Transparent conductive film and preparation method and application thereof

Through the combination of untreated carbon materials and sulfur-doped carbon materials, transparent conductive films with high transparency and low block resistance were prepared, which solved the problem of insufficient transparency and conductivity of existing transparent conductive films. They were suitable for small solar heaters , achieves the effect of uniform heating, reducing energy consumption and no visible light emission.

CN119008086APending Publication Date: 2024-11-22HEBEI UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411202221.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing transparent conductive films have shortcomings in terms of transparency and conductivity, and it is difficult to meet the simultaneous application needs of high transparency and good conductivity.

Method used

Using the combination of untreated carbon materials and sulfur-doped carbon materials, a transparent conductive film with improved conductivity and transparency is prepared by a specific mass ratio and preparation method, combined with organic matter and nanowires, and applied to the spraying method Curved structure of small sun heater.

Benefits of technology

It achieves a transparent conductive film with high transparency and low block resistance. It has the characteristics of uniform heating, reduced energy consumption, low cost and no visible light emission. It is suitable for small solar heaters, reduces vision damage, and improves physical therapy functions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008086A_ABST
    Figure CN119008086A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of conductive materials, and provides a transparent conductive film and a preparation method and application thereof. Raw materials of the transparent conductive film comprise a conductive material and an organic matter. The conductive material includes an untreated carbon material and a sulfur-doped carbon material. According to the technical scheme, the problems of poor transparency and conductivity of the transparent conductive film in the prior art are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of conductive materials, and in particular to a transparent conductive film and a preparation method and application thereof. Background Art

[0002] Transparent conductive films can maintain high transparency in the visible light range while having good conductivity. They mainly include metal film systems, oxide film systems, polymer film systems and composite film systems. The preparation methods mainly include magnetron sputtering, vacuum evaporation, impregnation, chemical vapor deposition and spraying. Because of their unique optical and electrical properties, they are widely used in optoelectronic devices as window materials for devices, which can allow light to pass through and provide the necessary conductive path, such as LEDs and thin-film solar cells. However, the transparency and conductivity of existing transparent conductive films need to be further improved. Summary of the invention

[0003] The present invention provides a transparent conductive film and a preparation method and application thereof, which solve the problem of poor transparency and conductivity of the transparent conductive film in the related art.

[0004] The technical solution of the present invention is as follows: A transparent conductive film, the raw materials of which include conductive materials and organic matter; the conductive materials include untreated carbon materials and sulfur-doped carbon materials.

[0005] As a further technical solution, the organic matter includes one or more of sodium dodecyl sulfonate, perfluorosulfonic acid, polyvinyl pyrrolidone, N,N-dimethylformamide, N-methylpyrrolidone, and ester compounds.

[0006] As a further technical solution, the mass ratio of the untreated carbon material to the sulfur-doped carbon material is 1:1-2.

[0007] The present invention limits the mass ratio of the untreated carbon material to the sulfur-doped carbon material to 1:1-2, thereby further improving the conductivity of the transparent conductive film.

[0008] As a further technical solution, the method for preparing the sulfur-doped carbon material comprises the following steps: S1, mixing the carbon material, ZnCl2 and the dispersant, and drying to obtain a solid; S2. Mixing the solid with sulfur, grinding, heat treating, washing, and drying to obtain a sulfur-doped carbon material.

[0009] The carbon material in the present invention includes one or more of carbon nanotubes, graphene, graphyne, and carbon black, preferably carbon nanotubes.

[0010] As a further technical solution, the dispersant is a mixture of one or more of perfluorosulfonic acid, polystyrene sulfonic acid, sodium dodecyl sulfate, polyvinyl pyrrolidone and alcohols.

[0011] As a further technical solution, the mass concentration of one or more of perfluorosulfonic acid, polystyrene sulfonic acid, sodium dodecyl sulfate, and polyvinyl pyrrolidone in the dispersant is 0.1% to 5%.

[0012] As a further technical solution, the alcohol can be any alcohol solvent, preferably one or more of ethanol, isopropanol, and methanol.

[0013] As a further technical solution, the mass volume ratio of the carbon material, ZnCl2 and dispersant is 1g:1~2g:1mL.

[0014] As a further technical solution, the mass volume ratio of the carbon material, ZnCl2 and dispersant is 1g:1.5g:1mL.

