Qualitative and quantitative detection method for carbon fibers in plastic product

Through sulfuric acid solution digestion and scanning electron microscope-energy spectrometer analysis, combined with gradient temperature-raising digestion and decompression treatment, the deviation and interference problems in the existing carbon fiber detection methods are solved, and the accurate quantitative analysis of carbon fiber in plastic products is achieved. Improves detection accuracy and reliability.

CN119000212APending Publication Date: 2024-11-22CENT TESTING INT GRP CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411128201.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing carbon fiber detection methods such as ashing difference method and TGA thermal weight loss method have problems with test results and reliability, especially in carbonate-containing filler samples, it is difficult to accurately analyze the carbon fiber content.

Method used

Sulfuric acid solution digestion combined with scanning electron microscope-energy spectrometer analysis, the carbon fiber was isolated and identified through gradient temperature-raising digestion and decompression treatment, and its specific content was calculated to reduce interference from substrate and additives.

Benefits of technology

Accurate and quantitative analysis of carbon fiber in plastic products is achieved, the accuracy and reliability of detection is improved, and the interference of substance decomposition and substrate residual carbon is reduced. It is suitable for a variety of fiber-reinforced plastics and carbonate-containing filler samples.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119000212A_ABST
    Figure CN119000212A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of material analysis, and particularly relates to a qualitative and quantitative detection method for carbon fibers in plastic products, which comprises the following steps: mixing a to-be-detected sample with a sulfuric acid solution to obtain a reactant, digesting the reactant until the to-be-detected sample is dissolved to obtain a digesting solution, maintaining the digesting temperature, dropwise adding an impurity removal agent into the digesting solution until the digesting solution is clarified, whether insoluble substances exist in the digestion solution or not is observed, if the insoluble substances do not exist, it is directly judged that the to-be-detected sample does not contain the carbon fibers, if the insoluble substances exist, the scanning electron microscope-energy spectrometer is used for analyzing and judging whether the sample is the carbon fibers or not, if the sample is the carbon fibers, the same sample is taken, the mass is recorded as M0, and quantitative analysis is conducted according to the same step. Recording the mass of the carbon fiber in the insoluble substance as M1, and calculating the actual carbon fiber content of the sample to be detected according to the mass of M0 and M1. The method solves the problem that qualitative and quantitative determination of the carbon fiber in the plastic product is easily interfered by factors such as base material types or other additives, and results are abnormal, and has a practical application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of material analysis, and in particular relates to a qualitative and quantitative detection method for carbon fibers in plastic products. Background Art

[0002] In today's rapidly developing technological era, plastic products are widely used in our daily lives and industrial production. Among them, carbon fiber, as a high-performance reinforcing material, is increasingly added to plastic products to improve their mechanical properties and durability. However, with the increase in the use of carbon fiber, the detection of the carbon fiber content in plastic products has become particularly important. The common carbon fiber testing methods on the market are mainly based on the ashing difference method and the TGA thermal gravimetric method. However, both methods have certain limitations in practical applications.

[0003] The basic principle of the ashing difference method is to decompose the organic matrix by burning the carbon fiber-containing material at high temperature, and then calculate the carbon fiber content by weighing the mass of the remaining fiber. However, in actual operation, since part of the carbon fiber may be decomposed by heat during the decomposition process of the organic matrix, the test result is low. In addition, the ashing difference method is also affected by factors such as operating conditions and equipment accuracy, which often makes the accuracy of the test results problematic.

[0004] The principle of TGA thermal gravimetric method is to heat the carbon fiber material and observe the change of its mass with temperature, so as to infer the content of carbon fiber. However, in practical applications, due to the presence of other carbon-containing substances such as residual carbon in the substrate and carbonate fillers, these substances will also decompose during the heating process, resulting in distorted test results. In addition, TGA thermal gravimetric method is also affected by factors such as heating rate and atmospheric conditions, which limits the reliability of the test results to a certain extent.

[0005] Chinese patent CN202211651642.9 (publication date: March 28, 2023) discloses a method for determining the carbon fiber content in carbon fiber reinforced plastics, which uses a thermogravimetric analyzer and a microscope to perform qualitative and quantitative analysis on the carbon fiber in carbon fiber reinforced plastics. However, the inventors found that when the method actually tested samples of carbonate-containing fillers, the decomposition temperature of the carbonate overlapped with the carbon fiber part, resulting in obvious distortion of the obtained analysis results, and it was impossible to accurately analyze the carbon fiber in the plastic product. Therefore, the art urgently needs a method that can accurately qualitatively and quantitatively analyze the carbon fiber content in plastic products. Summary of the invention

[0006] In view of the above-mentioned deficiencies in the prior art, the present invention provides a qualitative and quantitative detection method for carbon fiber in plastic products, which can effectively solve the problem of qualitative and quantitative expression deviation in the existing ashing difference method and thermogravimetric analysis method.

[0007] To achieve this object of the invention, the present invention provides a method for qualitative and quantitative detection of carbon fibers in plastic products, comprising the following steps:

[0008] The sample to be tested is mixed with a sulfuric acid solution to obtain a reactant I, and the reactant I is digested until the sample to be tested is dissolved to obtain a digestion solution I, and a removal agent is added dropwise to the digestion solution I while maintaining the digestion temperature until the digestion solution I is clarified, and whether there is insoluble matter in the digestion solution I is observed. If there is no insoluble matter, it is directly determined that the sample to be tested does not contain carbon fiber, and the test is terminated;

[0009] If there are insolubles, dilute the digestion solution I with ultrapure water until the pH of the digestion solution I is 6<pH<7, separate and purify the digestion solution I to obtain the insolubles, and observe whether there are black fibers in the insolubles after drying. If there are no black fibers, it is directly determined that the sample to be tested does not contain carbon fibers, and the test is terminated;

[0010] If there are black fibers in the insoluble matter, the black fibers are analyzed by scanning electron microscope-energy spectrometer. If the analysis results show no carbon fiber-related characteristics, it is directly determined that the sample to be tested does not contain carbon fibers, and the test is terminated;

[0011] If there are carbon fiber related features, it proves that the sample to be tested contains carbon fiber, and the qualitative test is completed;

[0012] Take another part of the samples to be tested for quantitative testing:

[0013] A sample to be tested with a mass of M0 is mixed with a sulfuric acid solution to obtain a reactant II, and the reactant II is digested until the sample to be tested is dissolved to obtain a digestion solution II, and an impurity remover is added dropwise to the digestion solution II while maintaining the digestion temperature until the digestion solution II is clarified, and the digestion solution II is separated and purified to obtain black fibers. After drying, the mass of the black fibers is recorded as M1, and the specific content of the carbon fibers in the sample to be tested is calculated according to the masses of M0 and M1;

[0014] The specific calculation formula of the carbon fiber content in the sample to be tested is as follows:

[0015]

[0016] Where:

[0017] M1——mass of black fiber in quantitative test, unit (g);

[0018] M0——The initial mass of the sample in the quantitative test, unit (g).

