Preparation method and application of current collector with high binding force

By using ultra-thin porous nanoplate and metal foil in the battery, the nanowires are prepared and combined with conductive glue, the thermal deformation and insufficient binding force of the composite liquid collector is solved, and the cycle life and safety performance of the battery are significantly improved.

CN119008962AActive Publication Date: 2024-11-22JIANGYIN NANOPORE INNOVATIVE MATERIALS TECH LTD

Patent Information

Application Number
CN202411376980.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-22
Estimated Expiration
2044-09-30

AI Technical Summary

Technical Problem

The thermal deformation and insufficient binding force caused by heat shrinkage in lithium-ion batteries have caused the battery energy density and cycle life to decrease, and there are safety hazards.

Method used

The nanowires are prepared by ultra-thin porous nanoplate and metal foil by ultrasonic imprinting. The nanowires are sprayed on the surface of the polymer film and combined with conductive glue. The interlaced adhesion of the nanowires is used to increase the binding force of the current collector, and the modified polymerization is selected. Acrylic films to enhance mechanical properties.

Benefits of technology

It significantly improves the binding force of the current collector, extends the cycle life of the battery, enhances the safety performance of the battery, and reduces the risk of film fracture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the field of composite current collectors, and particularly discloses a preparation method and application of a high-binding-force current collector. The preparation method comprises the following steps: S1, taking the aluminum oxide ultrathin porous nano-plate and the metal foil, and cleaning; cutting into square chips; s2, uniformly coating the aluminum oxide ultrathin porous nano-plate with a solid lubricant, placing the aluminum oxide ultrathin porous nano-plate on a metal foil, and carrying out ultrasonic imprinting to obtain an aluminum oxide ultrathin porous nano-plate / substrate with a metal rod; s3, immersing the aluminum oxide ultrathin porous nano plate / substrate stack obtained in the step S2 into a NaOH solution to obtain a metal substrate with exposed nanowires; s4, the nanowires on the metal substrate are cut off through the nanometer laser cutting technology, and the nanowires are obtained; and S5, uniformly blade-coating a conductive adhesive on the surface of the polymer film, spraying nanowires, and curing under the conditions that the ultraviolet light intensity is 50-200mW / cm and the temperature is 110-120 DEG C to obtain the current collector.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of composite current collectors, and specifically discloses a preparation method and application of a current collector with high binding force. Background Art

[0002] With the rapid development of new energy and electronic technology, the requirements for battery cycle life, safety performance, and energy density are getting higher and higher. As an important component of the battery, the performance of the current collector will directly affect the performance of the battery.

[0003] At present, the positive and negative electrodes in lithium batteries and sodium batteries mostly use copper foil and aluminum foil as current collectors. This type of current collector has high cost and quality, which is not conducive to controlling battery costs and improving energy density. In this regard, composite foil has obvious advantages over traditional foils. Composite foil current collectors are usually a "sandwich" structure, with a polymer high molecular layer as the inner layer and metal conductive layers on both sides. Since the metal layer on the surface of the composite current collector is thinner and the polymer layer inside is lighter, it can greatly reduce the overall weight of the current collector and increase the energy density of lithium-ion batteries; at the same time, the thinner metal layer on the surface of the composite current collector is easier to disconnect than the traditional foil current collector when the lithium-ion battery has thermal runaway, thereby isolating the connection between the active material and the current collector and preventing the lithium-ion battery from continuing thermal runaway.