[0015] The present invention limits the mass volume ratio of the carbon material, ZnCl2 and the dispersant to 1g:1.5g:1mL, thereby further improving the conductivity of the transparent conductive film.

[0016] As a further technical solution, the mass ratio of the carbon material to sulfur is 1:0.1~1.

[0017] As a further technical solution, the mass ratio of the carbon material to sulfur is 1:0.4.

[0018] The present invention limits the mass ratio of carbon material to sulfur to 1:0.4, thereby further improving the conductivity of the transparent conductive film.

[0019] As a further technical solution, the heat treatment temperature is 500-900°C and the time is 0.5-1.5h.

[0020] As a further technical solution, the mass ratio of the conductive material to the organic matter is 0.1~0.5:0.1~5.

[0021] As a further technical solution, the conductive material further includes nanowires, and the mass ratio of the untreated carbon material and the sulfur-doped carbon material to the nanowires is 1:0.1~1.

[0022] The nanowires in the present invention include one or more of silver nanowires, copper nanowires, and nickel nanowires, preferably silver nanowires.

[0023] As a further technical solution, the mass ratio of the untreated carbon material and the sulfur-doped carbon material to the nanowires is 1:0.2.

[0024] The present invention also includes nanowires, and the mass ratio of the untreated carbon material and the sulfur-doped carbon material to the nanowires is limited to 1:0.2, which further improves the transparency and conductivity of the transparent conductive film.

[0025] The invention also proposes a method for preparing a transparent conductive film, which comprises the following steps: mixing raw materials and solvent evenly, and spraying to obtain the transparent conductive film.

[0026] As a further technical solution, the mixing method includes one or more of high-speed shearing, ultrasound, and high-pressure blasting.

[0027] As a further technical solution, the thickness of the transparent conductive film is 500nm~2μm.

[0028] As a further technical solution, the solvent is an alcohol, which can be any alcohol solvent, preferably one or more of ethanol, isopropanol, and methanol.

[0029] The present invention also proposes the use of the transparent conductive film or the transparent conductive film prepared by the preparation method in a small solar heater.

[0030] The working principle and beneficial effects of the present invention are: 1. The present invention provides a transparent conductive film, comprising a conductive material and an organic substance; the conductive material comprises an untreated carbon material and a sulfur-doped carbon material, and the two are used in combination to synergistically improve the conductivity and transparency of the film.

[0031] 2. The transparent conductive film provided by the present invention is applied to the reflector with curved structure, and the heating function can be realized by powering on. It can be applied to the small sun heater, and has the advantages of uniform heating, reduced energy consumption, and low cost. It is also transparent, emitting only infrared light, and no visible light, eliminating the visual damage caused by the visible light generated by the high-power small sun, and can better play the function of physical therapy. In addition, by utilizing its transparent heating characteristics, multiple designs of the appearance can be realized to achieve an aesthetic effect, such as designing various beautiful patterns on the curved reflector. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0033] Figure 1 This is a test diagram of the sheet resistance of the transparent conductive film obtained in Example 12; Figure 2 This is a test diagram of the sheet resistance of the transparent conductive film obtained in Comparative Example 1. DETAILED DESCRIPTION

[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] The parameters of the raw materials in the following examples and comparative examples are as follows: Carbon nanotube: Single-walled carbon nanotube, diameter 0.6~2μm, carbon content ≥80%.

[0036] Silver nanowires: diameter 25~35nm, length 10~30μm, concentration 1wt%, solvent is ethanol.

[0037] Polystyrene sulfonic acid: weight average molecular weight is 75000w.

[0038] Example 1 S1. Disperse 1 g of carbon nanotubes and 1 g of ZnCl2 in 1 mL of 0.1 wt% perfluorosulfonic acid ethanol solution, shear at a rotation speed of 25000 rpm for 20 min, dry at 50 ° C, mix the dried solid with 0.1 g of sulfur, grind for 10 min, transfer to a tube furnace for annealing at 650 ° C for 1 h in an argon atmosphere, wash with hydrochloric acid and deionized water, and dry at 50 ° C for 3 h to obtain sulfur-doped carbon nanotubes; S2. Add 0.2 g of untreated carbon nanotubes and 0.1 g of sulfur-doped carbon nanotubes into 100 g of 1 wt% perfluorosulfonic acid anhydrous ethanol solution, disperse them evenly by ultrasonication at an ultrasonic power of 600 W for 30 s, and spray to obtain a transparent conductive film with a thickness of 1 μm.