[0019] Optionally, the digestion is a gradient temperature increase digestion, and the gradient temperature increase digestion procedure is as follows:

[0020] The first heating stage begins with room temperature as the initial temperature, and the temperature is raised to 180-220°C at a rate of 10-15°C / min, and the temperature is kept constant for 3-8 minutes;

[0021] After the first heating stage, the second heating stage begins, heating to 290-310°C at a rate of 10-20°C / min, and maintaining the temperature for 3-8 minutes;

[0022] After the second heating stage, the third heating stage begins, heating to 340-360°C at a heating rate of 20-30°C / min, and maintaining the temperature for 20-40 minutes to complete the gradient heating digestion.

[0023] Optionally, the mass concentration of the sulfuric acid solution is 90% to 98%.

[0024] Optionally, the impurity remover is an aqueous hydrogen peroxide solution or a nitric acid solution.

[0025] Optionally, the mass concentration of the aqueous hydrogen peroxide solution is 25-40%.

[0026] Optionally, the mass concentration of the nitric acid solution is 30-40%.

[0027] Optionally, the method for separating and purifying the digestion solution is suction filtration or centrifugation.

[0028] Optionally, the filtration comprises the following steps:

[0029] The insoluble matter was collected by filtration using a sand core crucible, and the collected insoluble matter was washed with ethanol solution and ultrapure water in turn, and dried for later use.

[0030] Optionally, the centrifugation comprises the following steps:

[0031] The digestion solution was transferred to a centrifuge tube, and the centrifuge tube was placed in a centrifuge and centrifuged after setting the centrifugation parameters. After the centrifugation, the supernatant was discarded to obtain the purified insoluble matter. The collected insoluble matter was washed with ethanol solution and ultrapure water in turn, and dried for use.

[0032] Optionally, the centrifugal speed is 6000-8000 rpm, and the centrifugal time is 10-20 min.

[0033] Beneficial effects of the present invention:

[0034] The present invention combines the pretreatment of inorganic acid digestion with scanning electron microscope-energy spectrometer analysis, and forms a comprehensive qualitative and quantitative analysis method for plastic products, thereby solving the problem that the qualitative and quantitative determination of carbon fiber in plastic products is easily interfered by factors such as substrate type and other additives, resulting in abnormal results. Compared with the commonly used ash method and thermogravimetric analysis method, it can effectively reduce the impact of problems such as material decomposition, substrate residual carbon, carbonate interference, etc. Based on this invention, the carbon fiber component in plastic products can be quickly and effectively determined, which is helpful for the development and performance evaluation of carbon fiber composite materials, and is convenient for opening up the future market for carbon fiber composite materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 A schematic diagram of the analysis process of the qualitative and quantitative detection method of carbon fibers in plastic products provided by the present invention.

[0036] Figure 2 This is the SEM electron microscope image of the sample in Example 1.

[0037] Figure 3 This is the energy spectrum image of the sample in Example 1.

[0038] Figure 4 This is the SEM electron microscope image of the sample in Example 2.

[0039] Figure 5 This is the energy spectrum image of the sample in Example 2.

[0040] Figure 6 This is the SEM electron microscope image of the sample in Example 3.

[0041] Figure 7 This is the energy spectrum image of the sample in Example 3.

[0042] Figure 8 This is the analytical spectrum of the sample in Example 2 tested by TGA thermogravimetric method.

[0043] Fig. 9 This is the analytical spectrum of the composite fiber material with a carbon content of 99% tested by TGA thermal gravimetric method.

[0044] Fig.10 This is the analytical spectrum of the filler containing carbonate components tested by TGA thermal gravimetric method. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0046] As used herein, the terms "comprises," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0047] "Optional" or "any one" means that the subsequently described matter or event can or cannot occur, and that the description includes instances where the event occurs and instances where it does not.

[0048] The indefinite articles "a" and "an" before the elements or components of the present invention have no limitation on the quantity requirements (i.e. the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the quantity obviously refers to the singular form only.

[0049] The terms "one embodiment", "some embodiments", "exemplarily", "specific examples" or "some examples" described in the present invention mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this document, the schematic representation of the above terms does not necessarily refer to the same embodiment or example.

[0050] The numerical range described in the present invention not only includes the point values ​​listed in the embodiments, but also includes any point values ​​not listed between the numerical ranges described in the present invention. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0051] In the following examples, unless otherwise specified, all reagents and consumables were purchased from conventional reagent manufacturers in the field.

[0052] This embodiment provides a qualitative and quantitative detection method for carbon fiber in a plastic product, comprising the following steps:

[0053] The sample to be tested is mixed with a sulfuric acid solution to obtain a reactant I, and the reactant I is digested until the sample to be tested is dissolved to obtain a digestion solution I, and a removal agent is added dropwise to the digestion solution I while maintaining the digestion temperature until the digestion solution I is clarified, and whether there is insoluble matter in the digestion solution I is observed. If there is no insoluble matter, it is directly determined that the sample to be tested does not contain carbon fiber, and the test is terminated;

[0054] If there are insolubles, dilute the digestion solution I with ultrapure water until the pH of the digestion solution I is 6<pH<7, separate and purify the digestion solution I to obtain the insolubles, and observe whether there are black fibers in the insolubles after drying. If there are no black fibers, it is directly determined that the sample to be tested does not contain carbon fibers, and the test is terminated;

[0055] If there are black fibers in the insoluble matter, the black fibers are analyzed by scanning electron microscope-energy spectrometer. If the analysis results show no carbon fiber-related characteristics, it is directly determined that the sample to be tested does not contain carbon fibers, and the test is terminated;

[0056] If there are carbon fiber related features, it proves that the sample to be tested contains carbon fiber, and the qualitative test is completed;

[0057] Take another part of the samples to be tested for quantitative testing:

[0058] A sample to be tested with a mass of M0 is mixed with a sulfuric acid solution to obtain a reactant II, and the reactant II is digested until the sample to be tested is dissolved to obtain a digestion solution II, and an impurity remover is added dropwise to the digestion solution II while maintaining the digestion temperature until the digestion solution II is clarified, and the digestion solution II is separated and purified to obtain black fibers. After drying, the mass of the black fibers is recorded as M1, and the specific content of the carbon fibers in the sample to be tested is calculated according to the masses of M0 and M1;

[0059] The specific calculation formula of the carbon fiber content in the sample to be tested is as follows:

[0060]

[0061] Where:

[0062] M1——mass of black fiber in quantitative test, unit (g);

[0063] M0——The initial mass of the sample in the quantitative test, unit (g). This embodiment gradually eliminates non-carbon fiber components through multiple steps, first by digestion and impurity removal with sulfuric acid solution, then observing the color and morphology of insoluble matter, and finally using a scanning electron microscope-energy spectrometer for precise analysis, thereby ensuring the accuracy of qualitative detection. At the same time, by accurately measuring the mass of the sample and black fiber before and after digestion, the content of carbon fiber can be accurately calculated, improving the accuracy of quantitative detection.

