Method for improving binding force of neodymium iron boron deposition layer based on enhanced ion exchange deposition technology

By strengthening the ion exchange deposition technology, including surface microelectrolysis and frequency conversion electric field, the binding force of the surface deposition layer of the neodymium iron boron magnet is improved, and the problem of insufficient binding force of the plating layer is solved, which significantly enhances the corrosion resistance and stability of the material.

CN119008211AActive Publication Date: 2024-11-22JIANGXI UNIV OF SCI & TECH +1

Patent Information

Application Number
CN202410945171.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-22
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

The insufficient binding force of the existing NdFeB magnet surface plating leads to instability and safety risks of the materials during service, and a method to improve the binding force of the coating is urgently needed.

Method used

Based on the enhanced ion exchange deposition technology, the deposition layer on the surface of the neodymium iron boron magnet is prepared through surface microelectrolytic corrosion and frequency conversion electric field to enhance the bonding force between the deposition layer and the substrate. Specific steps include cleaning pretreatment, acid corrosion activation, surface microelectrolysis and frequency conversion electric field ion exchange deposition, and the use of electrolytes such as nickel-based electrolytes.

Benefits of technology

The bonding force and corrosion resistance of the deposited layer are significantly improved, the potential difference between the substrate and the deposited layer is reduced, the corrosion resistance of the deposited layer is enhanced, and the risk of magnet shedding is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004945417300000091
    Figure BDA0004945417300000091
  • Figure BDA0004945417300000101
    Figure BDA0004945417300000101
Patent Text Reader

Abstract

The invention provides a method for improving binding force of a neodymium-iron-boron deposition layer based on an enhanced ion exchange deposition technology, and belongs to the technical field of rare earth permanent magnet material preparation. The method comprises the following steps that a neodymium-iron-boron magnet is subjected to cleaning pretreatment, and pollutants and metal oxides on the surface of the magnet are removed; the preparation method comprises the following steps: preparing a pretreated magnet with a rough surface through acid corrosion activation of a neodymium-iron-boron magnet; soaking the pre-treated magnet in electrolyte and connecting the pre-treated magnet with a negative electrode, and performing ion exchange deposition on the surface of the magnet to be deposited by applying a pulse variable-frequency electric field on the surface of the magnet to prepare a deposition layer; wherein firstly, the surface of the magnet is subjected to micro-electrolysis modification, and then a variable-frequency electric field is applied for ion exchange precipitation. In the initial stage, stable current is adopted to continuously perform micro-electrolytic corrosion on the surface of the magnet to regulate and control the interface state of the magnet so as to realize surface modification, and effective combination of a deposition layer formed by subsequent ion exchange deposition is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rare earth permanent magnet material preparation, and particularly relates to a method for improving the bonding force of a NdFeB deposition layer based on an enhanced ion exchange deposition technology. Background Art

[0002] Sintered NdFeB magnets are known as the "king of magnets" for their excellent magnetic properties and are widely used in aerospace, wind power generation, energy-saving home appliances, electronic appliances, and new energy vehicles. However, due to its special multiphase structure and the differences in chemical properties between the phases, NdFeB rare earth permanent magnet materials exhibit inherent insufficient corrosion resistance. In particular, after the easily corroded Nd-rich grain boundary undergoes galvanic corrosion first, the potential difference between the phases accelerates the corrosion and dissolution of the Nd-rich phase at the grain boundary, and the binding medium between the main phase grains inside the magnet disappears, which will cause the main phase grains to fall off and even cause the magnet to fail due to pulverization. This increases the instability and safety risks of the material during service. Therefore, the application and development of NdFeB magnetic materials cannot be separated from reliable corrosion protection technology. At present, the most widely used way to improve the corrosion resistance of NdFeB magnetic materials is to add an anti-corrosion deposition layer on its surface.

[0003] At present, pulse electroplating is the main process for surface treatment of NdFeB magnets to obtain corrosion-resistant deposits. The positive cathode pulse current and the reverse anode pulse current are connected and cycled back and forth periodically. It has the advantages of reducing concentration polarization, high deposition efficiency, uniform and dense deposition layer, low porosity, high purity and flatness, elimination of hydrogen embrittlement, good electrolyte dispersion ability, and deep plating ability. However, the current coating still has the defect of poor bonding strength. The bonding strength of the coating is the most important indicator among all the indicators of electroplating performance. The bonding strength of the coating refers to the bonding strength between the deposition layer and the base metal or the intermediate deposition layer, that is, the force required to peel the coating per unit surface area from the base metal or the intermediate deposition layer.

