Ceramic packaging base and manufacturing method thereof

By using modified powder and sodium polyacrylate dispersant, combined with two-step degreasing and photopolymerization printing technology, the problems of high viscosity of ceramic slurry and low matching degree of molding process were solved, and high-quality ceramic encapsulation base was prepared.

CN119008539APending Publication Date: 2024-11-22NANJING HUTAO ELECTRONICS CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411121885.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing ceramic slurry has high viscosity and low solid content, which is not well matched with the molding process. This makes the ceramic encapsulation base prone to defects such as pores and cracks during the molding process, affecting the quality.

Method used

Modified powder and sodium polyacrylate were used as dispersants. A two-step degreasing process and photopolymerization printing technology were used to prepare ceramic and conductive slurries, which reduced the viscosity of the slurry and improved its dispersibility, thus ensuring molding accuracy and density.

Benefits of technology

It effectively reduces porosity and crack defects, improves the quality and performance of ceramic encapsulation bases, ensures molding accuracy and stability, reduces the proportion of organic matter, and avoids green body cracking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008539A_ABST
    Figure CN119008539A_ABST
Patent Text Reader

Abstract

The invention discloses a ceramic packaging base and a manufacturing method thereof, and belongs to the technical field of electronic components, the ceramic packaging base comprises a ceramic layer and a conductive layer, the ceramic layer and the conductive layer are adjacently arranged, the raw material of the ceramic layer comprises ceramic slurry, and the ceramic slurry comprises the following components: modified powder A, trimethylolpropane triacrylate A, 1, 2, 4-trimethyl-1, 3-pentanediol monoisobutyrate A, 1, 3, 4-pentanediol monoisobutyrate B, 1, 3, 4-pentanediol monoisobutyrate B and a solvent. The photoinitiator is prepared from 1, 6-hexanediol diacrylate A, a photoinitiator A and sodium polyacrylate A, in the invention, the sebacic acid can modify the surface potential of the alumina powder, and a part of carboxyl groups can form coordinate bonds or ionic bonds with atoms or ions on the surface of the alumina powder, so that the surface energy of the alumina powder can be reduced, the internal friction of the ceramic slurry subsequently prepared by taking the modified powder as the raw material is small, and the viscosity of the ceramic slurry is reduced; the other part of carboxyl is bridged on the surface of the aluminum oxide powder by forming hydrogen bonds, so that the potential of the surface of the aluminum oxide powder is changed, and the contact collision between the aluminum oxide powder is reduced due to mutual repulsion of the same charges.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electronic components, and in particular relates to a ceramic packaging base and a manufacturing method thereof. Background Art

[0002] Electronic products are widely used in modern life. Electronic components are the most basic building blocks of electronic products. Electronic components require high precision. In order to ensure that they are not disturbed by the external environment, ensure working accuracy and extend working life, electronic components need to be installed on a ceramic packaging base and packaged.

[0003] Some invention patents in the field of electronic component technology are disclosed in the prior art, among which the invention patent with application number CN201911338097.6 discloses a ceramic package base material composition, which contains the following components in percentage by mass: 1.6% to 3.0% silicon dioxide, 3.4% to 6.4% chromium oxide, 0.25% to 1% calcium oxide, 0.2% to 0.5% molybdenum, 0.5% to 2% manganese dioxide, and the balance is aluminum oxide. The present invention promotes the anisotropic growth of grains and forms long rod-shaped crystals by adding appropriate MnO2 to the ceramic raw material, which causes the cracks in the ceramic package base to deviate, changes and increases the path of crack propagation, and thus passivates the crack propagation; at the same time, it reduces the liquid phase ratio in the sintering process and reduces the amorphous phase from gathering in the porcelain body to form stress failure points. Therefore, the ceramic packaging base of this technical solution will not have problems such as chipping during grinding wheel cutting and slicing. However, this technical solution still has some shortcomings during its application. The ceramic slurry has problems such as high slurry viscosity and low matching degree between solid content and molding process, and it is easy to have incomplete degreasing, which will lead to defects such as pores and cracks, directly affecting the quality of the ceramic packaging base.