[0004] However, although the composite foil current collector has the advantages of low cost and light weight, a large amount of heat will be generated during battery cycling, causing the composite current collector to change in volume. Excessive heat shrinkage will cause the composite current collector to have a large thermal deformation. Most of the current composite current collector base films are made of PP (polypropylene) material, which has poor bonding strength, leading to deformation of the film surface and shedding of the copper layer, which seriously reduces the energy density and cycle life of the battery, and also brings safety problems to the battery. Therefore, it is of great significance to study a method for preparing a current collector with high bonding strength. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing and applying a current collector with high binding force, so as to solve the problems raised in the above-mentioned background technology.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: A method for preparing a current collector with high binding force, comprising the following steps: S1: taking an ultra-thin porous alumina nanoplate and a metal foil, washing them (first washing with deionized water for 5 to 10 minutes, then washing with isopropanol for 5 to 10 minutes, and finally washing with ethanol for 5 to 10 minutes); cutting them into square chips with a side length of 1 to 5 mm; S2: Coat a solid lubricant in the ultra-thin porous nanoplate of aluminum oxide, place it on top of the metal foil, and use an ultrasonic embossing device for ultrasonic embossing at a frequency of 15-25kHz to obtain an ultra-thin porous nanoplate of aluminum oxide / substrate with a metal rod; S3: The alumina ultra-thin porous nanoplate / substrate stack obtained in step S2 is immersed in a 1M NaOH solution for 2 hours to obtain a metal substrate with nanowires exposed; the nanowires are immersed in a water solvent containing 1.5wt% chromic acid and 6wt% phosphoric acid for 3 hours at a temperature of 70°C; S4: using nano laser cutting technology to cut away the nanowires on the metal substrate to obtain nanowires; S5: Evenly apply conductive glue on the surface of the polymer film, control the surface temperature to 70°C, and spray nanowires; use nanowire dispersion when spraying nanowires, the nanowire dispersion is 2~10mg / ml nanowire ethanol dispersion; spray speed 10~20mm / s; atomization pressure 5~30MPa; nozzle diameter 50~200μm; after spraying, cure for 5min under ultraviolet light intensity 50~200mW / cm² and temperature 110~120°C to obtain a current collector.

[0007] When spraying nanowires, a nanowire ethanol dispersion is used (the nanowires are dispersed in ethanol); if the nanowire concentration is too high, the nanowires may agglomerate, affecting the spraying effect; if the concentration is too low, a continuous and uniform coating may not be formed; The speed of spraying nanowires will affect the deposition rate and distribution uniformity of nanowires. If the spraying speed is too fast, the nanowires may not have enough time to spread evenly, while if the speed is too slow, the production efficiency may be affected. The atomization pressure of the nanowire spraying needs to be controlled. The appropriate atomization pressure can fully atomize the nanowire suspension to form droplets of uniform size, thereby ensuring the quality of the coating. The nozzle size for spraying nanowires will affect the size of the droplets and the spray flow rate. A smaller nozzle size can produce finer droplets, which is conducive to forming a uniform coating, but may lead to reduced spraying efficiency; a larger nozzle size has the opposite effect, so the appropriate nozzle size should also be selected.

[0008] More optimally, the preparation of the current collector includes the following steps: evenly scrape the surface of the polymer film with conductive glue, control the surface temperature to 70°C, and spray nanowires; use a nanowire dispersion when spraying the nanowires, and the nanowire dispersion is a 6mg / ml nanowire ethanol dispersion; the spraying speed is 15mm / s; the atomization pressure is 20MPa; the nozzle diameter is 100μm; after the spraying is completed, cure for 5min under ultraviolet light intensity of 75mW / cm² and temperature of 120°C to obtain the current collector.

[0009] Preferably, the cleaning process is: first use deionized water to clean for 10 minutes, then use isopropanol to clean for 10 minutes, and finally use ethanol to clean for 10 minutes.

[0010] More optimally, the thickness of the alumina ultra-thin porous nanoplate is 500-800 nm, and the size of the nanopores is 100-300 nm.

[0011] More optimally, the thickness of the alumina ultra-thin porous nanoplate is 600 nm.

[0012] More optimally, the size of the metal rod is 100-300 nm.

[0013] Preferably, the metal foil is a copper metal foil with a thickness of 100 μm.

[0014] More optimally, the solid lubricant is carbon 60, and the coating thickness is 80-120 nm.

[0015] More optimally, the solid lubricant is carbon 60, and the coating thickness is 100 nm.

[0016] More optimally, the polymer film is a BOPP polypropylene film with a thickness of 4 to 10 μm.

[0017] Preferably, the polymer film is a BOPP polypropylene film with a thickness of 5 μm (manufacturer: Jiadeli, model: 6014H).