[0004] Therefore, there is an urgent need for a method to improve the bonding strength of the surface coating of NdFeB magnets. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a method for improving the bonding strength of a NdFeB deposited layer based on enhanced ion exchange deposition technology, aiming to solve at least one technical problem in the background technology.

[0006] The present invention is achieved in that:

[0007] The method for improving the bonding strength of NdFeB deposited layer based on enhanced ion exchange deposition technology comprises the following steps:

[0008] Cleaning pretreatment of NdFeB magnets to remove pollutants and metal oxides on the magnet surface;

[0009] A pre-treated magnet with a rough surface is obtained by acid-corroding and activating a NdFeB magnet;

[0010] The pre-treated magnet is immersed in an electrolyte and connected to a negative electrode, and a deposition layer is prepared on the surface of the pre-treated magnet using a two-step process; wherein the two-step process is firstly applying surface micro-electrolytic corrosion and then performing ion exchange deposition under the action of a variable frequency electric field.

[0011] Preferably, the surface micro-electrolytic corrosion in the two-step treatment method is performed as follows:

[0012] Reverse current density 1-3A / dm 2 , reverse conduction time 1ms, reverse cut-off time 1ms, processing time is 30-60s.

[0013] Preferably, the parameters of the variable frequency electric field are: current density is 6-10A / dm 2 , the operating frequency is 200-600Hz and the duty cycle is 20-40%.

[0014] Preferably, the temperature of the two-step treatment is 45±5°C.

[0015] Preferably, the electrolyte adopts a nickel-based electrolyte; the nickel-based electrolyte contains at least the following components in concentrations: nickel sulfate 180-280 g / L; nickel chloride 20-40 g / L; boric acid 30-40 g / L; saccharin 0.6-1 g / L; 1,4-butynediol 0.2-0.5 g / L; coumarin 0.1-0.2 g / L; formaldehyde 0.1-0.2 g / L; sodium dodecyl sulfate 0.05-0.1 g / L.

[0016] Other corrosion-resistant electrolytes may also be used in the present invention, such as epoxy resin electrolyte, zinc-based electrolyte, chromium-based electrolyte or any other electrolytes for preparing coatings permitted in the art.

[0017] Preferably, the NdFeB magnet cleaning pretreatment to remove pollutants and metal oxides on the magnet surface specifically includes:

[0018] Place the NdFeB magnet in an alkaline cleaning solution and clean it at 65±5℃ to remove organic pollutants on the surface;

[0019] The magnet is cleaned to remove residual alkaline solution and immersed in nitric acid to remove metal oxides and inorganic pollutants on the surface.

[0020] Preferably, the alkaline wash solution contains at least the following components in concentration:

[0021] NaOH 5~10g / L;

[0022] Na2CO3 40~50g / L;

[0023] Na3PO4 40~60g / L;

[0024] OP-10 1~3g / L;

[0025] Sodium dodecyl sulfate 0.1~0.3g / L.

[0026] Preferably, the steps of acid corrosion activation are: firstly immersing the NdFeB magnet in sulfuric acid; and then ultrasonically cleaning and drying with ethanol.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] (1) The initial stable current of the present invention continuously performs micro-electrolytic corrosion on the surface of the magnet to regulate its interface state and thus achieve surface modification, so that the original surface structure of the magnet is changed under the coordinated regulation of chemical and electrochemical effects, the surface roughness is increased, the bonding force of the deposited layer is enhanced, and the corrosion resistance of the deposited layer is improved;

[0029] (2) The present invention uses alternating micro-electrolysis and electrodeposition on the NdFeB magnet before deposition to change the surface structure of the magnet while replacing a portion of the rare earth elements, thereby reducing the potential difference between the substrate and the deposited layer, reducing the surface stress, enhancing the bonding force of the deposited layer, and improving the corrosion resistance of the deposited layer. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific implementation cases described herein are only used to explain the present invention and are not used to limit the present invention.

[0031] A method for improving the bonding strength of a NdFeB deposited layer based on enhanced ion exchange deposition technology, the steps are as follows:

[0032] S1. Cleaning and pretreatment of NdFeB magnets to remove pollutants and metal oxides on the surface of the magnets;

[0033] First, the NdFeB magnet is placed in an alkaline cleaning solution and cleaned at 65±5°C for several minutes to remove organic pollutants on the surface, wherein the alkaline cleaning solution at least contains: NaOH 5-10 g / L; Na2CO3 40-50 g / L; Na3PO4 40-60 g / L; OP-10 1-3 g / L; sodium dodecyl sulfate 0.1-0.3 g / L;

[0034] Then, the magnet is cleaned with deionized water to remove the residual alkaline washing solution;

[0035] Then soak the magnet in nitric acid (usually no longer than 1 minute), and then clean it with deionized water to remove metal oxides and inorganic pollutants on the surface;

[0036] The alkaline cleaning solution can be adjusted according to actual needs, and any cleaning solution permitted in the art can be used. The components of the alkaline cleaning solution in the following example are: NaOH 7.5 g / L; Na2CO3 45 g / L; Na3PO4 50 g / L; OP-10 2 g / L; sodium dodecyl sulfate 0.2 g / L.