[0004] Based on this, the present invention designs a ceramic packaging base and a manufacturing method thereof to solve the above problems. Summary of the invention

[0005] The purpose of the present invention is to solve the problems of high viscosity of existing ceramic slurry and low matching degree between solid content and molding process, and incomplete degreasing, which may lead to defects such as pores and cracks, directly affecting the quality of the ceramic package base, and to propose a ceramic package base and a method for manufacturing the same.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A ceramic packaging base comprises a ceramic layer and a conductive layer, wherein the ceramic layer and the conductive layer are arranged adjacent to each other;

[0008] The raw material of the ceramic layer includes ceramic slurry, and the ceramic slurry includes the following components: modified powder A, trimethylolpropane triacrylate A, 1,6-hexanediol diacrylate A, photoinitiator A and sodium polyacrylate A;

[0009] The raw material of the conductive layer includes a conductive paste, and the conductive paste includes the following components: a conductive phase, a carrier solvent, a modified powder B, trimethylolpropane triacrylate B, 1,6-hexanediol diacrylate B, a photoinitiator B and sodium polyacrylate B;

[0010] In the conductive paste, the weight ratio of the conductive phase to the modified powder B is 1:0.05-0.25.

[0011] As a further description of the above technical solution:

[0012] The ceramic slurry comprises the following components in parts by weight: 70-80 parts of modified powder A, 2-18 parts of trimethylolpropane triacrylate A, 4-30 parts of 1,6-hexanediol diacrylate A, 2-4 parts of photoinitiator A and 2-5 parts of sodium polyacrylate A.

[0013] As a further description of the above technical solution:

[0014] The conductive paste comprises the following components in parts by weight: 16-72 parts of a conductive phase, 1-6 parts of a carrier solvent, 4-18 parts of a modified powder, 4-16 parts of trimethylolpropane triacrylate, 12-48 parts of 1,6-hexanediol diacrylate, 2-5 parts of a photoinitiator and 2-5 parts of sodium polyacrylate.

[0015] As a further description of the above technical solution:

[0016] The method for preparing the modified powder comprises:

[0017] Add dispersant A and ethanol solution into an ultrasonic device together, and control the ultrasonic device to promote the dissolution of dispersant A;

[0018] After the dispersant A is completely dissolved, a proper amount of alumina powder is weighed in proportion, and the weighed alumina powder is added into the ball mill together with the dispersant and ethanol solution in the ultrasonic equipment;

[0019] After the operation program set by the ball mill is completed, the mixed material in the ball mill is transferred to a vacuum drying device and dried in a vacuum environment at 58° C. to obtain a modified powder.

[0020] As a further description of the above technical solution:

[0021] The ball milling mixing speed of the ball mill is 280r / min, the ball milling time is 3.6h, and the operation program of the ball mill is clockwise rotation for 8min, counterclockwise rotation for 8min, and the interval is 4min;

[0022] The dispersant A is sebacic acid.

[0023] As a further description of the above technical solution:

[0024] The method for preparing the ceramic slurry comprises:

[0025] Add trimethylolpropane triacrylate and 1,6-hexanediol diacrylate in a mass ratio of 1:1 into a magnetic stirring device, and after the two are mixed evenly, add a photoinitiator with a mass fraction of 1.4%;

[0026] After the photoinitiator and the former are evenly mixed, the mixture is taken out and transferred to a three-roll mill. During this process, a certain amount of sodium polyacrylate needs to be added to the three-roll mill.

[0027] After sodium polyacrylate is evenly mixed with the former, a premixed resin is obtained, the premixed resin is taken out and added to a ball mill, and the modified powder is added to the ball mill for ball milling. After the modified powder and the premixed resin are fully mixed, they are taken out and transferred to a vacuum degassing device for vacuum degassing to obtain an alumina ceramic slurry, which is kept away from light for later use.

[0028] As a further description of the above technical solution:

[0029] The preparation method of the conductive paste comprises:

[0030] First, dispersant B is added into a ball mill containing a carrier solvent and stirred to mix evenly to obtain a dispersion system with a mass fraction of 1%;

[0031] Then, the conductive phase powder is added to the ball mill, and the obtained conductive phase slurry is placed in an ultrasonic dispersion device for ultrasonic dispersion treatment for 16 minutes;

[0032] After the ultrasonic dispersion treatment is completed, the mixture is water-milled for 28 min using a sand mill at a ball-to-material mass ratio of 10:1 and a rotation speed of 1350 r / min;

[0033] After the water grinding treatment, the mixture was sieved through 120 meshes and then subjected to a secondary ultrasonic dispersion treatment for 24 minutes to finally obtain a conductive slurry.

[0034] As a further description of the above technical solution:

[0035] The conductive phase is one or more of graphite, carbon black, graphene and carbon nanotubes;

[0036] The dispersant B is one or more of polyvinyl pyrrolidone, sodium polyacrylate and sodium lignin sulfonate, and the dispersant B is preferably sodium polyacrylate;

[0037] The carrier solvent is one or more of dimethylformamide, N-methylpyrrolidone and deionized water, and the carrier solvent is preferably deionized water.

