Sizing-agent-free carbon fiber based on difunctional diazonium salt modification as well as preparation method and application of sizing-agent-free carbon fiber
Through the dual-function diazon salt modification technology, electrochemical reduction and grafting and heat treatment form covalent bonds, solving the complexity and stability of interface modification between polyether ether ketone and carbon fiber, and achieving improvements in interface strength and corrosion resistance .
Patent Information
- Application Number
- CN202410933282.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-22
AI Technical Summary
In the interface modification between polyether ether ketone and carbon fiber, the prior art has problems such as complex chemical treatment, harsh reaction conditions and low stability at high temperatures, resulting in insufficient interface strength and corrosion resistance.
By using the bifunctional diazon salt modification method, the diazon salt with bridged functional groups is grafted onto the surface of carbon fiber through electrochemical reduction, and bridged with polyether ether ketone resin after heat treatment to form covalent bonds and strengthen Interface strength and resist erosion from harsh environments.
The interface processing process is simplified, complex equipment and harsh conditions are avoided, and the efficient interface combination of carbon fiber and polyether ether ketone resin is achieved, improving interface strength and harsh environmental resistance.
Smart Images

Figure CN118996849A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of carbon fiber surface treatment, and specifically relates to a sizing agent-free carbon fiber modified based on a bifunctional diazonium salt, a preparation method and application thereof, and especially relates to the application of the carbon fiber in reinforcing a polyaryletherketone resin-based composite material. Background Art
[0002] The interface enhancement between polyetheretherketone (PEEK) and carbon fiber is a key topic in composite material research. In order to improve the interface strength between polyetheretherketone and carbon fiber, researchers have conducted multi-faceted research. A large amount of work has been reported from the perspectives of wetting, mechanical locking, interface crystallization, secondary bond / chemical bond combination, diffusion, etc., which greatly improved the interface effect and strength between the two. Looking at the current carbon fiber interface modification schemes, the modification scheme based on sizing agent has obvious advantages due to its simple operation and convenient preparation. However, in the interface modification of PEEK / CF, due to the excellent solvent resistance of PEEK, it becomes particularly difficult to prepare the sizing agent without changing the chemical structure of PEEK, and complex chemical treatment is often required. The large amount of chemical solvents in the sizing process is also a huge challenge. Chemical bond combination can form a strong interaction force, which can theoretically provide the best modification effect. However, the traditional chemical bond modification interface strategy also has a series of problems. First, due to the inert structure of carbon fiber and PEEK, complex chemical modification is required to provide active reaction sites; second, the chemical bonds commonly used in interface modification, such as ester groups and amide structures, require relatively harsh conditions to generate; finally, whether these chemical bonds can stably exist at the high processing temperature of polyetheretherketone composite materials is also a problem that must be paid attention to. Therefore, finding a simple, efficient and easy interface treatment strategy has become the key to interface research.
[0003] Diazonium salt grafting is one of the interface modification methods that has received attention in recent years. It uses the amino group in the aniline structure to react with the nitrite structure to obtain a diazo structure, which can obtain electrons on the surface of the electrified carbon fiber and remove the diazo structure to generate a phenyl radical that is grafted onto the carbon fiber surface. Grafting with diazonium salts has good reaction efficiency, fast reaction speed and mild reaction conditions.
[0004] Patent CN 116623425 A discloses a method of preparing a carbon fiber sizing agent by combining hydroxylated boron nitride and hydroxylated carbon nanotubes as raw materials, combining the two into one through an esterification reaction, and combining with a polyetherimide sizing agent. However, the filler treatment required by this method is relatively cumbersome, and the conditions for the esterification reaction are relatively harsh. In addition, since the polyetherimide sizing agent that wraps the carbon fiber is dissolved in an organic solvent, this also causes the interface to fail easily under harsh environments.
[0005] Patent CN 115125735 B discloses a method for modifying sulfonated polyetheretherketone aqueous sizing agent using acidified carbon nanotubes, but this method requires sulfonation of polyetheretherketone and acidification of carbon nanotubes. In addition, sulfonation makes polyetheretherketone soluble in organic solvents, which easily leads to interface failure when corroded.