[0018] More optimally, the thickness of the conductive adhesive is 0.8-1 μm.

[0019] Preferably, the thickness of the conductive adhesive is 1 μm.

[0020] More optimally, the polymer membrane is a modified polypropylene membrane, and the specific preparation method includes the following steps: S1: taking hydroxyethyl methacrylate, polypropylene, and benzoyl peroxide, mixing, heating to 200-210°C, reacting for 2-3 hours, and obtaining an intermediate; taking the intermediate, adding it to N,N-dimethylformamide, stirring evenly, adding anhydrous sodium carbonate and bis(4-nitrophenyl) phosphate, heating to 180-190°C under a nitrogen atmosphere, reacting for 10-12 hours, and refluxing under reduced pressure to obtain modified polypropylene; S2: Melting and extruding the modified polypropylene; forming the obtained melt cast sheet, and sequentially performing longitudinal stretching and transverse stretching, heat preservation, and corona treatment to obtain a modified polypropylene film.

[0021] More optimally, the intermediate comprises the following raw materials, calculated by mass: 15-20 parts of hydroxyethyl methacrylate, 100 parts of polypropylene, and 1-2 parts of benzoyl peroxide; the modified polypropylene comprises the following raw materials, calculated by mass: 100 parts of the intermediate, 150-180 parts of N,N-dimethylformamide, 1-2 parts of anhydrous sodium carbonate, and 25-30 parts of bis(4-nitrophenyl) phosphate.

[0022] More optimally, the polypropylene melt index is 2.2 g / 10 min.

[0023] More optimally, the polypropylene is S51655 produced by Shanghai Yuanye.

[0024] More optimally, the specific preparation process of the modified polypropylene film comprises the following steps: melt-extrude the modified polypropylene; cast the obtained melt through a cooling roller and a high-pressure air knife, and then sequentially use a longitudinal stretching machine and a transverse stretching machine to perform longitudinal stretching and transverse stretching; the temperature of the cooling roller is 80-100°C, the gas temperature of the high-pressure air knife is 50-70°C, and the blowing speed is 130-150m / s; the stretching temperature of the longitudinal stretching is 130-150°C, the setting temperature is 140-160°C, preferably 150°C, and the stretching ratio is 5-8; the stretching temperature of the transverse stretching is 150-170°C, the setting temperature is 170-180°C, and the stretching ratio is 7-13; keep warm at 110-140°C for 3-5min, and perform corona treatment; the corona power is 50-100kW, and the line speed is 50-300m / min; and the modified polypropylene film is obtained.

[0025] More optimally, the above current collector can be used to prepare a battery.

[0026] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: (1) The present invention prepares nanowires by ultrasonic embossing, and then sprays the nanowires on the surface of a polymer film to prepare a composite current collector; the nanowires have good bonding strength with the polymer film, and will not cause thermal damage to the polymer base film during the process, and the internal stress is small, which can comprehensively improve the quality of the film surface. The nanowires are densely stacked and staggered, and during the stretching process, the nanorods are interlaced and adhered to each other, which will not damage the base film. They have strong tensile strength, can reduce film breakage, and reduce risks. The composite current collector under this process can significantly improve the safety performance of the battery and increase the cycle life of the battery.

[0027] (2) The polymer film is modified polypropylene film. During the modification process, the hydrogen on the tertiary carbon of polypropylene is first captured by free radicals under the action of an initiator to generate polypropylene macromolecular free radicals, and then hydroxyethyl methacrylate is grafted on the side chain, and then di(4-nitrophenyl) phosphate is grafted by the reaction of -OH and -NO2. The introduction of benzene rings can improve the mechanical properties of polypropylene, and the phosphate group can induce polypropylene crystallization, making the arrangement of polypropylene molecular segments more regular, improving mechanical properties, reducing breakage or deformation during peeling, and improving peeling force. The amount of hydroxyethyl methacrylate added needs to be controlled, because too many side chains will also reduce the crystallinity of polypropylene, which is not conducive to improving mechanical properties. Too few side chain grafts will result in an insignificant modification effect and a small improvement in peeling force. The choice of polypropylene also has an important influence. Polypropylene with a small molecular weight has good crystallization properties but its mechanical properties are not as good as those with a large molecular weight. If the molecular weight of polypropylene is too large, it will affect the crystallinity. Therefore, the choice of polypropylene also needs to be controlled. In summary, the polypropylene model and the amount of each raw material added need to be controlled to obtain a modified polypropylene film with good surface adhesion, good storage stability, and good mechanical properties, thereby improving peeling strength. DETAILED DESCRIPTION