[0037] S2, preparing a rough surface pre-treated magnet by acid corrosion activation of NdFeB magnets;

[0038] First, soak the NdFeB magnet in sulfuric acid for 5 to 30 seconds; then use alcohol ultrasonic cleaning and drying. Acid corrosion can form macroscopic roughness on the magnet surface.

[0039] S3, immersing the pre-treated magnet in an electrolyte and connecting it to a negative electrode, and preparing a deposition layer on the surface of the pre-treated magnet by a two-step process; wherein the two-step process is firstly applying surface micro-electrolytic corrosion and then performing ion exchange deposition under the action of a variable frequency electric field;

[0040] (1) Prepare electrolyte

[0041] The present invention can use an electrolyte that can produce a corrosion-resistant coating, such as an epoxy resin electrolyte, a zinc-based electrolyte, a chromium-based electrolyte, or any other electrolyte for preparing a coating permitted in the art. Based on considerations of cost, corrosion resistance, etc., a nickel-based electrolyte is preferred in the present invention;

[0042] The nickel-based electrolyte formula includes but is not limited to 180-280 g / L nickel sulfate, 20-40 g / L nickel chloride, 30-40 g / L boric acid, 0.6-1 g / L saccharin, 0.2-0.5 g / L 1,4-butynediol, 0.1-0.2 g / L coumarin, 0.1-0.2 g / L formaldehyde, 0.05-0.1 g / L sodium dodecyl sulfate, and deionized water; reagents can also be added to the above nickel-based electrolyte or the component formula can be adjusted to achieve deposition layers of different components. The nickel-based electrolyte formula of the following embodiment is set as: 230g / L nickel sulfate, 30g / L nickel chloride, 35g / L boric acid, 0.8g / L saccharin, 0.35g / L 1,4-butynediol, 0.15g / L coumarin, 0.15g / L formaldehyde, 0.07g / L sodium dodecyl sulfate, and is prepared with deionized water.

[0043] Nickel sulfate and nickel chloride are used as main salts to provide enough cations to be plated for the whole reaction. Boric acid is an essential pH stabilizer in the electroplating process, which maintains the pH value of the electrolyte stable during the electroplating process; saccharin is the primary brightener in nickel electroplating, which can improve the low area and reduce metal impurities, and can also reduce the stress in the deposited layer, and cooperate with the main brightener to brighten; 1,4-butynediol can be used as a stabilizer, adhesion and corrosion resistance promoter; coumarin can reduce the porosity of the deposited layer and increase the brightness; formaldehyde can be used as a brightener to promote the bright and delicate deposited layer and reduce the porosity; sodium dodecyl sulfate is used as a wetting agent in the electrolyte, and its role is to reduce the tension between the magnet surface and the electrolyte, which is conducive to obtaining a better deposition effect.

[0044] (2) Surface micro-electrolysis

[0045] The pre-treated magnet after the treatment in step S2 is placed in an electrolytic cell, an electrolyte is input into the electrolytic cell, the pre-treated magnet is connected to the negative electrode, the positive electrode and the negative electrode are connected to a power source, and the inside of the electrolytic cell is heated to 45±5°C;

[0046] The positive electrode in the present invention can be made of any positive electrode material permitted in the art, such as an inert platinum sheet electrode, a graphite electrode, etc.; the following embodiment uses a graphite sheet as the positive electrode;

[0047] Surface micro-electrolysis uses a relatively long and relatively stable reverse pulse of current to continuously reverse the magnet, further corrode the magnet and thus achieve magnet surface modification, which is beneficial to strengthen the bonding force of the subsequent ion exchange deposition to form a deposition layer. The process parameters are as follows: reverse current density 1-3A / dm 2 , reverse conduction time 1ms, reverse cut-off time 1ms, processing time is 30-60s.