[0038] A method for manufacturing a ceramic package base comprises the following steps:

[0039] S1: preparing ceramic slurry and conductive slurry respectively;

[0040] S2: loading the ceramic slurry and the conductive slurry into the material tank of the photocuring printing device respectively, and controlling the preparation process by a program according to the designed ceramic package base model;

[0041] S3: laying the ceramic slurry to obtain a ceramic layer, irradiating it with reactive light to solidify it, laying the conductive slurry to obtain a conductive layer, and irradiating it with reactive light to solidify it;

[0042] S4: repeating step S3, photocuring printing the ceramic layer and the conductive layer to form a body of the ceramic package base;

[0043] S5: the obtained green body is punched, the via holes are filled, laminated and metal paste is printed, the green body of the ceramic package base is dried and degreased in sequence, and then sintered into porcelain, and finally the ceramic package base is obtained.

[0044] As a further description of the above technical solution:

[0045] In the degreasing process, the dried green body is first degreased in a vacuum environment, and then decarbonized in air for a second degreasing process;

[0046] The heating rate of the degreasing curve in the air environment is about 0.9°C / min;

[0047] Based on the decomposition temperature of trimethylolpropane triacrylate and 1,6-hexanediol diacrylate for full reaction with oxygen, and the thermal decomposition temperature of dispersant A, three temperature nodes are set in the degreasing heating stage to facilitate full thermal decomposition of trimethylolpropane triacrylate, 1,6-hexanediol diacrylate and dispersant A.

[0048] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0049] 1. In the present invention, the ceramic package base produced by the two-step degreasing method has relatively few defects such as pores and cracks. When sodium polyacrylate is used as dispersant A and dispersant B, the edges and corners of the ceramic package base are more distinct. The modified powder is obtained by modifying the alumina powder. Sebacic acid can modify the surface potential of the alumina powder, wherein a part of the carboxyl groups will form coordination bonds or ionic bonds with the atoms or ions on the surface of the alumina powder, thereby reducing the surface energy of the alumina powder. The ceramic slurry subsequently produced using the modified powder as a raw material has low internal friction, thereby reducing the viscosity of the ceramic slurry. The other part of the carboxyl groups are bridged on the surface of the alumina powder by forming hydrogen bonds, thereby changing the potential on the surface of the alumina powder. The alumina powders repel each other due to the same charges, thereby reducing contact and collision, thereby improving the stability of the ceramic slurry.

[0050] 2. In the present invention, the viscosity is reduced while ensuring the solid content of the ceramic slurry, which is beneficial to improving the dispersibility of the ceramic slurry and adapting to the requirements of photocuring printing. Increasing the solid content while meeting the rheological properties of the ceramic slurry helps to improve printing accuracy and is beneficial to reducing the proportion of organic matter in the later degreasing and sintering process, avoiding defects such as cracking of the green body due to pyrolysis and volatilization of organic matter, thereby ensuring the density and performance of the ceramic body.

[0051] 3. In the present invention, sodium polyacrylate is used as a dispersant for preparing ceramic slurry. Sodium polyacrylate is a long-chain polymer electrolyte, which can not only enhance the electrostatic stabilization of ceramic slurry, but also has a steric stabilization effect, thereby enhancing the dispersion effect of alumina ceramic slurry. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 A schematic diagram of a process flow of a ceramic packaging base and a manufacturing method thereof proposed by the present invention;

[0053] Figure 2 A schematic diagram of the manufacturing process of a ceramic packaging base and a manufacturing method thereof proposed by the present invention;

[0054] Figure 3 A schematic diagram of a process for preparing a ceramic packaging base and a ceramic slurry in a method for preparing the same proposed by the present invention;

[0055] Figure 4 A schematic diagram of a process for preparing a conductive paste in a ceramic packaging base and a manufacturing method thereof proposed by the present invention;

[0056] Figure 5 The present invention provides a ceramic packaging base and a schematic diagram of the carbon-based conductive paste preparation process in the manufacturing method thereof. DETAILED DESCRIPTION

[0057] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0058] Embodiment 1

[0059] A ceramic packaging base comprises a ceramic layer and a conductive layer, wherein the ceramic layer and the conductive layer are arranged adjacent to each other;

[0060] The raw material of the ceramic layer includes ceramic slurry, and the ceramic slurry includes the following components: modified powder A, trimethylolpropane triacrylate A, 1,6-hexanediol diacrylate A, photoinitiator A and sodium polyacrylate A;

[0061] The raw material of the conductive layer includes a conductive paste, and the conductive paste includes the following components: a conductive phase, a carrier solvent, a modified powder B, trimethylolpropane triacrylate B, 1,6-hexanediol diacrylate B, a photoinitiator B and sodium polyacrylate B;

[0062] In the conductive paste, the weight ratio of the conductive phase to the modified powder B is 1:0.05-0.25;