[0006] Patent CN 111472172 A discloses an amino-modified polyetheretherketone water-based sizing agent obtained by copolymerizing aminobisphenol monomers with fluoroketone monomers. However, the synthesis of amino polymer monomers is relatively complicated and difficult to apply on a large scale. In addition, the amino structure has low stability at high temperatures and is difficult to resist corrosion from organic solvents.
[0007] Patent CN 110924162 B discloses a method for preparing a sizing agent by compounding a soluble ketimine polyaryletherketone with a reinforcing material. After the sizing agent is coated on the surface of the carbon fiber, it needs to be acidified to remove the aniline side groups and restore the crystallization ability. Although this strategy restores the crystallinity of the sizing agent to resist the erosion of organic solvents, it requires a long-term treatment with an acid solution, which is not conducive to large-scale continuous production.
[0008] Patent CN 110820315 B discloses a method for modifying the surface of carbon fiber using a crystalline cross-linkable polyaryletherketone sizing agent combined with diazonium salt modification, using electrochemical reduction to graft small molecule cross-linking groups onto the surface of carbon fiber, and then coating with a soluble polyaryletherketone sizing agent that also contains cross-linking groups, using heat treatment to induce chemical reactions between cross-linking groups and construct covalent bonds at the interface. Although this method can effectively improve the interface strength and the ability of the interface to withstand harsh environments, it requires multiple treatments such as grafting, sizing, and acidification, and the process is relatively complicated and cumbersome, making it difficult to promote. Summary of the invention
[0009] In order to solve the technical problems existing in the prior art, the purpose of the present invention is to prepare a carbon fiber modified with a "grafting-bridging" bifunctional diazonium salt, in which a diazonium salt with a bridging functional group is grafted onto the carbon fiber through electrochemical reduction. The surface-grafted functional group can undergo a bridging reaction with polyetheretherketone after heat treatment to connect the polyetheretherketone to the carbon fiber surface, thereby enhancing the interface strength between the carbon fiber and the polyetheretherketone resin matrix while also being able to resist corrosion in harsh environments.
[0010] In order to achieve the above-mentioned purpose, the technical solution adopted by the present invention is as follows.
[0011] The present invention provides a method for preparing grafted modified carbon fiber, the steps of which are as follows:
[0012] (1) dissolving a reaction monomer containing an aniline group and a bridging reaction group and tetrafluoronitrosoborate in acetonitrile respectively, then dropping the obtained reaction monomer solution in acetonitrile into the tetrafluoronitrosoborate solution in acetonitrile under stirring, reacting for 0.1-2h after the dropwise addition, then pouring the obtained reaction solution into an excess of ether to precipitate a diazonium salt, filtering and separating the diazonium salt, and drying under vacuum at -20°C to 30°C to obtain a bifunctional diazonium salt;
[0013] The molar ratio of the reactive monomer containing an aniline group and a bridging reactive group to tetrafluoronitrosoborate is 1:0.1 to 1:10;
[0014] (2) dissolving a bifunctional diazonium salt and tetrabutyl tetrafluoroboric acid in acetonitrile and stirring them thoroughly to obtain an electrolyte; then pulling a continuous carbon fiber into the electrolyte, and applying a negative potential of -2V to -0.1V to the carbon fiber at room temperature, electrochemically reducing and grafting the surface of the carbon fiber, so that the bifunctional diazonium salt is grafted onto the surface of the carbon fiber; finally, pulling the carbon fiber into acetonitrile to wash away the attached unreacted bifunctional diazonium salt, and drying to obtain a grafted modified carbon fiber (the grafted modified carbon fiber obtained at this time is a continuous carbon fiber);
[0015] The molar ratio of the bifunctional diazonium salt to tetrabutyl tetrafluoroboric acid is 1:1-1:20.
[0016] Furthermore, in step (1), the reactive monomer having an aniline group and a bridging reactive group comprises one or more of p-aminoaniline, p-aminophenylethylamine, and p-aminoamphetamine;
[0017] The structural formulas of p-aminobenzylamine, p-aminophenylethylamine and p-aminoamphetamine are as follows:
[0018]
[0019] Furthermore, in step (1), the molar ratio of the reactive monomer having an aniline group and a bridging reactive group to tetrafluoronitrosoborate is 3:1-1:3.
