEM. Figure 3 This is the SEM photo of PU composite fiber. Figure 4 is the SEM photo of SiO2 aerogel / PU composite fiber. It can be observed that Figure 3 (a) and Figure 4 In (a), both the PU composite fiber and the SiO2 aerogel / PU composite fiber have obvious skin-core structures. The core yarn UHMWPE fiber bundle is tightly wrapped by the skin core, the core yarn UHMWPE fiber bundle is regularly arranged, and the cross section of a single UHMWPE fiber is a smooth elliptical surface, while the cross section of the skin core is rough and irregularly distributed. The SEM photos of the skin core of the PU composite fiber and the skin core of the SiO2 aerogel / PU composite fiber are shown in Figure 1. Figure 3 (b) and Figure 4 As shown in (b). Due to factors such as uneven spinning solution extrusion and insufficient fiber coagulation in the coagulation bath during the spinning process, the thickness of the UHMWPE fiber bundle wrapped in the core yarn is not uniform. The core layer of the PU composite fiber is further magnified and observed, as shown in Figure 3As shown in (b), it is found that the cortex of the PU composite fiber is attached with a smooth and irregularly distributed PU film, and gaps between the solutions form voids of various shapes and sizes;
[0068] and Figure 4 (b) shows the SiO2 aerogel / PU composite skin layer, whose surface has many densely packed small holes, forming a randomly arranged porous structure. The irregular porous structure distribution of the skin-core is because the skin-core contains SiO2 aerogel nanopowder, which is a very excellent lightweight nanoporous amorphous solid material. Part of the air can be stored in its pores to reduce heat loss and achieve a thermal insulation effect.
[0069] Test Example 2
[0070] X-ray photoelectron spectroscopy characterization: X-ray photoelectron spectrometer (XPS) was used to characterize the changes in the surface chemical composition and group composition of SiO2 aerogel / PU composite fibers and PU composite fibers. The matching analysis software Advantage was used to perform peak fitting processing on the Si element spectrum, and the changes in the functional groups on the fiber surface were analyzed based on the presence or absence of spectrum peaks and the peak area.
[0071] In order to further explore whether the SiO2 aerogel powder was successfully attached to the fiber surface, energy spectrum scanning was performed on some positions of the cross section of the PU composite fiber and the SiO2 aerogel / PU composite fiber, such as Figure 5 and Figure 6 As shown in the figure, C, N, O, and Si elements can be detected by the spectrometer on SiO2 aerogel / PU composite fibers and PU composite fibers. C, O, and N elements are more distributed on the two types of fibers, with the C content of about 60% and the O content of about 30%. Due to the different PU contents, the N content is higher in the PU composite fibers, about 5%, and the content in the SiO2 aerogel / PU composite fibers is about 2%. These are common elements of ultra-high molecular weight polyethylene and PU. The Si content in the PU composite fibers is only 0.04%, which is negligible, but the content in the SiO2 aerogel / PU composite fibers is as high as 17.24%, indicating that the SiO2 aerogel is successfully attached to the surface of the core yarn UHMWPE fiber bundle, and from Figure 6 It can be seen that the Si element is evenly distributed on the surface of the core yarn UHMWPE fiber bundle.
[0072] Test Example 3
[0073] Morphological structure analysis of SiO2 aerogel / PU composite fabric: The fabric woven by a semi-automatic sample loom has a specification of 6×6cm, a warp and weft density of 100 strands / 5cm, and a reed number of 40.
[0074] Both SiO2 aerogel / PU composite fabric and PU composite fabric are woven in plain weave. When beating the weft, the weft yarn has the most contact points with the reed and is subjected to the greatest force, so as to ensure that the fabric structure is tight and not easy to be snagged, the fabric surface is stiff and flat, and the front and back sides have the same appearance. Figure 7 As shown in the figure, SiO2 aerogel / PU composite fabric is tighter than PU composite fabric, and the mixture of PU and SiO2 aerogel improves the mechanical properties of the thermal insulation and cut-resistant fiber cortex, overcomes the poor processing performance of SiO2 aerogel, and inevitably causes irreversible structural collapse during actual application, resulting in the loss of thermal insulation performance, thus overcoming the limitations of its application in thermal insulation textiles.
[0075] Test Example 4
[0076] Infrared thermal imager characterization: The thermal insulation performance of the fabric was measured using a testo 872 infrared thermal imager. At room temperature, the temperature of the heating platform was raised from 0°C to 40°C and stabilized for 5 minutes to allow the surface of the heating platform to be heated evenly. The surface temperature of the SiO2 aerogel / PU composite fabric and the PU composite fabric placed on the heating platform at 40°C was recorded with an infrared thermal imager and photographed to test their thermal insulation performance at high temperatures. After the test, the thermal insulation performance of the fabric was tested at 60°C, 80°C, and 100°C in the same manner, photographed and recorded, and compared and analyzed.