[0039] Example 2 S1. Disperse 1 g of carbon nanotubes and 1 g of ZnCl2 in 1 mL of 2 wt% polystyrene sulfonic acid isopropanol solution, shear at a rotation speed of 25000 rpm for 20 min, dry at 50 ° C, mix the dried solid with 0.1 g of sulfur, grind for 10 min, transfer to a tube furnace for annealing heat treatment at 500 ° C for 1.5 h in an argon atmosphere, wash with hydrochloric acid and deionized water, and dry at 50 ° C for 3 h to obtain sulfur-doped carbon nanotubes; S2. Add 0.07 g of untreated carbon nanotubes and 0.03 g of sulfur-doped carbon nanotubes into 100 g of 0.1 wt% sodium dodecyl sulfate anhydrous ethanol solution, disperse them evenly by ultrasonication at a power of 600 W for 30 s, and spray to obtain a transparent conductive film with a thickness of 500 nm.

[0040] Example 3 S1. Disperse 1 g of carbon nanotubes and 1 g of ZnCl2 in 1 mL of 5 wt% sodium dodecyl sulfate methanol solution, shear at a rotation speed of 25000 rpm for 20 min, dry at 50 ° C, mix the dried solid with 0.1 g of sulfur, grind for 10 min, transfer to a tube furnace for annealing heat treatment at 900 ° C for 0.5 h in an argon atmosphere, wash with hydrochloric acid and deionized water, and dry at 50 ° C for 3 h to obtain sulfur-doped carbon nanotubes; S2. Add 0.3 g of untreated carbon nanotubes and 0.2 g of sulfur-doped carbon nanotubes into 100 g of 5 wt% N,N-dimethylformamide anhydrous ethanol solution, shear and disperse for 20 min until uniform. The rotation speed during shearing is 25000 rpm, and spray to obtain a transparent conductive film with a thickness of 2 μm.

[0041] Example 4 S1. Disperse 1 g of carbon nanotubes and 1.5 g of ZnCl2 in 1 mL of 0.1 wt% perfluorosulfonic acid ethanol solution, shear at a rotation speed of 25000 rpm for 20 min, dry at 50 ° C, mix the dried solid with 0.1 g of sulfur, grind for 10 min, transfer to a tube furnace for annealing at 650 ° C for 1 h in an argon atmosphere, wash with hydrochloric acid and deionized water, and dry at 50 ° C for 3 h to obtain sulfur-doped carbon nanotubes; S2. Add 0.2 g of untreated carbon nanotubes and 0.1 g of sulfur-doped carbon nanotubes into 100 g of 1 wt% perfluorosulfonic acid anhydrous ethanol solution, disperse them evenly by ultrasonication at an ultrasonic power of 600 W for 30 s, and spray to obtain a transparent conductive film with a thickness of 1 μm.

[0042] Example 5 S1. Disperse 1 g of carbon nanotubes and 2 g of ZnCl2 in 1 mL of 0.1 wt% perfluorosulfonic acid ethanol solution, shear at a rotation speed of 25000 rpm for 20 min, dry at 50 ° C, mix the dried solid with 0.1 g of sulfur, grind for 10 min, transfer to a tube furnace for annealing at 650 ° C for 1 h in an argon atmosphere, wash with hydrochloric acid and deionized water, and dry at 50 ° C for 3 h to obtain sulfur-doped carbon nanotubes; S2. Add 0.2 g of untreated carbon nanotubes and 0.1 g of sulfur-doped carbon nanotubes into 100 g of 1 wt% perfluorosulfonic acid anhydrous ethanol solution, disperse them evenly by ultrasonication at an ultrasonic power of 600 W for 30 s, and spray to obtain a transparent conductive film with a thickness of 1 μm.

[0043] Example 6 S1. Disperse 1 g of carbon nanotubes and 1.5 g of ZnCl2 in 1 mL of 0.1 wt% perfluorosulfonic acid ethanol solution, shear at a rotation speed of 25000 rpm for 20 min, dry at 50 ° C, mix the dried solid with 0.4 g of sulfur, grind for 10 min, transfer to a tube furnace for annealing at 650 ° C for 1 h in an argon atmosphere, wash with hydrochloric acid and deionized water, and dry at 50 ° C for 3 h to obtain sulfur-doped carbon nanotubes; S2. Add 0.2 g of untreated carbon nanotubes and 0.1 g of sulfur-doped carbon nanotubes into 100 g of 1 wt% perfluorosulfonic acid anhydrous ethanol solution, disperse them evenly by ultrasonication at an ultrasonic power of 600 W for 30 s, and spray to obtain a transparent conductive film with a thickness of 1 μm.