[0028] The following is a preferred implementation of the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. For ordinary technicians in this technical field, all other embodiments obtained by ordinary technicians in this field without creative work without departing from the principle of the embodiment of the present invention are within the scope of protection of the present invention.

[0029] The following parts are by mass unless otherwise specified; Example 1: S1: Take an alumina ultra-thin porous nanoplate with a nanopore size of 130 nm and a 100 μm thick metal copper foil, first wash them with deionized water for 10 min, then wash them with isopropanol for 10 min, and finally wash them with ethanol for 10 min; cut them into square chips with a side length of 5 mm; S2: Coating a solid lubricant in the ultra-thin porous nanoplate of aluminum oxide, placing it on top of the metal foil, and ultrasonically imprinting it using a Branson 2000X ultrasonic imprinting device with a frequency of 20 kHz to obtain an ultra-thin porous nanoplate / substrate of aluminum oxide with a copper metal rod of 130 nm in size; S3: immersing the alumina ultrathin porous nanoplate / substrate stack obtained in step S2 in a 1M NaOH solution for 2 h to obtain a metal substrate with nanowires exposed; S4: using nano laser cutting technology to cut away the nanowires on the metal substrate to obtain nanowires; S5: Evenly scrape a conductive glue with a thickness of 1 μm on the surface of the polypropylene film, and spray the nanowires. When spraying the nanowires, a nanowire dispersion is used, and the nanowire dispersion is a 6 mg / ml nanowire ethanol dispersion; the spraying speed is 15 mm / s; the atomization pressure is 20 MPa; the nozzle diameter is 100 μm; after the spraying is completed, it is cured under ultraviolet light and 120°C for 5 minutes to obtain a current collector.

[0030] Example 2: S1: Take an alumina ultra-thin porous nanoplate with a nanopore size of 100 nm and a 100 μm thick metal copper foil, first wash them with deionized water for 10 min, then wash them with isopropanol for 10 min, and finally wash them with ethanol for 10 min; cut them into square chips with a side length of 5 mm; S2: Coating a solid lubricant in the ultra-thin porous nanoplate of aluminum oxide, placing it on top of the metal foil, and ultrasonically imprinting it using a Branson 2000X ultrasonic imprinting device with a frequency of 20 kHz to obtain an ultra-thin porous nanoplate of aluminum oxide / substrate with copper metal rods of 100 nm in size; S3: immersing the alumina ultrathin porous nanoplate / substrate stack obtained in step S2 in a 1M NaOH solution for 2 h to obtain a metal substrate with nanowires exposed; S4: using nano laser cutting technology to cut away the nanowires on the metal substrate to obtain nanowires; S5: Evenly scrape a conductive glue with a thickness of 1 μm on the surface of the polypropylene film, and spray the nanowires. When spraying the nanowires, a nanowire dispersion is used, and the nanowire dispersion is a 6 mg / ml nanowire ethanol dispersion; the spraying speed is 15 mm / s; the atomization pressure is 20 MPa; the nozzle diameter is 100 μm; after the spraying is completed, it is cured under ultraviolet light and 120°C for 5 minutes to obtain a current collector.