[0077] SiO2 aerogel has excellent thermal insulation properties. Theoretically, SiO2 aerogel / PU composite fabric made of SiO2 aerogel should also have excellent thermal insulation properties, making it applicable to the field of thermal protection. To explore the thermal insulation properties of the fabric made in this study, the fabric is shown in the figure below. Figure 8 As shown. The single-layer SiO2 aerogel / PU composite fabric and the PU composite fabric were placed on the heating table at the same time, and the testo 872 infrared thermal imager was used to measure the temperature of the single-layer SiO2 aerogel / PU composite fabric and the PU composite fabric as the heating table was heated from 0°C to 40°C and maintained for 5 minutes. The temperature of the two types of fabrics was recorded and photographed. Then the temperature was gradually increased, and a test was performed every 20°C. Photos were taken and data were recorded until the surface temperature of the fabric changed when the temperature was increased to 100°C, as shown in the figure. Fig. 9As shown in the figure, the sample on the left is a single-layer PU composite fabric, and the sample on the right is a single-layer SiO2 aerogel / PU composite fabric. The surface temperature of the two types of fabrics gradually increases with the increase of the temperature of the heating platform. When the heating platform is heated to 100°C, the surface temperature of the SiO2 aerogel / PU composite fabric is only 69.1°C, with a temperature difference of 30.9°C from the heating platform; the surface temperature of the PU composite fabric is 75.8°C, with a temperature difference of 24.2°C from the heating platform. The temperature difference between the two fabrics is 6.7°C, indicating that the thermal insulation performance of the SiO2 aerogel / PU composite fabric is better than that of the PU composite fabric, and it has good thermal insulation performance in high temperature environments.
[0078] In order to further explore the thermal insulation performance of SiO2 aerogel / PU composite fabric, the number of fabric layers was increased and the thickness of the fabric was increased to explore the effect of fabric thickness on thermal insulation performance. 3-layer and 5-layer SiO2 aerogel / PU composite fabric and PU composite fabric were placed on the heating table respectively. Fig.10 , Fig.11 As shown. According to the test method of single-layer fabric, the tests were carried out in sequence, and the surface temperature changes were photographed and recorded. When the temperature of the heating table rose to 100℃ and there were 3 layers of fabric for comparison, the surface temperature of SiO2 aerogel / PU composite fabric was only 51.1℃, with a temperature difference of 48.9℃ from the heating table; the surface temperature of PU composite fabric was 58.5℃, with a temperature difference of 41.5℃ from the heating table, and the temperature difference between the two fabrics was 7.4℃; when the temperature of the heating table rose to 100℃ and there were 5 layers of fabric for comparison, the surface temperature of SiO2 aerogel / PU composite fabric was only 42.6℃, with a temperature difference of 57.4℃ from the heating table; the surface temperature of PU composite fabric was 51.2℃, with a temperature difference of 48.8℃ from the heating table, and the temperature difference between the two fabrics was 8.6℃. This result shows that the thermal insulation performance is significantly enhanced with the increase of fabric thickness. This is because with the increase of fabric thickness, in addition to the inherent thermal insulation performance of the fabric itself, the air layer between the fabrics also blocks part of the heat conduction, thereby improving the thermal insulation performance of multi-layer aerogel woven fabrics. The test temperatures of SiO2 aerogel / PU composite fabrics and PU composite fabrics with different layers and the temperature difference between them are statistically calculated and a statistical chart is made as shown in the figure. Fig.12 As shown in the figure, it can be clearly seen that the surface temperature of SiO2 aerogel / PU composite fabric is always lower than that of PU composite fabric. At the same time, the increase in fabric thickness also reduces the surface temperature of SiO2 aerogel / PU composite fabric, and the temperature difference between the heating platform and the PU composite fabric gradually increases, indicating that the thermal insulation performance of SiO2 aerogel / PU composite fabric is excellent.
[0079] Test Example 5
[0080] QC-200A Cut Resistant Gloves Tester Characterization
[0081] First, put different types of gloves into the fixture as required, and clamp the aluminum foil on the glove with the red clamp of the signal line, and clamp the aluminum foil inside the glove with the other black clamp. Turn on the power switch, press the down button, and adjust the tool to a suitable height. Push the fixture horizontally into the fixture support plate, align the center of the first slot of the fixture with the blade of the tool, and lock the fixture with the fixture locking button.
[0082] Set the parameters required for the test: the initial load is set to 50N, the slow speed is 100mm / min, and the blade speed is 20rpm. Press the load key, and when the force value displayed on the display reaches the set value, press the cutting key first, and the cutting test begins. The display shows the force value and cutting cycle number at any time. When cutting through occurs, the test machine stops cutting and automatically drops a distance of 15mm. Repeat the above steps to test and record the data.