[0063] The ceramic slurry comprises the following components in parts by weight: 70 parts of modified powder A, 2 parts of trimethylolpropane triacrylate A, 4 parts of 1,6-hexanediol diacrylate A, 2 parts of photoinitiator and 2 parts of sodium polyacrylate;

[0064] The conductive paste comprises the following components in parts by weight: 16 parts of conductive phase, 1 part of carrier solvent, 4 parts of modified powder, 4 parts of trimethylolpropane triacrylate, 12 parts of 1,6-hexanediol diacrylate, 2 parts of photoinitiator and 2 parts of sodium polyacrylate;

[0065] A method for manufacturing a ceramic package base comprises the following steps:

[0066] S1: preparing ceramic slurry and conductive slurry respectively;

[0067] S2: loading the ceramic slurry and the conductive slurry into the material tank of the photocuring printing device respectively, and controlling the preparation process by a program according to the designed ceramic package base model;

[0068] S3: laying the ceramic slurry to obtain a ceramic layer, irradiating it with reactive light to solidify it, laying the conductive slurry to obtain a conductive layer, and irradiating it with reactive light to solidify it;

[0069] S4: repeating step S3, photocuring printing the ceramic layer and the conductive layer to form a body of the ceramic package base;

[0070] S5: punching holes, filling via holes, laminating and printing metal paste on the obtained green body, drying and degreasing the green body of the ceramic package base in sequence, and then sintering it into porcelain, finally obtaining the ceramic package base;

[0071] In the degreasing process, the dried green body is first degreased in a vacuum environment, and then decarbonized in air for a second degreasing process;

[0072] The heating rate of the degreasing curve in the air environment is about 0.9°C / min;

[0073] Based on the decomposition temperature of trimethylolpropane triacrylate and 1,6-hexanediol diacrylate for full reaction with oxygen, and the thermal decomposition temperature of dispersant A, three temperature nodes are set in the degreasing heating stage to facilitate full thermal decomposition of trimethylolpropane triacrylate, 1,6-hexanediol diacrylate and dispersant A.

[0074] Embodiment 2

[0075] A ceramic packaging base comprises a ceramic layer and a conductive layer, wherein the ceramic layer and the conductive layer are arranged adjacent to each other;

[0076] The raw material of the ceramic layer includes ceramic slurry, and the ceramic slurry includes the following components: modified powder A, trimethylolpropane triacrylate A, 1,6-hexanediol diacrylate A, photoinitiator A and sodium polyacrylate A;

[0077] The raw material of the conductive layer includes a conductive paste, and the conductive paste includes the following components: a conductive phase, a carrier solvent, a modified powder B, trimethylolpropane triacrylate B, 1,6-hexanediol diacrylate B, a photoinitiator B and sodium polyacrylate B;

[0078] In the conductive paste, the weight ratio of the conductive phase to the modified powder B is 1:0.05-0.25;

[0079] The ceramic slurry comprises the following components in parts by weight: 80 parts of modified powder A, 18 parts of trimethylolpropane triacrylate A, 30 parts of 1,6-hexanediol diacrylate A, 4 parts of photoinitiator A and 5 parts of sodium polyacrylate;

[0080] The conductive paste comprises the following components in parts by weight: 72 parts of conductive phase, 6 parts of carrier solvent, 18 parts of modified powder B, 16 parts of trimethylolpropane triacrylate B, 48 parts of 1,6-hexanediol diacrylate B, 5 parts of photoinitiator B and 5 parts of sodium polyacrylate;

[0081] A method for manufacturing a ceramic package base comprises the following steps:

[0082] S1: preparing ceramic slurry and conductive slurry respectively;

[0083] S2: loading the ceramic slurry and the conductive slurry into the material tank of the photocuring printing device respectively, and controlling the preparation process by a program according to the designed ceramic package base model;

[0084] S3: laying the ceramic slurry to obtain a ceramic layer, irradiating it with reactive light to solidify it, laying the conductive slurry to obtain a conductive layer, and irradiating it with reactive light to solidify it;

[0085] S4: repeating step S3, photocuring printing the ceramic layer and the conductive layer to form a body of the ceramic package base;

[0086] S5: punching holes, filling via holes, laminating and printing metal paste on the obtained green body, drying and degreasing the green body of the ceramic package base in sequence, and then sintering it into porcelain, finally obtaining the ceramic package base;

[0087] In the degreasing process, the dried green body is first degreased in a vacuum environment, and then decarbonized in air for a second degreasing process;

[0088] The heating rate of the degreasing curve in the air environment is about 0.9°C / min;

[0089] Based on the decomposition temperature of trimethylolpropane triacrylate and 1,6-hexanediol diacrylate for full reaction with oxygen, and the thermal decomposition temperature of dispersant A, three temperature nodes are set in the degreasing heating stage to facilitate full thermal decomposition of trimethylolpropane triacrylate, 1,6-hexanediol diacrylate and dispersant A.