[0064] In some specific embodiments, the digestion is a gradient temperature increase digestion, and the gradient temperature increase digestion procedure is as follows:

[0065] The first heating stage begins with room temperature as the initial temperature, and the temperature is raised to 180-220°C at a heating rate of 10-15°C / min, and the temperature is kept constant for 3-8 minutes.

[0066] As an example, the heating rate in the first heating stage may also be 11° C. / min, 12° C. / min, 13° C. / min, or 14° C. / min, as long as the heating rate is within the range.

[0067] As an example, the end point of the first heating stage may also be 190° C., 200° C., or 210° C., as long as the end point of the first heating stage is within the range.

[0068] As an example, the constant temperature time of the first heating stage can also be 4 minutes, 5 minutes, 6 minutes, or 7 minutes, as long as the constant temperature time of the first heating stage is within the range.

[0069] After the first heating stage, the second heating stage begins, and the temperature is raised to 290-310°C at a heating rate of 10-20°C / min, and the temperature is kept constant for 3-8 minutes.

[0070] As an example, the heating rate of the second heating stage can also be 12°C / min, 13°C / min, 15°C / min, 17°C / min, 18°C / min, 19°C / min, as long as the heating rate of the second heating stage is within the range.

[0071] As an example, the end point of the second heating stage may also be 295° C., 300° C., or 305° C., as long as the end point of the second heating stage is within the range.

[0072] As an example, the constant temperature time of the second heating stage can also be 4 minutes, 5 minutes, 6 minutes, or 7 minutes, as long as the constant temperature time of the second heating stage is within the range.

[0073] After the second heating stage, the third heating stage begins, heating to 340-360°C at a heating rate of 20-30°C / min, and maintaining the temperature for 20-40 minutes to complete the gradient heating digestion.

[0074] As an example, the heating rate of the third heating stage can also be 22°C / min, 24°C / min, 25°C / min, 26°C / min, 27°C / min, 29°C / min, as long as the heating rate of the third heating stage is within this range.

[0075] As an example, the end point of the third heating stage may also be 345° C., 350° C., or 355° C., as long as the end point of the third heating stage is within the range.

[0076] As an example, the constant temperature time of the third heating stage can also be 22 minutes, 25 minutes, 27 minutes, 30 minutes, 33 minutes, 35 minutes, or 38 minutes, as long as the constant temperature time of the third heating stage is within the range.

[0077] In this embodiment, the plastic substrate can be decomposed more slowly by digestion in a gradient heating manner, thereby reducing liquid splashing or incomplete sample decomposition caused by rapid heating.

[0078] In some specific embodiments, the mass concentration of the sulfuric acid solution is 90% to 98%. As an example, the mass concentration of the sulfuric acid solution can also be 91%, 92%, 93%, 94%, 95%, 96%, 97%, as long as the mass concentration of sulfuric acid is within this range. The sulfuric acid solution used in this embodiment has a high concentration and strong oxidizing properties, which can effectively decompose the organic matter in the plastic product, so that the carbon fiber is released from the matrix. This efficient digestion method ensures that the carbon fiber in the sample can be fully extracted, and then further combined with a gradient heating program, by gradually increasing the temperature of the digestion system, the chemical bonds of different stabilities are decomposed step by step. That is, this embodiment uses a sulfuric acid solution with a specific mass concentration and a gradient heating digestion program to fully decompose complex samples and reduce the risks and uncertainties caused by violent reactions to a certain extent.

[0079] In some specific embodiments, the impurity remover is an aqueous hydrogen peroxide solution or a nitric acid solution. Both the aqueous hydrogen peroxide solution and the nitric acid solution have strong oxidizing properties and can quickly oxidize the carbon element produced by sulfuric acid digestion into carbon dioxide overflow, thereby avoiding the influence of the carbon element on the analysis and ensuring the accuracy and reliability of subsequent scanning electron microscope-energy spectrum analysis data.

[0080] Further, the inventor has done a lot of experiments when selecting impurity remover. In theory, when using potassium permanganate aqueous solution as impurity remover, the positive 7-valent manganese ion therein is heated under acidic conditions, and can react completely with the carbon single substance produced, generating positive 2-valent manganese ions. At this time, the system color will also change from the purple red before the reaction to colorless, and the reaction end point can be more clearly distinguished. But in fact, the instability of potassium permanganate aqueous solution is extremely strong, and violent reactions will occur when contacting with carbon single substance, and even explosions will be caused, especially in higher concentrations or closed systems. This potential danger requires that experimental operation must be carried out under strict safety measures, further increasing the complexity and risk of operation, so the inventor has abandoned the use of potassium permanganate aqueous solution as impurity remover. In addition, although aqueous hydrogen peroxide solution needs to be properly stored to prevent decomposition, it is not easy to cause violent reactions compared to other strong oxidants such as potassium permanganate when used, ensuring the safety of the experimental process, and hydrogen peroxide will only generate oxygen and water after decomposition, which is also very friendly to the environment, so in nitric acid solution and aqueous hydrogen peroxide solution, it is more appropriate to select aqueous hydrogen peroxide solution as carbon remover.

[0081] In some specific embodiments, the mass concentration of the aqueous hydrogen peroxide solution is 25-40%. As an example, the mass concentration of the aqueous hydrogen peroxide solution can also be 27%, 30%, 31%, 33%, 35%, 38%, 39%, as long as the mass concentration of the aqueous hydrogen peroxide solution is within the range.

[0082] In some specific embodiments, the mass concentration of the nitric acid solution is 30-40%. As an example, the mass concentration of the nitric acid solution can also be 32%, 34%, 35%, 37%, 38%, or 39%, as long as the mass concentration of the nitric acid solution is within the range.

[0083] In some specific embodiments, the method for separating and purifying the digestion solution is suction filtration or centrifugation.