[0083] The cut-resistant performance of gloves made of SiO2 aerogel / PU composite fiber was tested and compared with that of different types of labor protection gloves purchased on the market. Fig.13 As shown. Different types of gloves are cut into samples with a specification of 5×5cm. The QC-200A anti-cut glove testing machine is used. First, the fabric is placed in the fixture. A rubber plate with insulating current is placed on the top of the clamp. A layer of aluminum foil is placed on the rubber plate. Then the sample is placed on it and a layer of aluminum foil is placed on the sample. The fixture is tightened with force to prevent the sample from slipping and causing errors. The loading force value of the instrument is set to 50N. The loading part uses a wide-band AC servo motor to load through the transmission screw. The blade speed is set to 20rpm and the slow speed is 100mm / min. The blade is driven by the AC servo motor through the gear speed change. After setting the parameters, start the equipment. As the blade rotates at a uniform speed, the fabric is gradually cut until a port appears on the fabric. The test is over and the fabric sample begins to fracture. The fracture shape is as follows Fig.14 shown.
[0084] from Fig.14 It can be seen from (a)-(f) that all types of gloves are cut by the cutting blade, but the shapes after cutting are different and the number of continuous cutting times during the cutting process is different. The cutting revolutions per unit mass of the SiO2 aerogel / PU composite fabric sample with a specification of 5×5cm are more than the cutting revolutions of other types of labor protection gloves, as shown in Table 3-1. At the same time, the surfaces of other labor protection gloves have elastic coatings of different thicknesses. The addition of coatings can bring wear resistance and cut resistance to the gloves, but it can be seen from the test results that the cut resistance of coated gloves is far inferior to that of SiO2 aerogel / PU composite fabric gloves, indicating that SiO2 aerogel / PU composite fabric gloves have good cut resistance. SiO2 aerogel / PU composite fibers have high strength and high modulus and excellent cut resistance, such as Fig.15 shown.
[0085] In summary, according to the number of cutting revolutions required for different types of gloves to be cut, the order of the gloves' anti-cutting performance is as follows: SiO2 aerogel / PU composite fabric gloves > nylon latex gloves > spandex tire rubber gloves > foam terry gloves > nitrile gloves > dotted cotton gloves.
[0086] Table 3-1 Test data of cut resistance performance of different types of gloves
[0087]
[0088] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A thermal insulation and cut-resistant aerogel fiber, characterized in that: It comprises a core yarn and a sheath-core coated on the surface of the core yarn; the core yarn is ultra-high molecular weight polyethylene fiber; the components of the sheath-core include SiO2 aerogel and a non-water-soluble adhesive.
2. The thermal insulation and cut-resistant aerogel fiber according to claim 1, characterized in that: The mass ratio of the SiO2 aerogel to the non-water-soluble binder is (2-4):(4-6).
3. The heat-insulating and cut-resistant aerogel fiber according to claim 1, characterized in that: The molecular weight of the ultra-high molecular weight polyethylene is 1 million to 5 million.
4. The heat-insulating and cut-resistant aerogel fiber according to claim 1, characterized in that: The non-water-soluble binder is polyurethane.
5. The heat-insulating and cut-resistant aerogel fiber according to claim 1, characterized in that: The core yarn has a diameter of 11.1 to 13.1 μm.
6. The heat-insulating and cut-resistant aerogel fiber according to claim 1, characterized in that: The thickness of the skin-core is 5-10 μm.
7. A method for preparing the thermal insulation and cut-resistant aerogel fiber according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step 1, mixing SiO2 aerogel and a non-water-soluble binder as a solute with a solvent to obtain a spinning solution, wherein the mass concentration of the solute is 12% to 15%; Step 2: Coaxially wet-spin the spinning solution and the core yarn to obtain the thermal insulation and cut-resistant aerogel fiber.
8. The method for preparing the thermal insulation and cut-resistant aerogel fiber according to claim 7, characterized in that: The solvent in step 1 is selected from N,N-dimethylformamide, butanone, cyclohexanone, acetone, ethyl acetate or toluene.
9. A thermal insulation and cut-resistant fabric, characterized in that: It is made by weaving the thermal insulation and cut-resistant aerogel fiber according to any one of claims 1 to 6.
10. Use of the thermal insulation and cut-resistant aerogel fiber according to any one of claims 1 to 6 or the thermal insulation and cut-resistant fabric according to claim 9 in the field of textile material technology.
Citation Information
Patent Citations
Cutting-resistant ultra high molecular weight polyethylene fiber, preparation method and application thereof
CN106350882A
Aerogel modified glue solution and preparation method thereof
CN112724908A
Thermal-insulation cut-resistant fabric and preparation method thereof
CN117418346A
Aerogel fiber as well as preparation method and application thereof
CN117604679A
Laminate structure and wearable article
GB201802895D0
Cited By
Aerogel heat preservation yarn and preparation method and application thereof
CN119321013A