[0048] (3) Variable frequency electric field ion exchange deposition

[0049] Ion exchange deposition is to connect the positive cathode pulse current and the reverse anode pulse current, and repeat the process periodically. When conducting in the forward direction, a large current can promote nucleation growth and generate a dense, bright, low-porosity deposition layer. When conducting in the reverse direction, a fixed small current is used to inhibit the excessive growth of grains, promote grain refinement, etch the sharp and coarse grains and potential defects on the cathode surface, and improve the flatness of the deposition layer;

[0050] In order to deposit a better deposited layer, the pulse parameters are optimized in this step. Specifically, the pulse current density is 6-10A / dm 2 The pulse operating frequency is 200-600 Hz, the pulse duty cycle is 20-40%, and the total electrodeposition time of the bidirectional pulse is 15-20 minutes.

[0051] Example 1

[0052] A method for improving the bonding strength of a NdFeB deposited layer based on enhanced ion exchange deposition technology, using an unmagnetized N40 commercial sintered NdFeB magnet as a prepared magnet, specifically comprising the following steps:

[0053] 1. First, place the magnet in an alkaline cleaning solution at 65±5℃ and stir to remove oil for 10 minutes. The alkaline cleaning formula is NaOH 7.5g / L; Na2CO3 45g / L; Na3PO4 50g / L; OP-10 2g / L; sodium dodecyl sulfate 0.2g / L. After cleaning and removing oil, rinse it with deionized water, then soak it in a 6wt% HNO3 solution for 30s, and then rinse it with deionized water;

[0054] 2. Soak the magnet in a 3wt% H2SO4 solution for 30 seconds, and then ultrasonically clean it with anhydrous ethanol for 3 minutes to obtain a pretreated sintered NdFeB magnet;

[0055] 3. Place the pretreated sintered NdFeB magnet in a nickel-based electrolyte, connect the magnet to the negative electrode, and use the graphite sheet as the positive electrode. Control the electrolyte temperature to 45°C and perform two-step ion exchange deposition.

[0056] 3-1. Surface micro-electrolysis: Reverse pulse current density 1A / dm 2 , reverse conduction time 1ms, reverse cut-off time 1ms, processing time is 60s;

[0057] 3-2. Variable frequency electric field ion exchange deposition: pulse current density is 10A / dm 2 , forward conduction time 0.5ms, forward cut-off time 0.5ms, pulse operating frequency 400Hz, duty cycle 30%; reverse current density 2A / dm 2 , reverse conduction time is 0.2ms, reverse shutdown time is 0.5ms, and processing time is 15min;

[0058] 3-3. Finally, the sintered NdFeB magnet with nickel plating on the surface is sequentially placed in 50°C deionized water for cleaning and anhydrous ethanol for ultrasonic cleaning.

[0059] The nickel-based electrolyte formula is: 230g / L nickel sulfate, 30g / L nickel chloride, 35g / L boric acid, 0.8g / L saccharin, 0.35g / L 1,4-butynediol, 0.15g / L coumarin, 0.15g / L formaldehyde, 0.07g / L sodium dodecyl sulfate, prepared with deionized water.

[0060] Example 2

[0061] This embodiment is a method for improving the bonding strength of a NdFeB deposited layer based on enhanced ion exchange deposition technology. The difference from Embodiment 1 is the reverse pulse current density of step 3-1, and the other parameters and conditions are the same as those of Embodiment 1.

[0062] 3-1 of this embodiment: Surface micro-electrolysis: Reverse pulse current density 2A / dm 2 , reverse conduction time is 1ms, reverse cut-off time is 1ms, and processing time is 60s.

[0063] Example 3

[0064] This embodiment is a method for improving the bonding strength of a NdFeB deposited layer based on enhanced ion exchange deposition technology. The difference from Embodiment 1 is the reverse pulse current density of step 3-1, and the other parameters and conditions are the same as those of Embodiment 1.

[0065] 3-1 of this embodiment: Surface micro-electrolysis: Reverse pulse current density of 3A / dm 2 , reverse conduction time is 1ms, reverse cut-off time is 1ms, and processing time is 60s.

[0066] Example 4

[0067] This embodiment is a method for improving the bonding strength of a NdFeB deposited layer based on enhanced ion exchange deposition technology. The difference from Embodiment 1 is the reverse pulse treatment time of step 3-1. The other parameters and conditions are the same as those of Embodiment 1.

[0068] 3-1 of this embodiment, surface micro-electrolysis: the current density of the reverse pulse applied was 1A / dm 2 , reverse conduction time is 1ms, reverse cut-off time is 1ms, and processing time is 30s.

[0069] Example 5

[0070] This embodiment is a method for improving the bonding strength of a NdFeB deposited layer based on enhanced ion exchange deposition technology. The difference from Embodiment 1 is the reverse pulse treatment time of step 3-1. The other parameters and conditions are the same as those of Embodiment 1.