[0084] In some specific embodiments, the filtration comprises the following steps:

[0085] The insoluble matter is collected by suction filtration using a sand core crucible, and then the collected insoluble matter is washed with an ethanol solution and ultrapure water in turn, and dried for later use. In this embodiment, the microporous structure of the sand core funnel can effectively intercept insoluble matter, including possible black fibers, while allowing liquid to pass quickly, thereby achieving efficient filtration. At the same time, the transparent glass material makes the filtration process visual, which is convenient for observing the filtration progress and monitoring possible abnormalities, such as blockage or accumulation of insoluble matter.

[0086] In some specific implementations, a coarser filter may be used for pre-filtration before filtering with a sand core crucible, and fine filtering may be performed with a microporous sand core crucible after removing large particles of impurities, thereby improving filtering efficiency.

[0087] In some specific embodiments, the centrifugation comprises the following steps:

[0088] Transfer the digestion solution to a centrifuge tube, place the centrifuge tube in a centrifuge, set the centrifugal parameters, and centrifuge. After the centrifugation, discard the supernatant to obtain the purified insoluble matter. Use ethanol solution and ultrapure water to wash the collected insoluble matter, and dry it for later use. Centrifugal separation is more direct and convenient than filtration. The operation is simple. Just put the sample to be separated into the centrifuge tube, set the speed and time, and the separation process can be automatically completed without complicated settings or adjustments.

[0089] In some specific embodiments, the centrifugal speed is 6000-8000rpm. As an example, the centrifugal speed can also be 6200rpm, 6400rpm, 6500rpm, 6800rpm, 7000rpm, 7200rpm, 7400rpm, 7500rpm, 7700rpm, 7900rpm. As long as the full speed centrifugal speed is within this range, the centrifugal speed within this range can provide the necessary centrifugal force to ensure that the solid particles in the sample are effectively settled or floated to the liquid surface, and the solid-liquid phase is fully separated. At the same time, too low a speed may lead to incomplete separation, while too high a speed may cause sample agitation, affecting the separation effect.

[0090] In some specific embodiments, the centrifugation time is 10 to 20 minutes. As an example, the centrifugation time can also be 11 minutes, 12 minutes, 13 minutes, 14 minutes, 15 minutes, 16 minutes, 17 minutes, 18 minutes, and 19 minutes. As long as the centrifugation time is within this range, the centrifugation time within this range can allow the solid particles to move to the appropriate position under the action of centrifugal force, avoiding incomplete separation due to too short a time, or unnecessary extension of the experimental cycle due to too long a time. More importantly, the above-mentioned centrifugal speed and time of this embodiment can be used as centrifugal parameters to speed up the experimental process on the basis of completing the separation, avoid unnecessary waiting, make the experimental process more efficient, help shorten the analysis and detection cycle, and improve the work efficiency of the laboratory.

[0091] In some specific embodiments, the drying method can be oven drying, microwave drying or infrared drying oven drying. Oven drying is the most commonly used drying method, and the oven is also a standing drying equipment in the laboratory, which is easy to obtain; microwave drying uses the thermal effect and non-thermal effect of microwaves to heat the water molecules inside the carbon fiber to achieve rapid drying. This method can heat evenly, has a fast drying speed, and is also easy to control; the infrared drying oven uses the radiant heat energy of the infrared emitter to directly act on the carbon fiber, causing it to quickly heat up and evaporate water. It has the advantages of strong penetration, fast response speed, and low energy consumption. It is particularly suitable for the rapid drying of thin layers or temperature-sensitive carbon fiber materials. The specific drying temperature and drying time are no longer limited in the present invention, and are determined according to the selected drying method, so as not to lose the carbon fiber.

[0092] The flow chart of the qualitative and quantitative detection method of carbon fiber in the plastic product of the present invention is as follows: Figure 1 As shown, the present invention will be further described below by means of specific embodiments:

[0093] Example 1

[0094] (1) Qualitative testing:

[0095] Weigh about 0.5g of fiber-reinforced epoxy resin plastic sample into a glass container, add 90% sulfuric acid solution to immerse the sample, and then put it into the digestion furnace to start digestion. The digestion heating program is as follows:

[0096] The first heating stage started from room temperature as the initial temperature, and the temperature was raised to 200°C at a rate of 10°C / min, and kept constant for 5 minutes;

[0097] After the first heating stage, the temperature was raised to 300°C at a rate of 10°C / min and kept constant for 5 min;

[0098] After the second heating stage, the third heating stage began, and the temperature was raised to 350°C at a rate of 20°C / min, and the digestion was completed after maintaining the temperature for 30 minutes.

[0099] After the sample matrix is ​​decomposed and the digestion solution becomes turbid, maintain the digestion temperature and add 25% mass concentration of hydrogen peroxide aqueous solution to the digestion solution until the digestion solution is clear. Remove the glassware and put it to room temperature, then add ultrapure water to dilute until the pH is 6.0, and then use a sand core crucible to filter and collect insoluble matter. After drying in an oven, place it under a scanning electron microscope-energy spectrometer for observation, magnify it to an appropriate multiple, frame the fiber area, and the SEM electron microscope image is as follows Figure 2 As shown, the energy spectrum image is Figure 3 As shown. By visual observation and combined Figure 2 and Figure 3 It can be seen that the fiber is non-black in appearance and translucent when observed with the naked eye. The element content distribution tested under an electron microscope / energy spectrometer contains silicon, aluminum, calcium and other elements. It does not meet the characteristics of carbon fiber but meets the characteristics of glass fiber. Therefore, it can be comprehensively determined that the fiber-reinforced epoxy resin plastic sample contains glass fiber components and the test is terminated.

[0100] Example 2

[0101] (1) Qualitative analysis:

[0102] Weigh about 0.5g of fiber-reinforced polyamide plastic sample into a glass container, add 95% sulfuric acid solution to immerse the sample, and then put it into the digestion furnace to start digestion. The digestion heating program is as follows:

[0103] The first heating stage started from room temperature as the initial temperature, and the temperature was raised to 200°C at a rate of 13°C / min, and kept constant for 5 minutes;

[0104] After the first heating stage, the temperature was raised to 300 °C at a rate of 13 °C / min and kept constant for 5 min;

[0105] After the second heating stage, the third heating stage began, and the temperature was raised to 350°C at a rate of 25°C / min, and the digestion was completed after maintaining the temperature for 30 minutes.

[0106] After the plastic sample substrate is decomposed and the digestion solution becomes turbid, maintain the digestion temperature and add a 40% mass concentration of hydrogen peroxide aqueous solution to the digestion solution until the digestion solution is clear. Remove the glassware and put it to room temperature, then add ultrapure water to dilute until the pH is 6.7. Then use a sand core crucible to filter and collect insoluble matter. After drying in an oven, place it under a scanning electron microscope-energy spectrometer for observation, magnify it to an appropriate multiple, frame the fiber area, and the SEM electron microscope image is as follows Figure 4 As shown, the energy spectrum image is Figure 5 As shown. Figure 4 and Figure 5 It can be seen that the element distribution in the test area has no obvious difference from that of carbon fiber, indicating that carbon fiber components exist in the sample and further quantitative analysis is carried out.