[0020] Furthermore, in step (1), the reaction temperature is -40°C to 25°C.
[0021] Furthermore, in step (1), the structural formula of the bifunctional diazonium salt is one or more of the following structures:
[0022]
[0023] Furthermore, in step (1), the vacuum degree of the vacuum is 2Pa to 200Pa.
[0024] Furthermore, in step (2), the pulling rate of the carbon fiber is 15 to 100 mm / min.
[0025] Furthermore, in step (2), an infrared heater is used for drying, and the drying temperature is 50 to 200°C.
[0026] Furthermore, in step (2), after drying, the carbon fibers are cut into chopped carbon fibers or discontinuous long fibers to obtain grafted modified carbon fibers.
[0027] The present invention also provides sizing agent-free carbon fiber based on bifunctional diazonium salt modification prepared by the above preparation method.
[0028] The present invention also provides the use of the grafted modified carbon fiber in reinforcing polyaryletherketone resin-based composite materials or prepregs. During the molding process, when the temperature is first raised to 150-250°C, the temperature is kept for 30-120 minutes to initiate a reaction between the bridging groups of the grafted modified carbon fiber and the polyetheretherketone resin to enhance the interface bonding. Other processes are the same as those of the prior art.
[0029] Furthermore, the volume fraction of the carbon fiber in the reinforced polyaryletherketone resin-based composite material is 1% to 80%.
[0030] Further, the polyaryletherketone resin includes one or more of polyetherketoneketone, polyetheretherketone, polyetherketone, polyetheretherketoneketone, polyetherketoneetherketoneketone, biphenyl-type polyetheretherketone, and biphenyl-type polyetheretherketoneketone;
[0031] The structural formulas of the polyetherketoneketone, polyetheretherketone, polyetherketone, polyetheretherketoneketone, polyetherketoneetherketoneketone, biphenyl-type polyetheretherketone, and biphenyl-type polyetheretherketoneketone are as follows:
[0032]
[0033] In the formula, n is independently a positive integer, 10≤n≤200.
[0034] The principle of the present invention is: a monomer containing aniline and a bridging reaction group reacts with tetrafluoronitrosoborate to obtain a bifunctional diazonium salt and grafts it onto the surface of the carbon fiber. Subsequently, a heat treatment is performed at a high temperature to induce a Schiff base reaction between the bridging reaction group and the carbonyl group in the polyetheretherketone, thereby connecting the polyetheretherketone resin matrix to the surface of the carbon fiber.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] 1. The method of the present invention realizes surface modification of carbon fiber by electrochemical grafting of diazonium salt, and the reaction conditions are simple and the reaction time is fast. The method can be carried out based on the electrolytic cell of the existing carbon fiber production line, without the need for complex equipment modification, and can continuously process a large number of carbon fibers, which has good industrialization potential.
[0037] 2. The bridging group in the bifunctional diazonium salt of the present invention can efficiently react with the carbonyl group in polyetheretherketone and produce a covalent bond connection at the interface, which greatly simplifies the reaction process of interface treatment. No additional chemical reagents and harsh reaction conditions are required, and it can occur in situ under heating conditions.
[0038] 3. The method of the present invention does not require sizing agents and subsequent chemical treatment, and can effectively avoid the problem of solvent treatment in large-scale production and the problem of recycling waste acids and alkalis.
[0039] 4. The method of the present invention is applicable to a variety of polyaryletherketone resin matrices containing carbonyl groups, covering most of the polyaryletherketone resin brands currently used in actual production, without the need for additional adjustments to the chemical structure and reaction conditions, and has good universality. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0041] Figure 1 is the infrared spectrum of the bifunctional diazonium salt in Example 1 of the present invention;
[0042] Figure 2 1 is a cyclic voltammetry spectrum of the electrochemical reduction grafting process in Example 1 of the present invention;
[0043] Figure 3 This is a test curve of the interface shear strength between the grafted modified carbon fiber and the polyetheretherketone matrix resin in Example 1 of the present invention. DETAILED DESCRIPTION
[0044] The method of the present invention is described below by way of examples. The examples described are merely specific descriptions of the claims of the present invention, and the claims include but are not limited to the contents of the examples described.