[0031] Example 3: S1: Take an alumina ultra-thin porous nanoplate with a nanopore size of 200 nm and a 100 μm thick metal copper foil, first wash them with deionized water for 10 min, then wash them with isopropanol for 10 min, and finally wash them with ethanol for 10 min; cut them into square chips with a side length of 5 mm; S2: Coat a solid lubricant in the ultra-thin porous nanoplate of aluminum oxide, place it on top of the metal foil, and perform ultrasonic embossing using a Branson 2000X ultrasonic embossing device with a frequency of 20 kHz to obtain an ultra-thin porous nanoplate of aluminum oxide / substrate with a copper metal rod with a size of 200 nm; S3: immersing the alumina ultrathin porous nanoplate / substrate stack obtained in step S2 in a 1M NaOH solution for 2 h to obtain a metal substrate with nanowires exposed; S4: using nano laser cutting technology to cut away the nanowires on the metal substrate to obtain nanowires; S5: Evenly scrape a conductive glue with a thickness of 1 μm on the surface of the polypropylene film, and spray the nanowires. When spraying the nanowires, a nanowire dispersion is used, and the nanowire dispersion is a 6 mg / ml nanowire ethanol dispersion; the spraying speed is 15 mm / s; the atomization pressure is 20 MPa; the nozzle diameter is 100 μm; after the spraying is completed, it is cured under ultraviolet light and 120°C for 5 minutes to obtain a current collector.

[0032] Example 4: S1: Take an alumina ultra-thin porous nanoplate with a nanopore size of 300 nm and a 100 μm thick metal copper foil, first wash them with deionized water for 10 min, then wash them with isopropanol for 10 min, and finally wash them with ethanol for 10 min; cut them into square chips with a side length of 5 mm; S2: Coating a solid lubricant in the ultra-thin porous nanoplate of aluminum oxide, placing it on top of the metal foil, and ultrasonically imprinting it using a Branson 2000X ultrasonic imprinting device with a frequency of 20 kHz to obtain an ultra-thin porous nanoplate of aluminum oxide / substrate with a copper metal rod of 300 nm in size; S3: immersing the alumina ultrathin porous nanoplate / substrate stack obtained in step S2 in a 1M NaOH solution for 2 h to obtain a metal substrate with nanowires exposed; S4: using nano laser cutting technology to cut away the nanowires on the metal substrate to obtain nanowires; S5: Evenly scrape a conductive glue with a thickness of 1 μm on the surface of the polypropylene film, and spray the nanowires. When spraying the nanowires, a nanowire dispersion is used, and the nanowire dispersion is a 6 mg / ml nanowire ethanol dispersion; the spraying speed is 15 mm / s; the atomization pressure is 20 MPa; the nozzle diameter is 100 μm; after the spraying is completed, it is cured under ultraviolet light and 120°C for 5 minutes to obtain a current collector.

[0033] Example 5: S1: Take an alumina ultra-thin porous nanoplate with a nanopore size of 130 nm and a 100 μm thick metal copper foil, first wash them with deionized water for 10 min, then wash them with isopropanol for 10 min, and finally wash them with ethanol for 10 min; cut them into square chips with a side length of 5 mm; S2: Coating a solid lubricant in the ultra-thin porous nanoplate of aluminum oxide, placing it on top of the metal foil, and ultrasonically imprinting it using a Branson 2000X ultrasonic imprinting device with a frequency of 15 kHz to obtain an ultra-thin porous nanoplate / substrate of aluminum oxide with a copper metal rod of 130 nm in size; S3: immersing the alumina ultrathin porous nanoplate / substrate stack obtained in step S2 in a 1M NaOH solution for 2 h to obtain a metal substrate with nanowires exposed; S4: using nano laser cutting technology to cut away the nanowires on the metal substrate to obtain nanowires; S5: Evenly scrape a conductive glue with a thickness of 1 μm on the surface of the polypropylene film, and spray the nanowires. When spraying the nanowires, a nanowire dispersion is used, and the nanowire dispersion is a 6 mg / ml nanowire ethanol dispersion; the spraying speed is 15 mm / s; the atomization pressure is 20 MPa; the nozzle diameter is 100 μm; after the spraying is completed, it is cured under ultraviolet light and 120°C for 5 minutes to obtain a current collector.