[0107] (2) Quantitative analysis:

[0108] Weigh a fiber-reinforced polyamide plastic sample with a mass M0 of 0.5082 g and place it in a glass container. Add 95% sulfuric acid solution to immerse the sample and place it in a digestion furnace to start digestion. The digestion heating program is as follows:

[0109] The first heating stage started from room temperature as the initial temperature, and the temperature was raised to 200°C at a rate of 13°C / min, and kept constant for 5 minutes;

[0110] After the first heating stage, the temperature was raised to 300 °C at a rate of 13 °C / min and kept constant for 5 min;

[0111] After the second heating stage, the third heating stage began, and the temperature was raised to 350°C at a rate of 25°C / min, and the digestion was completed after maintaining the temperature for 30 minutes.

[0112] After the plastic sample substrate is decomposed and the digestion solution becomes turbid, maintain the digestion temperature and add a 30% mass concentration of hydrogen peroxide aqueous solution to the digestion solution until the digestion solution becomes clear. Remove the glassware and put it to room temperature, then add ultrapure water to dilute until the pH is 6.7. Then use a sand core crucible to filter and collect insoluble matter. After drying in an oven, weigh the black fiber that is screened out and record it as mass M1, which is 0.2998g. The calculation formula is as follows:

[0113]

[0114] According to the formula, the carbon fiber content in the fiber-reinforced epoxy resin plastic sample of Example 2 is 58.99%.

[0115] Example 3

[0116] (1) Qualitative analysis:

[0117] Use commercially available carbon fiber with a purity of more than 99% to prepare a composite material sample containing about 60% carbon fiber. Weigh about 0.5g and put it into a glass container. Add 98% sulfuric acid solution to immerse the sample and then put it into a digestion furnace to start digestion. The digestion heating program is as follows:

[0118] The first heating stage started from room temperature as the initial temperature, and the temperature was raised to 200°C at a rate of 15°C / min, and kept constant for 5 minutes;

[0119] After the first heating stage, the temperature was raised to 300°C at a rate of 20°C / min and kept constant for 5 min;

[0120] After the second heating stage, the third heating stage began, and the temperature was raised to 350°C at a rate of 30°C / min, and the digestion was completed after maintaining the temperature for 30 minutes.

[0121] After the plastic sample substrate is decomposed and the digestion solution becomes turbid, a 35% mass concentration nitric acid solution is added to the digestion solution at the digestion temperature until the digestion solution becomes clear. The glassware is removed and placed at room temperature, and then ultrapure water is added to dilute until the pH is 6.5. The digestion solution is transferred to a centrifuge tube, and the centrifuge tube is placed in a centrifuge and centrifuged at 7000 rpm for 15 minutes. After the centrifugation, the supernatant is discarded to obtain the purified insoluble matter. The collected insoluble matter is washed with anhydrous ethanol and ultrapure water for 3 times each, and then placed in an infrared drying oven for drying. The black fibers screened out after drying are placed under a scanning electron microscope-energy spectrometer for observation, magnified to an appropriate multiple, and the fiber area is framed. The SEM electron microscope image is shown as follows: Figure 6 As shown, the energy spectrum image is Figure 7 shown.

[0122] pass Figure 6 and Figure 7 It can be seen that the element distribution in the test area has no obvious difference from that of carbon fiber, indicating that carbon fiber components exist in the sample and further quantitative analysis is carried out.

[0123] (2) Quantitative analysis:

[0124] Weigh 0.4762g of the reinforced fiber composite plastic sample with the same mass M0 as the qualitative analysis and put it into a glass container. Take about 0.5g of the same carbon fiber composite material as the material used for qualitative analysis, record the initial mass M0 as 0.4762g, add 98% sulfuric acid solution to immerse the sample, and then put it into the digestion furnace to start digestion. The digestion heating program is as follows:

[0125] The first heating stage started from room temperature as the initial temperature, and the temperature was raised to 200°C at a rate of 15°C / min, and kept constant for 5 minutes;

[0126] After the first heating stage, the temperature was raised to 300°C at a rate of 20°C / min and kept constant for 5 min;

[0127] After the second heating stage, the third heating stage began, and the temperature was raised to 350°C at a rate of 30°C / min, and the digestion was completed after maintaining the temperature for 30 minutes.

[0128] After the plastic sample substrate is decomposed and the digestion solution becomes turbid, a 35% mass concentration nitric acid solution is added to the digestion solution while maintaining the digestion temperature until the digestion solution becomes clear. The glassware is removed and placed at room temperature, and then ultrapure water is added to dilute until the pH is 6.6. The digestion solution is transferred to a centrifuge tube, and the centrifuge tube is placed in a centrifuge and centrifuged at 7000 rpm for 15 minutes. After the centrifugation, the supernatant is discarded to obtain the purified insoluble matter. The collected insoluble matter is washed with anhydrous ethanol and ultrapure water for 3 times each, and then placed in an infrared drying oven for drying. The black fiber screened out after drying is weighed and recorded as mass M1 of 0.2722 g. The calculation formula is as follows:

[0129]

[0130] According to the formula, the carbon fiber content in the sample of Example 3 is 57.16%.

[0131] It can be found that compared with Example 2 using aqueous hydrogen peroxide solution as the impurity remover, the carbon fiber content separated in Example 3 using nitric acid solution as the carbon remover is a little lower. The inventor speculates that this is because nitric acid has a strong oxidizing property. After mixing with concentrated sulfuric acid and continuously heating at high temperature, part of the carbon fibers in the sample are oxidized or even decomposed, making the final result lower, but the result deviation is still within the controllable range. Therefore, using nitric acid solution as an impurity remover still meets the test requirements.

[0132] Example 4

[0133] (1) Qualitative analysis:

[0134] Weigh about 0.5g of fiber-reinforced polyphenylene sulfide plastic sample containing magnesium carbonate and put it into a glass container. Add 94% sulfuric acid solution to immerse the sample and then put it into a digestion furnace to start digestion. The digestion heating program is as follows:

[0135] The first heating stage started from room temperature as the initial temperature, and the temperature was raised to 210°C at a rate of 14°C / min, and kept constant for 6 minutes;

[0136] After the first heating stage, the temperature was raised to 305°C at a rate of 14°C / min and kept constant for 5 min;

[0137] After the second heating stage, the third heating stage began, and the temperature was raised to 350°C at a rate of 25°C / min, and the digestion was completed after maintaining the temperature for 40 minutes.