[0090] Embodiment 3

[0091] A ceramic packaging base comprises a ceramic layer and a conductive layer, wherein the ceramic layer and the conductive layer are arranged adjacent to each other;

[0092] The raw material of the ceramic layer includes ceramic slurry, and the ceramic slurry includes the following components: modified powder A, trimethylolpropane triacrylate A, 1,6-hexanediol diacrylate A, photoinitiator A and sodium polyacrylate A;

[0093] The raw material of the conductive layer includes a conductive paste, and the conductive paste includes the following components: a conductive phase, a carrier solvent, a modified powder B, trimethylolpropane triacrylate B, 1,6-hexanediol diacrylate B, a photoinitiator B and sodium polyacrylate B;

[0094] In the conductive paste, the weight ratio of the conductive phase to the modified powder B is 1:0.05-0.25;

[0095] The ceramic slurry comprises the following components in parts by weight: 75 parts of modified powder A, 10 parts of trimethylolpropane triacrylate A, 17 parts of 1,6-hexanediol diacrylate A, 3 parts of photoinitiator A and 3.5 parts of sodium polyacrylate;

[0096] The conductive paste comprises the following components in parts by weight: 39 parts of conductive phase, 3.5 parts of carrier solvent, 11 parts of modified powder B, 10 parts of trimethylolpropane triacrylate B, 30 parts of 1,6-hexanediol diacrylate B, 3.5 parts of photoinitiator B and 3.5 parts of sodium polyacrylate B;

[0097] A method for manufacturing a ceramic package base comprises the following steps:

[0098] S1: preparing ceramic slurry and conductive slurry respectively;

[0099] S2: loading the ceramic slurry and the conductive slurry into the material tank of the photocuring printing device respectively, and controlling the preparation process by a program according to the designed ceramic package base model;

[0100] S3: laying the ceramic slurry to obtain a ceramic layer, irradiating it with reactive light to solidify it, laying the conductive slurry to obtain a conductive layer, and irradiating it with reactive light to solidify it;

[0101] S4: repeating step S3, photocuring printing the ceramic layer and the conductive layer to form a body of the ceramic package base;

[0102] S5: punching holes, filling via holes, laminating and printing metal paste on the obtained green body, drying and degreasing the green body of the ceramic package base in sequence, and then sintering it into porcelain, finally obtaining the ceramic package base;

[0103] In the degreasing process, the dried green body is first degreased in a vacuum environment, and then decarbonized in air for a second degreasing process;

[0104] The heating rate of the degreasing curve in the air environment is about 0.9°C / min;

[0105] Based on the decomposition temperature of trimethylolpropane triacrylate and 1,6-hexanediol diacrylate for full reaction with oxygen, and the thermal decomposition temperature of dispersant A, three temperature nodes are set in the degreasing heating stage to facilitate full thermal decomposition of trimethylolpropane triacrylate, 1,6-hexanediol diacrylate and dispersant A.

[0106] Compared with the first and second embodiments, the third embodiment reduces the viscosity while ensuring the solid content of the slurry, which is beneficial to improving the dispersibility of the slurry and meeting the requirements of light-curing printing.

[0107] Embodiment 4

[0108] A ceramic packaging base comprises a ceramic layer and a conductive layer, wherein the ceramic layer and the conductive layer are arranged adjacent to each other;

[0109] The raw material of the ceramic layer includes ceramic slurry, and the ceramic slurry includes the following components: modified powder A, trimethylolpropane triacrylate A, 1,6-hexanediol diacrylate A, photoinitiator A and sodium polyacrylate A;

[0110] The raw material of the conductive layer includes a conductive paste, and the conductive paste includes the following components: a conductive phase, a carrier solvent, a modified powder B, trimethylolpropane triacrylate B, 1,6-hexanediol diacrylate B, a photoinitiator B and sodium polyacrylate B;

[0111] In the conductive paste, the weight ratio of the conductive phase to the modified powder B is 1:0.05-0.25;

[0112] The ceramic slurry comprises the following components in parts by weight: 75 parts of modified powder A, 10 parts of trimethylolpropane triacrylate A, 17 parts of 1,6-hexanediol diacrylate A, 3 parts of photoinitiator A and 3.5 parts of sodium polyacrylate;

[0113] The conductive paste comprises the following components in parts by weight: 39 parts of conductive phase, 3.5 parts of carrier solvent, 11 parts of modified powder B, 10 parts of trimethylolpropane triacrylate B, 30 parts of 1,6-hexanediol diacrylate B, 3.5 parts of photoinitiator B and 3.5 parts of sodium polyacrylate B;