[0044] Example 7 S1. Disperse 1 g of carbon nanotubes and 1.5 g of ZnCl2 in 1 mL of 0.1 wt% perfluorosulfonic acid ethanol solution, shear at a rotation speed of 25000 rpm for 20 min, dry at 50 ° C, mix the dried solid with 1 g of sulfur, grind for 10 min, transfer to a tube furnace for annealing at 650 ° C for 1 h in an argon atmosphere, wash with hydrochloric acid and deionized water, and dry at 50 ° C for 3 h to obtain sulfur-doped carbon nanotubes; S2. Add 0.2 g of untreated carbon nanotubes and 0.1 g of sulfur-doped carbon nanotubes into 100 g of 1 wt% perfluorosulfonic acid anhydrous ethanol solution, disperse them evenly by ultrasonication at an ultrasonic power of 600 W for 30 s, and spray to obtain a transparent conductive film with a thickness of 1 μm.

[0045] Example 8 S1. Disperse 1 g of carbon nanotubes and 1.5 g of ZnCl2 in 1 mL of 0.1 wt% perfluorosulfonic acid ethanol solution, shear at a rotation speed of 25000 rpm for 20 min, dry at 50 ° C, mix the dried solid with 0.4 g of sulfur, grind for 10 min, transfer to a tube furnace for annealing at 650 ° C for 1 h in an argon atmosphere, wash with hydrochloric acid and deionized water, and dry at 50 ° C for 3 h to obtain sulfur-doped carbon nanotubes; S2. Add 0.15 g of untreated carbon nanotubes and 0.15 g of sulfur-doped carbon nanotubes into 100 g of 1 wt% perfluorosulfonic acid anhydrous ethanol solution, disperse them evenly by ultrasonication at an ultrasonic power of 600 W for 30 s, and spray to obtain a transparent conductive film with a thickness of 1 μm.

[0046] Example 9 S1. Disperse 1 g of carbon nanotubes and 1.5 g of ZnCl2 in 1 mL of 0.1 wt% perfluorosulfonic acid ethanol solution, shear at a rotation speed of 25000 rpm for 20 min, dry at 50 ° C, mix the dried solid with 0.4 g of sulfur, grind for 10 min, transfer to a tube furnace for annealing at 650 ° C for 1 h in an argon atmosphere, wash with hydrochloric acid and deionized water, and dry at 50 ° C for 3 h to obtain sulfur-doped carbon nanotubes; S2. Add 0.1 g of untreated carbon nanotubes and 0.2 g of sulfur-doped carbon nanotubes into 100 g of 1 wt% perfluorosulfonic acid anhydrous ethanol solution, disperse them evenly by ultrasonication at an ultrasonic power of 600 W for 30 s, and spray to obtain a transparent conductive film with a thickness of 1 μm.

[0047] Example 10 S1. Disperse 1 g of carbon nanotubes and 1.5 g of ZnCl2 in 1 mL of 0.1 wt% perfluorosulfonic acid ethanol solution, shear at a rotation speed of 25000 rpm for 20 min, dry at 50 ° C, mix the dried solid with 0.4 g of sulfur, grind for 10 min, transfer to a tube furnace for annealing at 650 ° C for 1 h in an argon atmosphere, wash with hydrochloric acid and deionized water, and dry at 50 ° C for 3 h to obtain sulfur-doped carbon nanotubes; S2. Add 0.05 g of untreated carbon nanotubes and 0.25 g of sulfur-doped carbon nanotubes into 100 g of 1 wt% perfluorosulfonic acid anhydrous ethanol solution and disperse them evenly by ultrasonication at a power of 600 W for 30 s. Spray coating to obtain a transparent conductive film with a thickness of 1 μm. Embodiment 11 S1. Disperse 1 g of carbon nanotubes and 1.5 g of ZnCl2 in 1 mL of 0.1 wt% perfluorosulfonic acid ethanol solution, shear at a rotation speed of 25000 rpm for 20 min, dry at 50 ° C, mix the dried solid with 0.4 g of sulfur, grind for 10 min, transfer to a tube furnace for annealing at 650 ° C for 1 h in an argon atmosphere, wash with hydrochloric acid and deionized water, and dry at 50 ° C for 3 h to obtain sulfur-doped carbon nanotubes; S2. Add 0.1 g of untreated carbon nanotubes, 0.2 g of sulfur-doped carbon nanotubes, and 0.03 g of silver nanowires into 100 g of 1 wt% perfluorosulfonic acid anhydrous ethanol solution, and disperse them evenly by ultrasonication at an ultrasonic power of 600 W for 30 s, and then spray to obtain a transparent conductive film with a thickness of 1 μm.