[0045] Unless otherwise specified, the reagents and materials described in the following examples can be obtained from commercial sources; the test methods described are conventional methods unless otherwise specified.
[0046] Example 1
[0047] In terms of molar amount, 1 part of p-aminobenzylamine and 0.45 part of tetrafluoronitrosoborate are dissolved in acetonitrile respectively. Subsequently, the acetonitrile solution of p-aminobenzylamine is added dropwise to the acetonitrile solution of tetrafluoronitrosoborate, mixed and mechanically stirred, and reacted at 25°C for 6 minutes to obtain a mixture solution. The mixture solution is precipitated in ether, and the diazonium salt is filtered and separated, and then dried at -20°C and 20Pa under vacuum to obtain a bifunctional diazonium salt. One part of a bifunctional diazonium salt and 10 parts of tetrabutyl tetrafluoroboric acid were dissolved in 0.1 L of acetonitrile to prepare an electrolyte, and then the continuous carbon fiber was pulled into the above electrolyte at a speed of 15 mm / min, and a negative potential of -0.1 V was applied to the carbon fiber at room temperature, and the surface of the carbon fiber was electrochemically reduced and grafted to graft the bifunctional diazonium salt onto the surface of the carbon fiber; finally, the carbon fiber was pulled into acetonitrile to wash away the attached unreacted bifunctional diazonium salt, and dried at 80°C with an infrared heater to obtain a grafted continuous carbon fiber; when the grafted continuous carbon fiber was used to prepare a carbon fiber reinforced polyetheretherketone resin-based composite material, the carbon fiber was kept at 200°C for 30 minutes during the molding process to induce a reaction between the bridging group and the polyetheretherketone resin, thereby enhancing the interface bonding and obtaining a reinforced polyaryletherketone resin-based composite material.
[0048] Figure 1 is the infrared spectrum of the bifunctional diazonium salt in Example 1 of the present invention, in which the nitrogen-nitrogen triple bond vibration peak in the diazonium salt can be observed, which illustrates the synthesis of the diazonium salt; Figure 2 The cyclic voltammetry spectrum of the electrochemical reduction grafting process in Example 1 of the present invention shows that an obvious reduction peak appears, indicating the occurrence of the electrochemical reduction reaction; Figure 3 This is a test curve of the interface shear strength between the grafted modified carbon fiber and the polyetheretherketone matrix resin in Example 1 of the present invention. It can be seen that the two have good interface shear strength.
[0049] Example 2
[0050] In terms of molar amount, 1 part of p-aminobenzylamine and 1 part of tetrafluoronitrosoborate are dissolved in acetonitrile respectively. Subsequently, the acetonitrile solution of p-aminobenzylamine is added dropwise to the acetonitrile solution of tetrafluoronitrosoborate, mixed and mechanically stirred, and reacted at 25°C for 6 minutes to obtain a mixture solution. The mixture solution is precipitated in ether, and the diazonium salt is filtered and separated, and then dried at 0°C and 5Pa under vacuum to obtain a bifunctional diazonium salt. 10 parts of bifunctional diazonium salt and 100 parts of tetrabutyl tetrafluoroboric acid are dissolved in 1L of acetonitrile to prepare an electrolyte, and then the continuous carbon fiber is pulled into the above electrolyte at a speed of 20 mm / min, and a negative potential of -0.1 V is applied to the carbon fiber at room temperature, and the surface of the carbon fiber is electrochemically reduced and grafted to graft the bifunctional diazonium salt onto the surface of the carbon fiber; finally, the carbon fiber is pulled into acetonitrile to wash away the attached unreacted bifunctional diazonium salt, and is dried at 100°C with an infrared heater to obtain a grafted continuous carbon fiber; when the grafted continuous carbon fiber is used to prepare a carbon fiber reinforced polyetherketoneketone resin-based composite material prepreg, it is kept at 160°C for 30 minutes during the molding process to induce a reaction between the bridging group and the polyetherketoneketone resin, so that the interface bonding is enhanced to obtain a reinforced polyaryletherketone resin-based composite material.