[0071] 3-1 of this embodiment, surface micro-electrolysis: the current density of the reverse pulse applied was 1A / dm 2 , reverse conduction time is 1ms, reverse cut-off time is 1ms, and processing time is 40s.

[0072] Example 6

[0073] This embodiment is based on a method for improving the bonding strength of a NdFeB deposited layer using enhanced ion exchange deposition technology. The difference from Embodiment 1 is the reverse pulse treatment time in step 3-1. The remaining parameters and conditions are the same as those in Embodiment 1.

[0074] 3-1 of this embodiment, surface micro-electrolysis: the current density of the reverse pulse applied was 1A / dm 2 , reverse conduction time is 1ms, reverse cut-off time is 1ms, and processing time is 50s.

[0075] Example 7

[0076] This embodiment is a method for improving the bonding strength of a NdFeB deposited layer based on enhanced ion exchange deposition technology. The difference from Embodiment 1 is the pulse current density of step 3-2, and the other parameters and conditions are the same as those of Embodiment 1.

[0077] 3-2 of this embodiment: variable frequency electric field ion exchange deposition: pulse current density is 6A / dm 2 , forward conduction time 0.5ms, forward cut-off time 0.5ms, pulse operating frequency 400Hz, duty cycle 30%; reverse current density 2A / dm 2 , reverse conduction time is 0.2ms, reverse shutdown time is 0.5ms, and processing time is 15min.

[0078] Example 8

[0079] This embodiment is a method for improving the bonding strength of a NdFeB deposited layer based on enhanced ion exchange deposition technology. The difference from Embodiment 1 is the pulse current density of step 3-2, and the other parameters and conditions are the same as those of Embodiment 1.

[0080] 3-2 of this embodiment: variable frequency electric field ion exchange deposition: pulse current density is 8A / dm 2 , forward conduction time 0.5ms, forward cut-off time 0.5ms, pulse operating frequency 400Hz, duty cycle 30%; reverse current density 2A / dm 2 , reverse conduction time is 0.2ms, reverse shutdown time is 0.5ms, and processing time is 15min.

[0081] Example 9

[0082] This embodiment is a method for improving the bonding strength of a NdFeB deposited layer based on enhanced ion exchange deposition technology. The difference from Embodiment 1 is the pulse operating frequency of step 3-2, and the other parameters and conditions are the same as those of Embodiment 1.

[0083] 3-2 of this embodiment: variable frequency electric field ion exchange deposition: pulse current density is 10A / dm 2 , forward conduction time 0.5ms, forward cut-off time 0.5ms, pulse operating frequency 200Hz, duty cycle 30%; reverse current density 2A / dm 2 , reverse conduction time is 0.2ms, reverse shutdown time is 0.5ms, and processing time is 15min.

[0084] Example 10

[0085] This embodiment is a method for improving the bonding strength of a NdFeB deposited layer based on enhanced ion exchange deposition technology. The difference from Embodiment 1 is the pulse operating frequency of step 3-2, and the other parameters and conditions are the same as those of Embodiment 1.

[0086] 3-2 of this embodiment: variable frequency electric field ion exchange deposition: pulse current density is 10A / dm 2 , forward conduction time 0.5ms, forward cut-off time 0.5ms, pulse operating frequency 600Hz, duty cycle 30%; reverse current density 2A / dm 2 , reverse conduction time is 0.2ms, reverse shutdown time is 0.5ms, and processing time is 15min.

[0087] Embodiment 11

[0088] This embodiment is a method for improving the bonding strength of a NdFeB deposited layer based on enhanced ion exchange deposition technology. The difference from Embodiment 1 is the pulse duty cycle of step 3-2, and the other parameters and conditions are the same as those of Embodiment 1.

[0089] 3-2 of this embodiment: variable frequency electric field ion exchange deposition: pulse current density is 10A / dm 2 , forward conduction time 0.5ms, forward cut-off time 0.5ms, pulse operating frequency 400Hz, pulse duty cycle 20%; reverse current density 2A / dm 2 , reverse conduction time is 0.2ms, reverse shutdown time is 0.5ms, and processing time is 15min.

[0090] Example 12

[0091] This embodiment is a method for improving the bonding strength of a NdFeB deposited layer based on enhanced ion exchange deposition technology. The difference from Embodiment 1 is the pulse duty cycle of step 3-2, and the other parameters and conditions are the same as those of Embodiment 1.