[0048] Example 12 S1. Disperse 1 g of carbon nanotubes and 1.5 g of ZnCl2 in 1 mL of 0.1 wt% perfluorosulfonic acid ethanol solution, shear at a rotation speed of 25000 rpm for 20 min, dry at 50 ° C, mix the dried solid with 0.4 g of sulfur, grind for 10 min, transfer to a tube furnace for annealing at 650 ° C for 1 h in an argon atmosphere, wash with hydrochloric acid and deionized water, and dry at 50 ° C for 3 h to obtain sulfur-doped carbon nanotubes; S2. Add 0.1 g of untreated carbon nanotubes, 0.2 g of sulfur-doped carbon nanotubes, and 0.06 g of silver nanowires into 100 g of 1 wt% perfluorosulfonic acid anhydrous ethanol solution, and disperse them evenly by ultrasonication at an ultrasonic power of 600 W for 30 s, and then spray to obtain a transparent conductive film with a thickness of 1 μm.

[0049] Example 13 S1. Disperse 1 g of carbon nanotubes and 1.5 g of ZnCl2 in 1 mL of 0.1 wt% perfluorosulfonic acid ethanol solution, shear at a rotation speed of 25000 rpm for 20 min, dry at 50 ° C, mix the dried solid with 0.4 g of sulfur, grind for 10 min, transfer to a tube furnace for annealing at 650 ° C for 1 h in an argon atmosphere, wash with hydrochloric acid and deionized water, and dry at 50 ° C for 3 h to obtain sulfur-doped carbon nanotubes; S2. Add 0.1 g of untreated carbon nanotubes, 0.2 g of sulfur-doped carbon nanotubes, and 0.3 g of silver nanowires into 100 g of 1 wt% perfluorosulfonic acid anhydrous ethanol solution, disperse them evenly by ultrasonication at an ultrasonic power of 600 W for 30 s, and spray to obtain a transparent conductive film with a thickness of 1 μm.

[0050] Comparative Example 1 0.3 g of carbon nanotubes were added to 100 g of 1 wt % perfluorosulfonic acid anhydrous ethanol solution and dispersed evenly by ultrasonication at an ultrasonic power of 600 W for 30 s, and then sprayed to obtain a transparent conductive film with a thickness of 1 μm.

[0051] Comparative Example 2 S1. Disperse 1 g of carbon nanotubes and 1 g of ZnCl2 in 1 mL of 0.1 wt% perfluorosulfonic acid ethanol solution, shear at a rotation speed of 25000 rpm for 20 min, dry at 50 ° C, mix the dried solid with 0.1 g of sulfur, grind for 10 min, transfer to a tube furnace for annealing at 650 ° C for 1 h in an argon atmosphere, wash with hydrochloric acid and deionized water, and dry at 50 ° C for 3 h to obtain sulfur-doped carbon nanotubes; S2. Add 0.3 g of sulfur-doped carbon nanotubes into 100 g of 1 wt% perfluorosulfonic acid anhydrous ethanol solution, disperse them evenly by ultrasonication at an ultrasonic power of 600 W for 30 s, and spray to obtain a transparent conductive film with a thickness of 1 μm.

[0052] The transparent conductive films obtained in Examples 1 to 13 and Comparative Examples 1 to 2 were tested for transmittance and sheet resistance. The sheet resistance test graph of the transparent conductive film obtained in Example 12 is as follows: Figure 1 As shown; the square resistance test diagram of the transparent conductive film obtained in Comparative Example 1 is as shown Figure 2 The test results are recorded in Table 1.

[0053] Table 1 Transmittance and sheet resistance of transparent conductive films

[0054] It can be seen from Table 1 that the transparent conductive film provided by the present invention has high light transmittance and low sheet resistance, and has good transparency and conductivity.