[0051] Example 3
[0052] In terms of molar amount, 1 part of p-aminophenylethylamine and 0.75 parts of tetrafluoronitrosoborate are dissolved in acetonitrile respectively. Subsequently, the acetonitrile solution of p-aminophenylethylamine is added dropwise to the acetonitrile solution of tetrafluoronitrosoborate, mixed and mechanically stirred, and reacted at 0°C for 30 minutes to obtain a mixture solution. The mixture solution is precipitated in ether, and the diazonium salt is filtered and separated, and then dried at 10°C and 50Pa vacuum to obtain a bifunctional diazonium salt. 10 parts of bifunctional diazonium salt and 90 parts of tetrabutyl tetrafluoroboric acid are dissolved in 1L of acetonitrile to prepare an electrolyte, and then the continuous carbon fiber is pulled into the above electrolyte at a speed of 20 mm / min, and a negative potential of -0.5 V is applied to the carbon fiber at room temperature, and the surface of the carbon fiber is electrochemically reduced and grafted to graft the bifunctional diazonium salt onto the surface of the carbon fiber; finally, the carbon fiber is pulled into acetonitrile to wash away the attached unreacted bifunctional diazonium salt, and is dried at 80°C with an infrared heater, and is cut to obtain grafted chopped carbon fibers; when the grafted chopped carbon fibers are used to prepare carbon fiber reinforced polyether ketone resin-based composite materials, the carbon fibers are kept at 220°C for 30 minutes during the molding process to induce a reaction between the bridging group and the polyether ketone resin, thereby enhancing the interface bonding and obtaining a reinforced polyaryletherketone resin-based composite material.
[0053] Example 4
[0054] In terms of molar weight, 1 part of p-aminoamphetamine and 0.75 part of tetrafluoronitrosoborate are dissolved in acetonitrile, respectively. Subsequently, the acetonitrile solution of p-aminoamphetamine is added dropwise to the acetonitrile solution of tetrafluoronitrosoborate, mixed and mechanically stirred, and reacted at -40°C for 30 minutes to obtain a mixture solution. The mixture solution is precipitated in ether, and the diazonium salt is filtered and separated, and then dried at 20°C and under a vacuum of 200 Pa to obtain a bifunctional diazonium salt. 15 parts of bifunctional diazonium salt and 130 parts of tetrabutyl tetrafluoroboric acid were dissolved in 1L of acetonitrile to prepare an electrolyte, and then the continuous carbon fiber was pulled into the above electrolyte at a speed of 20 mm / min, and a negative potential of -0.5 V was applied to the carbon fiber at room temperature, and the surface of the carbon fiber was electrochemically reduced and grafted to graft the bifunctional diazonium salt onto the surface of the carbon fiber; finally, the carbon fiber was pulled into acetonitrile to wash away the attached unreacted bifunctional diazonium salt, and dried at 80°C with an infrared heater, and then cut to obtain a grafted non-continuous long carbon fiber; when the grafted non-continuous long carbon fiber was used to prepare a carbon fiber reinforced polyether ketone resin-based composite material, the carbon fiber was kept at 220°C for 30 minutes during the molding process to induce a reaction between the bridging group and the biphenyl polyether ketone ether resin, so that the interface bonding was enhanced to obtain a reinforced polyaryletherketone resin-based composite material.
[0055] Example 5
[0056] In terms of molar weight, 1 part of p-aminoamphetamine and 4 parts of tetrafluoronitrosoborate are dissolved in acetonitrile, respectively. Subsequently, the acetonitrile solution of p-aminoamphetamine is added dropwise to the acetonitrile solution of tetrafluoronitrosoborate, mixed and mechanically stirred, and reacted at -25°C for 1 hour to obtain a mixture solution. The mixture solution is precipitated in ether, and the diazonium salt is filtered and separated, and then dried at 20°C and 200 Pa under vacuum to obtain a bifunctional diazonium salt. 15 parts of bifunctional diazonium salt and 130 parts of tetrabutyl tetrafluoroboric acid were dissolved in 1L of acetonitrile to prepare an electrolyte, and then the carbon fiber was pulled into the above electrolyte at a speed of 20 mm / min, and a negative potential of -0.5 V was applied to the carbon fiber at room temperature, and the surface of the carbon fiber was electrochemically reduced and grafted to graft the bifunctional diazonium salt onto the surface of the carbon fiber; finally, the continuous carbon fiber was pulled into acetonitrile to wash away the attached unreacted bifunctional diazonium salt, and dried at 80°C with an infrared heater to obtain a grafted continuous carbon fiber; when the grafted continuous carbon fiber was used to prepare a carbon fiber reinforced polyether ketone resin-based composite material, the temperature was kept at 250°C for 30 minutes during the molding process to induce a reaction between the bridging group and the polyether ether ketone ketone resin to obtain a reinforced polyarylether ketone resin-based composite material.