[0092] 3-2 of this embodiment: variable frequency electric field ion exchange deposition: pulse current density is 10A / dm 2 , forward conduction time 0.5ms, forward cut-off time 0.5ms, pulse operating frequency 400Hz, pulse duty cycle 40%; reverse current density 2A / dm 2 , reverse conduction time is 0.2ms, reverse shutdown time is 0.5ms, and processing time is 15min.

[0093] Comparative Example 1

[0094] This comparative example is based on a method for enhancing the bonding strength of a NdFeB deposited layer using enhanced ion exchange deposition technology. The difference from Example 1 is the reverse pulse treatment time in step 3-1. The remaining parameters and conditions are the same as those in Example 1.

[0095] 3-1 of this comparative example, surface micro-electrolysis: the current density of the reverse pulse applied was 4A / dm 2 , reverse conduction time is 1ms, reverse cut-off time is 1ms, and processing time is 60s.

[0096] Comparative Example 2

[0097] The method of this comparative example is different from that of Example 1 in that step 3-1 is omitted and ion exchange deposition is directly performed. The other parameters and conditions are the same as those of Example 1.

[0098] Comparative Example 3

[0099] The method of this comparative example is different from that of Example 1 in step 3-1, and the other parameters and conditions are the same as those of Example 1.

[0100] 3-1 of this comparative example, positive pulse electrodeposition: the current density of the applied positive pulse is 6A / dm 2 , forward conduction time is 1ms, forward cut-off time is 1ms, and processing time is 60s.

[0101] Comparative Example 4

[0102] The method of this comparative example is different from that of Example 1 in step 3-1, and the other parameters and conditions are the same as those of Example 1.

[0103] 3-1 of this example, positive pulse electrodeposition: the current density of the applied positive pulse is 6A / dm 2 , forward conduction time is 1ms, forward cut-off time is 1ms, and processing time is 90s.

[0104] Comparative Example 5

[0105] This comparative example is based on a method for enhancing the bonding strength of a NdFeB deposited layer using enhanced ion exchange deposition technology. The difference from Example 1 is the reverse pulse treatment time in step 3-1. The remaining parameters and conditions are the same as those in Example 1.

[0106] 3-1 of this comparative example, surface micro-electrolysis: the current density of the reverse pulse applied was 1A / dm 2 , reverse conduction time is 1ms, reverse cut-off time is 1ms, and processing time is 10s.

[0107] Comparative Example 6

[0108] This comparative example is based on a method for enhancing the bonding strength of a NdFeB deposited layer using enhanced ion exchange deposition technology. The difference from Example 1 is the reverse pulse treatment time in step 3-1. The remaining parameters and conditions are the same as those in Example 1.

[0109] 3-1 of this comparative example, surface micro-electrolysis: the current density of the reverse pulse applied was 1A / dm 2 , reverse conduction time is 1ms, reverse cut-off time is 1ms, and processing time is 70s.

[0110] Comparative Example 7

[0111] This comparative example is based on a method for improving the bonding strength of a NdFeB deposited layer using enhanced ion exchange deposition technology. The difference from Example 1 is the pulse current density of step 3-2, and the other parameters and conditions are the same as those of Example 1.

[0112] 3-2 of this comparative example, variable frequency electric field ion exchange deposition: pulse current density is 11A / dm 2 , forward conduction time 0.5ms, forward cut-off time 0.5ms, pulse operating frequency 400Hz, duty cycle 30%; reverse current density 2A / dm 2 , reverse conduction time is 0.2ms, reverse shutdown time is 0.5ms, and processing time is 15min.

[0113] Comparative Example 8

[0114] This comparative example is based on a method for improving the bonding strength of a NdFeB deposited layer using enhanced ion exchange deposition technology. The difference from Example 1 is the pulse operating frequency of step 3-2, and the remaining parameters and conditions are the same as those of Example 1.

[0115] 3-2 of this comparative example, variable frequency electric field ion exchange deposition: pulse current density is 10A / dm 2 , forward conduction time 0.5ms, forward cut-off time 0.5ms, pulse operating frequency 650Hz, duty cycle 30%; reverse current density 2A / dm 2 , reverse conduction time is 0.2ms, reverse shutdown time is 0.5ms, and processing time is 15min.

[0116] Comparative Example 9

[0117] This comparative example is based on a method for improving the bonding strength of a NdFeB deposited layer using enhanced ion exchange deposition technology. The difference from Example 1 is the pulse duty cycle of step 3-2, and the remaining parameters and conditions are the same as those of Example 1.

[0118] 3-2 of this comparative example, variable frequency electric field ion exchange deposition: pulse current density is 10A / dm 2, forward conduction time 0.5ms, forward cut-off time 0.5ms, pulse operating frequency 400Hz, duty cycle 15%; reverse current density 2A / dm 2 , reverse conduction time is 0.2ms, reverse shutdown time is 0.5ms, and processing time is 15min.