[0138] After the plastic sample matrix decomposes and the digestion solution becomes turbid, maintain the digestion temperature and add 35% mass concentration of hydrogen peroxide aqueous solution to the digestion solution until the digestion solution becomes clear. Remove the glassware and let it reach room temperature, then add ultrapure water to dilute it until the pH is 6.8. Use a sand core crucible to filter and collect insoluble matter. After drying in an oven, place it under a scanning electron microscope-energy spectrometer for observation. Both the SEM image and the energy spectrum image show carbon fiber-related characteristics, indicating that carbon fiber components are present in the sample, and further quantitative analysis is carried out.

[0139] (2) Quantitative analysis:

[0140] Weigh 0.5025g of the fiber-reinforced polyphenylene sulfide plastic sample containing magnesium carbonate that is the same as the qualitative analysis, put it into a glass container, add 94% sulfuric acid solution to immerse the sample, and then put it into a digestion furnace to start digestion. The digestion heating program is as follows:

[0141] The first heating stage started from room temperature as the initial temperature, and the temperature was raised to 210°C at a rate of 14°C / min, and kept constant for 6 minutes;

[0142] After the first heating stage, the temperature was raised to 305°C at a rate of 14°C / min and kept constant for 5 min;

[0143] After the second heating stage, the third heating stage began, and the temperature was raised to 350°C at a rate of 25°C / min, and the digestion was completed after maintaining the temperature for 40 minutes.

[0144] After the plastic sample substrate is decomposed and the digestion solution becomes turbid, maintain the digestion temperature and add a 30% mass concentration of hydrogen peroxide aqueous solution to the digestion solution until the digestion solution becomes clear. Remove the glassware and put it to room temperature, then add ultrapure water to dilute until the pH is 6.7. Then use a sand core crucible to filter and collect insoluble matter. After drying in an oven, weigh the black fiber that is screened out and record it as mass M1, which is 0.3752g. The calculation formula is as follows:

[0145]

[0146] According to the formula, the carbon fiber content in the fiber-reinforced epoxy resin plastic sample of Example 2 is 74.67%.

[0147] It can be seen from Examples 1 to 4 of the present invention that the analysis method provided by the present invention can be used for carbon fiber content analysis of various fiber reinforced plastics and carbon fiber reinforced plastics containing carbonate fillers. That is, the method provided by the present invention is not limited by the type of substrate and is not interfered by carbonate additives. It can obtain relatively accurate analysis results in carbon fiber reinforced plastic products with different substrates and has good applicability.

[0148] In order to further prove the accuracy and reliability of the method provided by the present invention, a comparative test is now carried out, and the comparative examples are respectively verified by the ashing difference method and the TGA thermal gravimetric method, as shown below.

[0149] Comparative Example 1

[0150] This comparative example is the ashing difference method:

[0151] Weigh about 0.5 g of the same fiber-reinforced epoxy resin plastic sample as in Example 2 and record the initial mass M0 as 0.4955 g, place it in a ceramic crucible of suitable size, place it in a muffle furnace and heat it to 600° C. and keep the temperature constant for 150 min, take it out and wash it to remove other powder impurities, use microwave drying and cooling, and weigh the fiber mass M1 as 0.2683 g. The calculation formula is as follows:

[0152]

[0153] According to the formula, the carbon fiber content is 54.15%.

[0154] By comparative analysis, it can be seen that the same sample not only decomposes the composite material substrate during heating in the muffle furnace, but also decomposes the carbon fiber in the process, resulting in a test result that is 4.84% less than Example 2 of testing the same material, and 5.85% less than the nominal expected 60% carbon fiber. It can be found that compared with the ashing difference method used in Comparative Example 1, the solution of dripping the impurity remover after sulfuric acid digestion in the present invention can reduce sample loss and avoid distortion of test results due to sample loss in the pre-treatment stage.

[0155] Comparative Example 2

[0156] This comparative example is the ashing difference method:

[0157] Weigh about 0.5 g of the same fiber-reinforced polyphenylene sulfide plastic sample containing magnesium carbonate as in Example 4 and record the initial mass M0 as 0.4985 g, place it in a ceramic crucible of suitable size, place it in a muffle furnace and heat it to 600° C. and keep the temperature constant for 150 min. Take it out and cool it down, and weigh M1 as 0.252 g. The calculation formula is as follows:

[0158]

[0159] According to the formula, the carbon fiber content is 65.25%. Through comparative analysis, it can be seen that the result obtained in this comparative example is 12.15% less than that obtained in Example 4, and the mass loss of the sample in Comparative Example 1 is even greater, and the result is more distorted. The inventor analyzed that this is because the ashing difference method not only decomposes part of the carbon fiber at a higher temperature, but also decomposes part of the magnesium carbonate reinforcing agent in the sample, resulting in more abnormal results. At the same time, this result also reflects that the qualitative and quantitative method provided by the present invention is not affected by additives and can obtain more accurate analysis results.

[0160] On the other hand, it can also be seen that the qualitative and quantitative analysis method provided by the present invention can be used for different types of carbon fiber reinforced plastic samples and has certain applicability.

[0161] Comparative Example 3

[0162] This comparative example is the ashing difference method:

[0163] Weigh about 0.5g of commercially available carbon fiber material sample with a content of >99% and record the initial mass M0 as 0.4667g, place it in a ceramic crucible of appropriate size, heat it to 600℃ in a muffle furnace and keep it at a constant temperature for 150min, take it out and cool it down, weigh M1 as 0.3497g, and calculate it as follows:

[0164]

[0165] According to the formula, the carbon fiber content is 70.15%.

[0166] By comparative analysis, it can be seen that the same pure carbon fiber sample decomposes during the constant temperature heating process in the muffle furnace, and the mass is reduced by 17.60%. That is, the method provided by the present invention mixes the sample to be tested with sulfuric acid and digests it by gradient heating, and removes the impurities generated in the digestion process by using an impurity remover at the end of the digestion. The carbon fiber obtained after purification does not produce mass loss, which can solve the problem of distorted results caused by the existing ashing difference method analysis.

[0167] The following comparative examples were all tested using the TGA thermal gravimetry method, with reference to the "Carbon-fibre-reinforced composites Determination of fibre weight content by thermogravimetry (TG)" standard number ISO22821:2021 (E).