[0114] A method for manufacturing a ceramic package base comprises the following steps:

[0115] S1: preparing ceramic slurry and conductive slurry respectively;

[0116] S2: loading the ceramic slurry and the conductive slurry into the material tank of the photocuring printing device respectively, and controlling the preparation process by a program according to the designed ceramic package base model;

[0117] S3: laying the ceramic slurry to obtain a ceramic layer, irradiating it with reactive light to solidify it, laying the conductive slurry to obtain a conductive layer, and irradiating it with reactive light to solidify it;

[0118] S4: repeating step S3, photocuring printing the ceramic layer and the conductive layer to form a body of the ceramic package base;

[0119] S5: punching holes, filling via holes, laminating and printing metal paste on the obtained green body, drying and degreasing the green body of the ceramic package base in sequence, and then sintering it into porcelain, finally obtaining the ceramic package base;

[0120] In the degreasing process, the dried green body is first degreased in a vacuum environment, and then decarbonized in air for a second degreasing process;

[0121] The heating rate of the degreasing curve in the air environment is about 0.9°C / min;

[0122] Based on the decomposition temperature of the trimethylolpropane triacrylate and 1,6-hexanediol diacrylate at which they fully react with oxygen, and the thermal decomposition temperature of the dispersant A, three temperature nodes are set in the degreasing heating stage to facilitate the full thermal decomposition of the trimethylolpropane triacrylate, 1,6-hexanediol diacrylate and the dispersant A;

[0123] The method for preparing the modified powder comprises:

[0124] Add dispersant A and ethanol solution into an ultrasonic device together, and control the ultrasonic device to promote the dissolution of dispersant A;

[0125] After the dispersant A is completely dissolved, a proper amount of alumina powder is weighed in proportion, and the weighed alumina powder is added into the ball mill together with the dispersant and ethanol solution in the ultrasonic equipment;

[0126] After the operation program set by the ball mill is completed, the mixed material in the ball mill is transferred to a vacuum drying device and dried in a vacuum environment at 58°C to obtain a modified powder;

[0127] The ball milling mixing speed of the ball mill is 280r / min, the ball milling time is 3.6h, the operation procedure of the ball mill is clockwise rotation for 8min, counterclockwise rotation for 8min, and the interval is 4min in between, and the dispersant A is sebacic acid;

[0128] Sodium polyacrylate is used as a dispersant for ceramic slurry preparation. Sodium polyacrylate is a long-chain polymer electrolyte that can not only enhance the electrostatic stabilization of ceramic slurry, but also has a steric stabilization effect, thereby enhancing the dispersion effect of alumina ceramic slurry.

[0129] The method for preparing the ceramic slurry comprises:

[0130] Add trimethylolpropane triacrylate and 1,6-hexanediol diacrylate in a mass ratio of 1:1 into a magnetic stirring device, and after the two are mixed evenly, add a photoinitiator with a mass fraction of 1.4%;

[0131] After the photoinitiator and the former are evenly mixed, the mixture is taken out and transferred to a three-roll mill. During this process, a certain amount of sodium polyacrylate needs to be added to the three-roll mill.

[0132] After the sodium polyacrylate is evenly mixed with the former, a premixed resin is obtained, the premixed resin is taken out and added to a ball mill, and the modified powder is added to the ball mill for ball milling. After the modified powder and the premixed resin are fully mixed, the premixed resin is taken out and transferred to a vacuum degassing device for vacuum degassing to obtain an alumina ceramic slurry, which is kept away from light for later use;

[0133] Modified powder is obtained by modifying alumina powder. Sebacic acid can modify the surface potential of alumina powder. A part of the carboxyl groups will form coordination bonds or ionic bonds with the atoms or ions on the surface of alumina powder, thereby reducing the surface energy of alumina powder. The ceramic slurry subsequently made with the modified powder as raw material has low internal friction.

[0134] Embodiment 5

[0135] A ceramic packaging base comprises a ceramic layer and a conductive layer, wherein the ceramic layer and the conductive layer are arranged adjacent to each other;

[0136] The raw material of the ceramic layer includes ceramic slurry, and the ceramic slurry includes the following components: modified powder A, trimethylolpropane triacrylate A, 1,6-hexanediol diacrylate A, photoinitiator A and sodium polyacrylate A;

[0137] The raw material of the conductive layer includes a conductive paste, and the conductive paste includes the following components: a conductive phase, a carrier solvent, a modified powder B, trimethylolpropane triacrylate B, 1,6-hexanediol diacrylate B, a photoinitiator B and sodium polyacrylate B;