[0119] Comparative Example 10

[0120] This comparative example is based on a method for improving the bonding strength of a NdFeB deposited layer using enhanced ion exchange deposition technology. The difference from Example 1 is the pulse duty cycle of step 3-2, and the remaining parameters and conditions are the same as those of Example 1.

[0121] 3-2 of this comparative example, variable frequency electric field ion exchange deposition: pulse current density is 10A / dm 2 , forward conduction time 0.5ms, forward cut-off time 0.5ms, pulse operating frequency 400Hz, duty cycle 45%; reverse current density 2A / dm 2 , reverse conduction time is 0.2ms, reverse shutdown time is 0.5ms, and processing time is 15min.

[0122] The NdFeB magnets prepared in Examples 1 to 6 and Comparative Examples 1 to 6 were tested, including the charge transfer resistance R ct , corrosion potential E corr , corrosion current density I corr , corrosion inhibition efficiency and bonding strength, and the untreated sintered NdFeB magnet without deposition layer was used as the control group. The results are shown in Table 1.

[0123] Table 1 Comparison of the performance of the deposited layers of various embodiments and comparative examples

[0124]

[0125] It can be seen from Table 1 that pulse electrodeposition has a significant improvement on the corrosion resistance of the deposited layer, but the bonding strength of the NdFeB deposited layer can only be enhanced by applying a surface micro-electrolysis current before ion exchange deposition.

[0126] It can be seen from Examples 1 to 3 that, under the same deposition time, as the surface micro-electrolysis current density increases, the bonding force of the deposited layer increases, but the charge transfer resistance R ct , corrosion potential E corr , corrosion current density I corr When the surface micro-electrolysis current density increased to 3A / dm 2 Above, as shown in Comparative Example 1 4A / dm 2The bonding strength of the deposited layer is reduced because the excessive current density causes excessive corrosion of the intergranular phase of the base magnetic material, and the surface structure of the magnet begins to be unstable; therefore, the initial surface micro-electrolysis current density is set to 1-3A / dm 2 .

[0127] Comparative Example 2 directly adopts conventional ion exchange deposition, and the bonding force of the deposited layer is 13 MPa, which is much lower than the effect of applying surface micro-electrolysis in Example 1.

[0128] It can be seen from Comparative Examples 3 and 4 that applying a forward pulse current before ion exchange deposition does not increase the bonding strength at all, but weakens the bonding strength of the deposited layer. The reason is that the riveting effect of the nickel layer deposited by simply applying a forward current on the flat substrate is weaker than that of the surface treated with micro-electrolysis.

[0129] It can be seen from Comparative Example 5 that if the surface micro-electrolysis is applied for too short a time, although the bonding strength of the deposited layer can be increased, the effect is not good.

[0130] It can be seen from Comparative Example 6 that if the surface micro-electrolysis application time is too long, the deposition layer bonding strength and charge transfer resistance Rct, corrosion potential Ecorr, corrosion current density Icorr, and corrosion inhibition efficiency are slightly reduced compared with Example 1. The reason is that too long current application time also makes the magnet surface unstable.

[0131] The NdFeB magnets prepared in Examples 1, 7 to 12 and Comparative Examples 7 to 10 were tested, including the charge transfer resistance R ct , corrosion potential E corr , corrosion current density I corr , corrosion inhibition efficiency and bonding strength, and the untreated sintered NdFeB magnet without deposition layer was used as the control group. The results are shown in Table 2.

[0132] Table 2 Comparison of the performance of the deposited layers of various embodiments and comparative examples

[0133]

[0134] Combining Table 1 and Table 2, it can be seen from Examples 1, 7 to 8 that with the increase of the variable frequency electric field current density, the bonding force of the deposited layer decreases slightly, but the charge transfer resistance R ct , corrosion potential E corr , corrosion current density I corr , the corrosion inhibition efficiency is improved to a certain extent; when the pulse current density increases to 10A / dm 2 Above, as shown in Comparative Example 7, 11A / dm 2 The performance of the deposited layer is reduced because too high current density is not conducive to the formation of a dense deposited layer; therefore, the forward pulse current density is preferably 6-10A / dm2 .

[0135] It can be seen from Examples 1, 9 to 10 that with the increase of the forward pulse frequency, the performance of the deposited layer is optimal at 400 Hz; when the pulse frequency density increases to above 600 Hz, such as 650 Hz shown in Comparative Example 8, the performance of the deposited layer begins to decline. The reason is that the variable frequency electric field with too high a frequency is not conducive to the formation of the growth of the deposited layer; therefore, the forward pulse frequency is preferably 200-600 Hz.