[0168] Comparative Example 4

[0169] This comparative example uses commercially available carbon fiber materials with a content of >99% to perform thermogravimetric analysis, as follows:

[0170] Take about 5 mg of commercially available carbon fiber with a purity of more than 99% and record the initial mass M0 as 5.20 mg, then place it in a TGA crucible, with an initial temperature of 30°C and a nitrogen flow rate of 20 ml / min. After the instrument is purged and stabilized, adjust the balance to zero; maintain the nitrogen atmosphere at a rate of 20°C / min to 600°C and maintain for 10 minutes, with a nitrogen flow rate of 20 ml / min; maintain the nitrogen atmosphere at a rate of 20°C / min to 400°C, with a nitrogen flow rate of 20 ml / min; switch to an oxygen atmosphere and increase the temperature to 850°C at a rate of 20°C / min, with an oxygen flow rate of 20 ml / min. The TGA analysis spectrum is shown below Figure 8 As shown, through Figure 8 It can be seen that:

[0171] (1): The mass change of carbon fiber in the first stage of heating from 30°C to 600°C in a nitrogen atmosphere is -0.88%. Excluding instrument measurement errors, possible interference from other factors such as moisture, it can be considered that the carbon fiber has not been decomposed.

[0172] (2) The mass change of carbon fiber in the second stage of heating from 400°C to 850°C in an oxygen atmosphere is -100.37%. Excluding the instrument measurement error, it can be regarded as the complete decomposition of carbon fiber.

[0173] Comparative Example 5

[0174] This comparative example uses the same carbon fiber composite material (carbon fiber content is about 60%) as used in Example 2 for TGA thermogravimetric analysis, as follows:

[0175] Take about 5 mg of the same carbon fiber composite material as in Example 2, record the initial mass M0 as 4.39 mg, and place it in a TGA crucible, with an initial temperature of 30°C and a nitrogen flow rate of 20 ml / min. After the instrument is purged and stabilized, adjust the balance to zero; maintain the nitrogen atmosphere at a rate of 20°C / min to 600°C and maintain for 10 minutes, with a nitrogen flow rate of 20 ml / min; maintain the nitrogen atmosphere at a rate of 20°C / min to 400°C, with a nitrogen flow rate of 20 ml / min; switch to an oxygen atmosphere and increase the temperature to 850°C at a rate of 20°C / min, with an oxygen flow rate of 20 ml / min. The spectrum is as follows: Fig. 9 As shown, through Fig. 9 It can be seen that:

[0176] (1) The mass change of the carbon fiber composite material in the first stage of heating from 30°C to 600°C in a nitrogen atmosphere is -30.83%, which can be regarded as the decomposition of the composite matrix.

[0177] (2) In the second stage of heating from 400°C to 850°C in an oxygen atmosphere, the carbon fiber undergoes decomposition with a mass change of -67.52%.

[0178] (3) 67.52% is 7.52% higher than the nominal expected 60% carbon fiber content, and 8.53% higher than the result obtained in Example 2, which is a large gap. It can be seen that when using the TGA thermogravimetric method to analyze the actual carbon fiber content, the residual carbon produced by the decomposition of the substrate and the simultaneous decomposition of the carbon fiber cause the result to be biased. In Example 2 of the present application, after mixing the sample to be tested with sulfuric acid and performing a gradient temperature digestion, an impurity remover is used to remove the impurities generated during the digestion process, which effectively avoids the influence of the substrate decomposition caused by the existing TGA thermogravimetric method on the determination of carbon fibers, making the measured results more accurate.

[0179] Comparative Example 6

[0180] This comparative example is to conduct TGA thermogravimetric analysis test on plastic fiber containing carbonate filler, as follows:

[0181] Take about 0.55 mg of the same magnesium carbonate reinforced plastic fiber as in Example 4, record the initial mass M0 as 5.33 mg and place it in a TGA crucible, with an initial temperature of 30°C and a nitrogen flow rate of 20 ml / min. After the instrument is purged and stabilized, adjust the balance to zero; maintain the nitrogen atmosphere at a rate of 20°C / min to 600°C and maintain for 10 minutes, with a nitrogen flow rate of 20 ml / min; maintain the nitrogen atmosphere at a rate of 20°C / min to 400°C, with a nitrogen flow rate of 20 ml / min; switch to an oxygen atmosphere and increase the temperature to 850°C at a rate of 20°C / min, with an oxygen flow rate of 20 ml / min. The spectrum is shown in Figure 1. Fig. 9 As shown, through Fig. 9 It can be seen that:

[0182] ① The mass change of the filler in the first stage of heating from 30°C to 600°C in a nitrogen atmosphere is -58.85%, which can be regarded as the initial decomposition of the filler components.

[0183] ② The filler undergoes decomposition in the second stage of heating from 400°C to 850°C in an oxygen atmosphere, and the change in mass is -9.00%.

[0184] ③From the comparative test analysis, it can be seen that if fillers containing carbonates or other similar ingredients are added to the composite material, and these substances cannot be completely decomposed in the first stage of the TGA heating program, some of them will be synchronously decomposed with the carbon fiber in the second stage of the heating, thereby interfering with the test of the carbon fiber content, resulting in distorted results. In contrast, the method adopted in Example 4 of the present application is to mix the sample and sulfuric acid and digest it through a gradient heating program, and then use an impurity remover to remove the impurities generated during the digestion process, thereby obtaining more accurate test results, which is not achievable by the method disclosed in Comparative Example 6. That is, the qualitative and quantitative method provided by the present invention can solve the problem that the TGA thermogravimetric analysis method cannot accurately analyze the carbon fiber content in plastic samples, and has practical application value.

[0185] Comparative Example 7

[0186] The method used in this comparative example is the method disclosed in the patent document CN2022116516429 cited in the background technology. The magnesium carbonate fiber-reinforced polyphenylene sulfide plastic sample tested in Example 4 of the present invention is tested with reference to Example 1 of the patent, as follows:

[0187] (1) Qualitative analysis:

[0188] Take about 10 mg of magnesium carbonate fiber reinforced polyphenylene sulfide plastic sample and put it into a crucible, and use a thermogravimetric analyzer to heat it under the set analysis parameters. Analysis parameters: N2 purge at 30°C for 5 minutes, N2 flow rate 50ml / min. Maintain N2 atmosphere and increase to 600°C at a rate of 20°C / min, N2 flow rate 50ml / min. After cooling to room temperature, take the residue in the crucible and flatten it on a glass slide, then observe it under a microscope at 100 times magnification. The imaging under the microscope shows the presence of carbon fiber, and continue with quantitative analysis.