[0138] In the conductive paste, the weight ratio of the conductive phase to the modified powder B is 1:0.05-0.25;

[0139] The ceramic slurry comprises the following components in parts by weight: 75 parts of modified powder A, 10 parts of trimethylolpropane triacrylate A, 17 parts of 1,6-hexanediol diacrylate A, 3 parts of photoinitiator A and 3.5 parts of sodium polyacrylate;

[0140] The conductive paste comprises the following components in parts by weight: 39 parts of conductive phase, 3.5 parts of carrier solvent, 11 parts of modified powder B, 10 parts of trimethylolpropane triacrylate B, 30 parts of 1,6-hexanediol diacrylate B, 3.5 parts of photoinitiator B and 3.5 parts of sodium polyacrylate B;

[0141] A method for manufacturing a ceramic package base comprises the following steps:

[0142] S1: preparing ceramic slurry and conductive slurry respectively;

[0143] S2: loading the ceramic slurry and the conductive slurry into the material tank of the photocuring printing device respectively, and controlling the preparation process by a program according to the designed ceramic package base model;

[0144] S3: laying the ceramic slurry to obtain a ceramic layer, irradiating it with reactive light to solidify it, laying the conductive slurry to obtain a conductive layer, and irradiating it with reactive light to solidify it;

[0145] S4: repeating step S3, photocuring printing the ceramic layer and the conductive layer to form a body of the ceramic package base;

[0146] S5: punching holes, filling via holes, laminating and printing metal paste on the obtained green body, drying and degreasing the green body of the ceramic package base in sequence, and then sintering it into porcelain, finally obtaining the ceramic package base;

[0147] In the degreasing process, the dried green body is first degreased in a vacuum environment, and then decarbonized in air for a second degreasing process;

[0148] The heating rate of the degreasing curve in the air environment is about 0.9°C / min;

[0149] Based on the decomposition temperature of the trimethylolpropane triacrylate and 1,6-hexanediol diacrylate at which they fully react with oxygen, and the thermal decomposition temperature of the dispersant A, three temperature nodes are set in the degreasing heating stage to facilitate the full thermal decomposition of the trimethylolpropane triacrylate, 1,6-hexanediol diacrylate and the dispersant A;

[0150] The preparation method of the conductive paste comprises:

[0151] First, dispersant B is added into a ball mill containing a carrier solvent and stirred to mix evenly to obtain a dispersion system with a mass fraction of 1%;

[0152] Then, the conductive phase powder is added to the ball mill, and the obtained conductive phase slurry is placed in an ultrasonic dispersion device for ultrasonic dispersion treatment for 16 minutes;

[0153] After the ultrasonic dispersion treatment is completed, the mixture is water-milled for 28 min using a sand mill at a ball-to-material mass ratio of 10:1 and a rotation speed of 1350 r / min;

[0154] After the water milling treatment, the mixture was sieved through 120 meshes and then subjected to a secondary ultrasonic dispersion treatment for 24 min to obtain a conductive slurry.

[0155] It is beneficial to reduce the proportion of organic matter in the later degreasing and sintering process, avoid defects such as cracking of the green body caused by pyrolysis and volatilization of organic matter, and ensure the density and performance of the ceramic body.

[0156] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A ceramic package base, characterized in that: It comprises a ceramic layer and a conductive layer, wherein the ceramic layer and the conductive layer are arranged adjacent to each other; The raw material of the ceramic layer includes ceramic slurry, and the ceramic slurry includes the following components: modified powder A, trimethylolpropane triacrylate A, 1,6-hexanediol diacrylate A, photoinitiator A and sodium polyacrylate A; The raw material of the conductive layer includes a conductive paste, and the conductive paste includes the following components: a conductive phase, a carrier solvent, a modified powder B, trimethylolpropane triacrylate B, 1,6-hexanediol diacrylate B, a photoinitiator B and sodium polyacrylate B; In the conductive paste, the weight ratio of the conductive phase to the modified powder B is 1:0.05-0.

25.

2. The ceramic package base according to claim 1, characterized in that: The ceramic slurry comprises the following components in parts by weight: 70-80 parts of modified powder A, 2-18 parts of trimethylolpropane triacrylate A, 4-30 parts of 1,6-hexanediol diacrylate A, 2-4 parts of photoinitiator A and 2-5 parts of sodium polyacrylate A.

3. The ceramic package base according to claim 1, characterized in that: The conductive paste comprises the following components in parts by weight: 16-72 parts of a conductive phase, 1-6 parts of a carrier solvent, 4-18 parts of a modified powder, 4-16 parts of trimethylolpropane triacrylate, 12-48 parts of 1,6-hexanediol diacrylate, 2-5 parts of a photoinitiator and 2-5 parts of sodium polyacrylate.