[0136] It can be seen from Examples 1, 11 to 12 and Comparative Examples 9-10 that different changes in the forward pulse duty cycle have an impact on the corrosion resistance of the deposited layer of the NdFeB magnet. When the forward pulse duty cycle is 20-40%, the impedance value of the deposited layer increases and the corrosion resistance is better. As the duty cycle continues to increase, the performance of the deposited layer decreases significantly.

[0137] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for improving the bonding strength of NdFeB deposited layers based on enhanced ion exchange deposition technology. It is characterized in that The method comprises the following steps: Cleaning pretreatment of NdFeB magnets to remove pollutants and metal oxides on the magnet surface; A rough surface pre-treated magnet is obtained by acid corrosion activation of NdFeB magnets; The pre-treated magnet is immersed in an electrolyte and connected to a negative electrode, and a deposition layer is prepared on the surface of the pre-treated magnet by a two-step process of surface micro-electrolytic corrosion combined with ion exchange deposition technology; wherein, surface micro-electrolytic corrosion is first applied to strengthen the magnet surface, and then a variable frequency electric field is applied to strengthen the ion exchange deposition.

2. A method for improving the bonding strength of a NdFeB deposited layer based on enhanced ion exchange deposition technology according to claim 1, It is characterized in that The surface micro-electrolytic corrosion in the two-step treatment is carried out as follows: Reverse current density 1-3A / dm 2 , reverse conduction time 1ms, reverse cut-off time 1ms, processing time is 30-60s.

3. The method for improving the bonding strength of NdFeB deposited layer based on enhanced ion exchange deposition technology according to claim 1 or 2, It is characterized in that The frequency conversion electric field parameters are: current density is 6-10A / dm 2 , the operating frequency is 200-600Hz and the duty cycle is 20-40%.

4. The method for improving the bonding strength of NdFeB deposited layer based on enhanced ion exchange deposition technology according to claim 1, It is characterized in that The temperature of the two-step treatment is 45±5°C.

5. The method for improving the bonding strength of NdFeB deposited layer based on enhanced ion exchange deposition technology according to claim 1, It is characterized in that The electrolyte adopts nickel-based electrolyte; The nickel-based electrolyte contains at least the following components: Nickel sulfate 180~280g / L; Nickel chloride 20-40 g / L; Boric acid 30-40 g / L; Saccharin 0.6~1g / L; 1,4-butynediol 0.2~0.5g / L; Coumarin 0.1~0.2g / L; Formaldehyde 0.1~0.2g / L; Sodium dodecyl sulfate 0.05~0.1g / L.

6. The method for improving the bonding strength of NdFeB deposited layer based on enhanced ion exchange deposition technology according to claim 1, It is characterized in that The NdFeB magnet cleaning pretreatment removes pollutants and metal oxides on the magnet surface, specifically including: Place the NdFeB magnet in an alkaline cleaning solution and clean it at 65±5℃ to remove organic pollutants on the surface; The magnet is cleaned to remove residual alkaline solution and immersed in nitric acid to remove metal oxides and inorganic pollutants on the surface.

7. The method for improving the bonding strength of NdFeB deposited layer based on enhanced ion exchange deposition technology according to claim 6, It is characterized in that The alkaline washing solution at least comprises the following components: NaOH 5~10g / L; So 2 CO 3 40~50g / L; Na 3 P.O. 4 40~60g / L; OP-10 1~3g / L; Sodium dodecyl sulfate 0.1~0.3g / L.

8. The method for improving the bonding strength of NdFeB deposited layer based on enhanced ion exchange deposition technology according to claim 1, It is characterized in that The steps of acid corrosion activation are: firstly immersing the NdFeB magnet in sulfuric acid; and then ultrasonically cleaning and drying with ethanol.

Citation Information

Patent Citations

  • Preparation method of corrosion-resistant double coatings of improved sintered Nd-Fe-B magnet

    CN111005050A

  • Trivalent chromium plating method for neodymium iron boron workpiece

    CN115433980A

  • Method for improving binding force of ultra-thick and heavy rare earth coating on surface of sintered neodymium-iron-boron magnet

    CN115620979A

  • Electroplating and vapour deposition combined protection method for neodymium-iron-boron magnet

    WO2014153694A1

  • Rare-earth sintered magnet

    WO2021111921A1

Cited By

  • Neodymium iron boron surface protective layer and preparation method thereof

    CN120082939A

  • A NdFeB surface protective layer and preparation method thereof

    CN120082939B