[0057] Example 6
[0058] In terms of molar weight, 1 part of p-aminoamphetamine and 4 parts of tetrafluoronitrosoborate are dissolved in acetonitrile, respectively. Subsequently, the acetonitrile solution of p-aminoamphetamine is added dropwise to the acetonitrile solution of tetrafluoronitrosoborate, mixed and mechanically stirred, and reacted at -25°C for 1 hour to obtain a mixture solution. The mixture solution is precipitated in ether, and the diazonium salt is filtered and separated, and then dried at 25°C and 5Pa under vacuum to obtain a bifunctional diazonium salt. 150 parts of bifunctional diazonium salt and 1500 parts of tetrabutyl tetrafluoroboric acid were dissolved in 10L acetonitrile to prepare an electrolyte, and then the continuous carbon fiber was pulled into the above electrolyte at a speed of 20mm / min, and a negative potential of -0.5V was applied to the carbon fiber at room temperature, and the surface of the carbon fiber was electrochemically reduced and grafted to graft the bifunctional diazonium salt onto the surface of the carbon fiber; finally, the carbon fiber was pulled into acetonitrile to wash away the attached unreacted bifunctional diazonium salt, and dried at 80°C with an infrared heater to obtain a grafted continuous carbon fiber; when the grafted continuous carbon fiber was used to prepare a carbon fiber reinforced polyether ketone resin-based composite material, the temperature was kept at 210°C for 30 minutes during the molding process to induce a reaction between the bridging group and the polyether ketone ether ketone ketone resin to obtain a reinforced polyarylether ketone resin-based composite material.
[0059] Example 7
[0060] In terms of molar weight, 1 part of p-aminoamphetamine and 4 parts of tetrafluoronitrosoborate are dissolved in acetonitrile, respectively. Subsequently, the acetonitrile solution of p-aminoamphetamine is added dropwise to the acetonitrile solution of tetrafluoronitrosoborate, mixed and mechanically stirred, and reacted at -25°C for 1 hour to obtain a mixture solution. The mixture solution is precipitated in ether, and the diazonium salt is filtered and separated, and then dried at 25°C and 5Pa under vacuum to obtain a bifunctional diazonium salt. 150 parts of bifunctional diazonium salt and 1500 parts of tetrabutyl tetrafluoroboric acid were dissolved in 10L acetonitrile to prepare an electrolyte, and then the continuous carbon fiber was pulled into the above electrolyte at a speed of 20mm / min, and a negative potential of -0.5V was applied to the carbon fiber at room temperature, and the surface of the carbon fiber was electrochemically reduced and grafted to graft the bifunctional diazonium salt onto the surface of the carbon fiber; finally, the carbon fiber was pulled into acetonitrile to wash away the attached unreacted bifunctional diazonium salt, and dried at 80°C with an infrared heater to obtain a grafted continuous carbon fiber; when the grafted continuous carbon fiber was used to prepare a carbon fiber reinforced polyetherketone resin-based composite material, the temperature was kept at 210°C for 30 minutes during the molding process to induce a reaction between the bridging group and the biphenyl-type polyetheretherketoneketone resin, so that the interface bonding was enhanced to obtain a reinforced polyaryletherketone resin-based composite material.