4. The ceramic package base according to claim 1, characterized in that: The method for preparing the modified powder comprises: Add dispersant A and ethanol solution into an ultrasonic device together, and control the ultrasonic device to promote the dissolution of dispersant A; After the dispersant A is completely dissolved, a proper amount of alumina powder is weighed in proportion, and the weighed alumina powder is added into the ball mill together with the dispersant and ethanol solution in the ultrasonic equipment; After the operation program set by the ball mill is completed, the mixed material in the ball mill is transferred to a vacuum drying device and dried in a vacuum environment at 58° C. to obtain a modified powder.

5. The ceramic package base according to claim 4, characterized in that: The ball milling mixing speed of the ball mill is 280r / min, the ball milling time is 3.6h, and the operation program of the ball mill is clockwise rotation for 8min, counterclockwise rotation for 8min, and the interval is 4min; The dispersant A is sebacic acid.

6. The ceramic package base according to claim 1, characterized in that: The method for preparing the ceramic slurry comprises: Add trimethylolpropane triacrylate and 1,6-hexanediol diacrylate in a mass ratio of 1:1 into a magnetic stirring device, and after the two are mixed evenly, add a photoinitiator with a mass fraction of 1.4%; After the photoinitiator and the former are evenly mixed, the mixture is taken out and transferred to a three-roll mill. During this process, a certain amount of sodium polyacrylate needs to be added to the three-roll mill. After sodium polyacrylate is evenly mixed with the former, a premixed resin is obtained, the premixed resin is taken out and added to a ball mill, and the modified powder is added to the ball mill for ball milling. After the modified powder and the premixed resin are fully mixed, they are taken out and transferred to a vacuum degassing device for vacuum degassing to obtain an alumina ceramic slurry, which is kept away from light for later use.

7. The ceramic package base according to claim 1, characterized in that: The preparation method of the conductive paste comprises: First, dispersant B is added into a ball mill containing a carrier solvent and stirred to mix evenly to obtain a dispersion system with a mass fraction of 1%; Then, the conductive phase powder is added to the ball mill, and the obtained conductive phase slurry is placed in an ultrasonic dispersion device for ultrasonic dispersion treatment for 16 minutes; After the ultrasonic dispersion treatment is completed, the mixture is water-milled for 28 min using a sand mill at a ball-to-material mass ratio of 10:1 and a rotation speed of 1350 r / min; After the water grinding treatment, the mixture was sieved through 120 meshes and then subjected to a secondary ultrasonic dispersion treatment for 24 minutes to finally obtain a conductive slurry.

8. The ceramic package base according to claim 7, characterized in that: The conductive phase is one or more of graphite, carbon black, graphene and carbon nanotubes; The dispersant B is one or more of polyvinyl pyrrolidone, sodium polyacrylate and sodium lignin sulfonate, and the dispersant B is preferably sodium polyacrylate; The carrier solvent is one or more of dimethylformamide, N-methylpyrrolidone and deionized water, and the carrier solvent is preferably deionized water.

9. A method for manufacturing a ceramic package base according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1: preparing ceramic slurry and conductive slurry respectively; S2: loading the ceramic slurry and the conductive slurry into the material tank of the photocuring printing device respectively, and controlling the preparation process by a program according to the designed ceramic package base model; S3: laying the ceramic slurry to obtain a ceramic layer, irradiating it with reactive light to solidify it, laying the conductive slurry to obtain a conductive layer, and irradiating it with reactive light to solidify it; S4: repeating step S3, photocuring printing the ceramic layer and the conductive layer to form a body of the ceramic package base; S5: the obtained green body is punched, the via holes are filled, laminated and metal paste is printed, the green body of the ceramic package base is dried and degreased in sequence, and then sintered into porcelain, and finally the ceramic package base is obtained.

10. The method for manufacturing a ceramic package base according to claim 9, characterized in that: In the degreasing process, the dried green body is first degreased in a vacuum environment, and then decarbonized in air for a second degreasing process; The heating rate of the degreasing curve in the air environment is about 0.9°C / min; Based on the decomposition temperature of trimethylolpropane triacrylate and 1,6-hexanediol diacrylate for full reaction with oxygen, and the thermal decomposition temperature of dispersant A, three temperature nodes are set in the degreasing heating stage to facilitate full thermal decomposition of trimethylolpropane triacrylate, 1,6-hexanediol diacrylate and dispersant A.

Citation Information

Cited By

  • Preparation and application of YAG (yttrium aluminum garnet) ceramic slurry for photocuring molding

    CN119683990A

  • Preparation and application of a YAG ceramic slurry for photocuring.

    CN119683990B