[0189] (2) Quantitative analysis:

[0190] Take about 10 mg of magnesium carbonate fiber reinforced polyphenylene sulfide plastic sample and put it into a crucible, record the initial mass M0 as 10.1752 mg, and use a thermogravimetric analyzer for quantitative analysis. The analysis parameters are: N2 purge for 5 minutes at 30°C, N2 flow rate 50ml / min; maintain N2 atmosphere and increase to 600°C at a rate of 20°C / min, N2 flow rate 50ml / min; maintain N2 atmosphere and decrease to 400°C at a rate of 20°C / min, N2 flow rate 50ml / min; switch to O2 atmosphere and increase to 800°C at a rate of 20°C / min, O2 flow rate 50ml / min. The weight loss is calculated based on the weight loss step of the 500°C temperature section of the thermal weight loss curve, and the weight loss mass M2=3.9602 mg is recorded. The specific content formula calculation shall be based on the embodiment of the invention. The actual content of the corresponding sample after thermal gravimetric analysis is M1, M1=M0-M2. M1 is obtained to be 6.2150 mg, and the carbon fiber content calculation formula is as follows:

[0191]

[0192] The carbon fiber content calculated according to the formula is 61.08%, which is much lower than 74.67% of Example 4 of the present invention. Similar to Comparative Examples 5 and 6, this type of quantitative analysis of reinforced fiber plastics containing carbonate components using TGA thermogravimetric method produces a large result error, because the carbonate component cannot be completely decomposed in the first stage of heating, and part of it will be synchronously decomposed with the carbon fiber in the second stage of heating, thereby interfering with the test of the carbon fiber content and causing distorted results.

[0193] Compared with the solutions in the cited patent documents, the present invention adopts different qualitative pretreatment methods to accurately complete qualitative analysis; for the quantitative method, the present invention mixes the sample to be tested with sulfuric acid and then digests it by gradient temperature increase, and uses an impurity remover to decompose the impurities generated in the digestion process. The final carbon fiber content obtained is closer to the theoretical value, which can solve the problem of distortion of the existing TGA thermal gravimetric method for analyzing the carbon fiber content in reinforced plastics.

[0194] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A qualitative and quantitative detection method for carbon fiber in plastic products. It is characterized in that The following steps are involved: The sample to be tested is mixed with a sulfuric acid solution to obtain a reactant I, and the reactant I is digested until the sample to be tested is dissolved to obtain a digestion solution I, and a removal agent is added dropwise to the digestion solution I while maintaining the digestion temperature until the digestion solution I is clarified, and whether there is insoluble matter in the digestion solution I is observed. If there is no insoluble matter, it is directly determined that the sample to be tested does not contain carbon fiber, and the test is terminated; If there are insolubles, dilute the digestion solution I with ultrapure water until the pH of the digestion solution I is 6<pH<7, separate and purify the digestion solution I to obtain the insolubles, and observe whether there are black fibers in the insolubles after drying. If there are no black fibers, it is directly determined that the sample to be tested does not contain carbon fibers, and the test is terminated; If there are black fibers in the insoluble matter, the black fibers are analyzed by scanning electron microscope-energy spectrometer. If the analysis results show no carbon fiber-related characteristics, it is directly determined that the sample to be tested does not contain carbon fibers, and the test is terminated; If there are carbon fiber related features, it proves that the sample to be tested contains carbon fiber, and the qualitative test is completed; Take another part of the samples to be tested for quantitative testing: A sample to be tested with a mass of M0 is mixed with a sulfuric acid solution to obtain a reactant II, and the reactant II is digested until the sample to be tested is dissolved to obtain a digestion solution II, and an impurity remover is added dropwise to the digestion solution II while maintaining the digestion temperature until the digestion solution II is clarified, and the digestion solution II is separated and purified to obtain black fibers. After drying, the mass of the black fibers is recorded as M1, and the specific content of the carbon fibers in the sample to be tested is calculated according to the masses of M0 and M1; The specific calculation formula of the carbon fiber content in the sample to be tested is as follows: Where: M 1 ——Black fiber mass in quantitative test, unit (g); M 0 ——Initial mass of sample in quantitative test, unit (g).

2. The method for qualitative and quantitative detection of carbon fiber in a plastic product according to claim 1, It is characterized in that The digestion is a gradient temperature increase digestion, and the gradient temperature increase digestion procedure is as follows: The first heating stage begins with room temperature as the initial temperature, and the temperature is raised to 180-220°C at a rate of 10-15°C / min, and the temperature is kept constant for 3-8 minutes; After the first heating stage, the second heating stage begins, heating to 290-310°C at a rate of 10-20°C / min, and maintaining the temperature for 3-8 minutes; After the second heating stage, the third heating stage began, and the temperature was raised to 340-360°C at a heating rate of 20-30°C / min, and the temperature was kept constant for 20-40 minutes to complete the gradient heating digestion.

3. The method for qualitative and quantitative detection of carbon fiber in a plastic product according to claim 1, It is characterized in that The mass concentration of the sulfuric acid solution is 90% to 98%.

4. The method for qualitative and quantitative detection of carbon fiber in a plastic product according to claim 1, It is characterized in that The impurity remover is a hydrogen peroxide solution or a nitric acid solution.

5. The method for qualitative and quantitative detection of carbon fiber in a plastic product according to claim 4, It is characterized in that The mass concentration of the hydrogen peroxide aqueous solution is 25-40%.

6. The method for qualitative and quantitative detection of carbon fiber in a plastic product according to claim 4, It is characterized in that The mass concentration of the nitric acid solution is 30-40%.

7. The method for qualitative and quantitative detection of carbon fiber in a plastic product according to claim 1, It is characterized in that The method for separating and purifying the digestion solution is suction filtration or centrifugation.

8. The method for qualitative and quantitative detection of carbon fiber in a plastic product according to claim 7, It is characterized in that The suction filtration comprises the following steps: The insoluble matter was collected by filtration using a sand core crucible, and the collected insoluble matter was washed with ethanol solution and ultrapure water in turn, and dried for later use.

9. The method for qualitative and quantitative detection of carbon fiber in a plastic product according to claim 7, It is characterized in that The centrifugation comprises the following steps: The digestion solution was transferred to a centrifuge tube, and the centrifuge tube was placed in a centrifuge and centrifuged after setting the centrifugation parameters. After the centrifugation, the supernatant was discarded to obtain the purified insoluble matter. The collected insoluble matter was washed with ethanol solution and ultrapure water in turn, and dried for use.

10. The method for qualitative and quantitative detection of carbon fiber in a plastic product according to claim 7, It is characterized in that The centrifugal speed is 6000-8000 rpm, and the centrifugal time is 10-20 min.

Citation Information

Cited By

  • Method for measuring content of sizing agent in fiber

    CN119845771A

  • Method and device for testing resin content and fiber surface density of thermoplastic prepreg

    CN121830379A