[0061] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0062] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing grafted modified carbon fiber, characterized in that: Here are the steps: (1) dissolving a reaction monomer containing an aniline group and a bridging reaction group and tetrafluoronitrosoborate in acetonitrile respectively, then dropping the obtained reaction monomer solution in acetonitrile into the tetrafluoronitrosoborate solution in acetonitrile under stirring, reacting for 0.1-2h after the dropwise addition, then pouring the obtained reaction solution into an excess of ether to precipitate a diazonium salt, filtering and separating the diazonium salt, and drying under vacuum at -20°C to 30°C to obtain a bifunctional diazonium salt; The molar ratio of the reactive monomer containing an aniline group and a bridging reactive group to tetrafluoronitrosoborate is 1:0.1 to 1:10; (2) dissolving a bifunctional diazonium salt and tetrabutyl tetrafluoroboric acid in acetonitrile and stirring them thoroughly to obtain an electrolyte; then pulling the continuous carbon fiber into the electrolyte, and applying a negative potential of -2V to -0.1V to the carbon fiber at room temperature, electrochemically reducing and grafting the surface of the carbon fiber, so that the bifunctional diazonium salt is grafted onto the surface of the carbon fiber; finally, pulling the carbon fiber into acetonitrile to wash away the attached unreacted bifunctional diazonium salt, and drying to obtain a grafted modified carbon fiber; The molar ratio of the bifunctional diazonium salt to tetrabutyl tetrafluoroboric acid is 1:1-1:
20.
2. The method for preparing grafted modified carbon fiber according to claim 1, characterized in that: In step (1), the reactive monomer having an aniline group and a bridging reactive group comprises one or more of p-aminoaniline, p-aminophenylethylamine, and p-aminoamphetamine; The structural formulas of p-aminobenzylamine, p-aminophenylethylamine and p-aminoamphetamine are as follows:
3. The method for preparing grafted modified carbon fiber according to claim 1, characterized in that: In step (1), the molar ratio of the reactive monomer having an aniline group and a bridging reactive group to tetrafluoronitrosoborate is 3:1-1:
3.
4. The method for preparing grafted modified carbon fiber according to claim 1, characterized in that: In step (1), the reaction temperature is -40°C to 25°C; And / or, the vacuum degree of the vacuum is 2Pa to 200Pa.
5. The method for preparing grafted modified carbon fiber according to claim 1, characterized in that: In step (1), the structural formula of the bifunctional diazonium salt is one or more of the following structures:
6. The method for preparing grafted modified carbon fiber according to claim 1, characterized in that: In step (2), the pulling rate of the carbon fiber is 15 to 100 mm / min; And / or, use an infrared heater for drying, and the drying temperature is 50-200°C.
7. The method for preparing grafted modified carbon fiber according to claim 1, characterized in that: In step (2), after drying, the carbon fibers are cut into short chopped carbon fibers or discontinuous long fibers to obtain grafted modified carbon fibers.
8. Graft-modified carbon fiber prepared according to the preparation method according to any one of claims 1 to 7.
9. The use of the grafted modified carbon fiber in reinforcing polyaryletherketone resin-based composite materials according to claim 8, characterized in that: During the molding process, when the temperature is first raised to 150-250°C, it is kept warm for 30-120 minutes to initiate a reaction between the bridging groups of the grafted modified carbon fibers and the polyetheretherketone resin, thereby enhancing the interface bonding.
10. The use of the grafted modified carbon fiber according to claim 9 in reinforcing polyaryletherketone resin-based composite materials or prepregs, characterized in that: The volume fraction of the carbon fiber in the reinforced polyaryletherketone resin-based composite material is 1% to 80%; And / or, the polyaryletherketone resin includes one or more of polyetherketoneketone, polyetheretherketone, polyetherketone, polyetheretherketoneketone, polyetherketoneetherketoneketone, biphenyl-type polyetheretherketone, and biphenyl-type polyetheretherketoneketone; The structural formulas of the polyetherketoneketone, polyetheretherketone, polyetherketone, polyetheretherketoneketone, polyetherketoneetherketoneketone, biphenyl-type polyetheretherketone, and biphenyl-type polyetheretherketoneketone are as follows: In the formula, n is independently a positive integer, 10≤n≤200.
Citation Information
Cited By
Organic electrolyte matched with (poly) dicyclopentadiene for use and carbon fiber surface treatment method
CN119899127A
Cross-linked polymer modified carbon fiber, preparation method and composite material
CN121363113A