[0055] Compared with Comparative Examples 1-2, Examples 1-13 use untreated carbon nanotubes and sulfur-doped carbon nanotubes, Comparative Example 1 uses untreated carbon nanotubes, and Comparative Example 2 uses sulfur-doped carbon nanotubes. The transmittance of the transparent conductive film obtained in Examples 1-13 is higher than that in Comparative Example 1, and the sheet resistance is lower than that in Comparative Examples 1-2, indicating that the combination of untreated carbon nanotubes and sulfur-doped carbon nanotubes synergistically improves the conductivity and transparency of the film.

[0056] The square resistance of the transparent conductive film obtained in Example 4 is lower than that in Example 1 and Example 5, indicating that the mass volume ratio of carbon nanotubes, ZnCl2 and dispersant is 1g:1.5g:1mL, which can further improve the conductivity of the transparent conductive film.

[0057] The sheet resistance of the transparent conductive film obtained in Example 6 is lower than that in Example 4 and Example 7, indicating that the mass ratio of carbon nanotubes to sulfur is 1:0.4, which can further improve the conductivity of the transparent conductive film.

[0058] The square resistance of the transparent conductive film obtained in Examples 8-9 is lower than that in Examples 6 and 10, indicating that the mass ratio of the untreated carbon nanotubes to the sulfur-doped carbon nanotubes is 1:1-2, which can further improve the conductivity of the transparent conductive film.

[0059] The light transmittance of the transparent conductive film obtained in Example 12 is higher than that of the other examples, and the sheet resistance is lower than that of the other examples, indicating that on the basis of untreated carbon nanotubes and sulfur-doped carbon nanotubes, silver nanowires are further added, and the mass ratio of silver nanowires to carbon nanotubes is 0.2:1, which can further improve the transparency and conductivity of the transparent conductive film.

[0060] The transparent conductive films obtained in Examples 1 to 13 and Comparative Examples 1 to 2 are respectively applied to the small sun heater, and the method is as follows: the transparent conductive film is prepared on the curved surface of the small sun by spraying, with a thickness of 500 nm, and metal electrodes are prepared at both ends of the circular transparent conductive film to provide voltage to the transparent conductive film.

[0061] The small sun heaters prepared in Examples 1 to 13 can reach 70°C within 5 minutes, and the temperature of the small sun can be maintained at the set temperature through the temperature control device, while the small sun heaters prepared in Comparative Examples 1 to 2 can only reach 40°C within 15 minutes. In addition, the transparent conductive heating film of the present invention only emits infrared light, no visible light, eliminating the visual damage caused by the visible light generated by the high-power small sun, and applying it to the curved surface heating small sun can better play the function of physical therapy.

[0062] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A transparent conductive film, characterized in that: The raw materials include conductive materials and organic matter; the conductive materials include untreated carbon materials and sulfur-doped carbon materials.

2. A transparent conductive film according to claim 1, characterized in that: The mass ratio of the untreated carbon material to the sulfur-doped carbon material is 1:1-2.

3. The transparent conductive film according to claim 1, characterized in that: The method for preparing the sulfur-doped carbon material comprises the following steps: S1, mixing the carbon material, ZnCl2 and the dispersant, and drying to obtain a solid; S2. Mixing the solid with sulfur, grinding, heat treating, washing, and drying to obtain a sulfur-doped carbon material.

4. A transparent conductive film according to claim 3, characterized in that: The mass volume ratio of the carbon material, ZnCl2 and dispersant is 1g:1~2g:1mL.

5. The transparent conductive film according to claim 3, characterized in that: The mass ratio of the carbon material to sulfur is 1:0.1~1.

6. The transparent conductive film according to claim 3, characterized in that: The heat treatment temperature is 500-900° C. and the time is 0.5-1.5 h.

7. The transparent conductive film according to claim 1, characterized in that: The mass ratio of the conductive material to the organic matter is 0.1-0.5:0.1-5.

8. The transparent conductive film according to claim 1, characterized in that: The conductive material also includes nanowires, and the mass ratio of the untreated carbon material and the sulfur-doped carbon material to the nanowires is 1:0.1-1.

9. The method for preparing a transparent conductive film according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: mixing raw materials and solvent evenly, spraying, and obtaining a transparent conductive film.

10. Use of the transparent conductive film according to any one of claims 1 to 8 or the transparent conductive film prepared by the preparation method according to claim 9 in a small solar heater.