[0034] Example 6: S1: Take an alumina ultra-thin porous nanoplate with a nanopore size of 130 nm and a 100 μm thick metal copper foil, first wash them with deionized water for 10 min, then wash them with isopropanol for 10 min, and finally wash them with ethanol for 10 min; cut them into square chips with a side length of 5 mm; S2: Coating a solid lubricant in the ultra-thin porous nanoplate of aluminum oxide, placing it on top of the metal foil, and ultrasonically imprinting it using a Branson 2000X ultrasonic imprinting device with a frequency of 25kHz to obtain an ultra-thin porous nanoplate / substrate of aluminum oxide with a copper metal rod of 130nm in size; S3: immersing the alumina ultrathin porous nanoplate / substrate stack obtained in step S2 in a 1M NaOH solution for 2 h to obtain a metal substrate with nanowires exposed; S4: using nano laser cutting technology to cut away the nanowires on the metal substrate to obtain nanowires; S5: Evenly scrape a conductive glue with a thickness of 1 μm on the surface of the polypropylene film, and spray the nanowires. When spraying the nanowires, a nanowire dispersion is used, and the nanowire dispersion is a 6 mg / ml nanowire ethanol dispersion; the spraying speed is 15 mm / s; the atomization pressure is 20 MPa; the nozzle diameter is 100 μm; after the spraying is completed, it is cured under ultraviolet light and 120°C for 5 minutes to obtain a current collector.

[0035] Example 7: S1: Take an alumina ultra-thin porous nanoplate with a nanopore size of 300 nm and a 100 μm thick metal copper foil, first wash them with deionized water for 10 min, then wash them with isopropanol for 10 min, and finally wash them with ethanol for 10 min; cut them into square chips with a side length of 5 mm; S2: Coating a solid lubricant in the ultra-thin porous nanoplate of aluminum oxide, placing it on top of the metal foil, and ultrasonically imprinting it using a Branson 2000X ultrasonic imprinting device with a frequency of 20 kHz to obtain an ultra-thin porous nanoplate of aluminum oxide / substrate with a copper metal rod of 300 nm in size; S3: immersing the alumina ultrathin porous nanoplate / substrate stack obtained in step S2 in a 1M NaOH solution for 2 h to obtain a metal substrate with nanowires exposed; S4: using nano laser cutting technology to cut away the nanowires on the metal substrate to obtain nanowires; S5: 16 parts of hydroxyethyl methacrylate, 100 parts of polypropylene and 1 part of benzoyl peroxide were mixed, heated to 210°C, and reacted for 3 hours to obtain an intermediate; 100 parts of the intermediate were added to 150 parts of N,N-dimethylformamide, stirred evenly, 2 parts of anhydrous sodium carbonate and 25 parts of bis(4-nitrophenyl) phosphate were added, heated to 185°C under a nitrogen atmosphere, reacted for 12 hours, and refluxed under reduced pressure to obtain modified polypropylene; The modified polypropylene is melt-extruded; the obtained melt is cast into a sheet by a cooling roller and a high-pressure air knife, and then longitudinally stretched and transversely stretched by a longitudinal stretching machine and a transverse stretching machine in sequence; the temperature of the cooling roller is 90°C, the gas temperature of the high-pressure air knife is 60°C, and the blowing speed is 150m / s; the stretching temperature of the longitudinal stretching is 150°C, the setting temperature is 150°C, preferably 150°C, and the stretching ratio is 7; the stretching temperature of the transverse stretching is 160°C, the setting temperature is 175°C, and the stretching ratio is 12; the temperature is kept at 120°C for 5 minutes, and a corona treatment is performed; the corona power is 80kW, and the line speed is 200m / min; a modified polypropylene film is obtained; S6: Evenly scrape a conductive glue with a thickness of 1 μm on the surface of the modified polypropylene film, and spray the nanowires. When spraying the nanowires, a nanowire dispersion is used, and the nanowire dispersion is 6 mg / ml nanowire ethanol dispersion; the spraying speed is 15 mm / s; the atomization pressure is 20 MPa; the nozzle diameter is 100 μm; after the spraying is completed, it is cured under ultraviolet light and 120°C for 5 minutes to obtain a current collector.

[0036] Comparative Example 1 (not using nanoimprinting technology, using conventional magnetron sputtering + water plating): Step 1: magnetron sputtering a 100nm copper layer on both sides of a 5μm polypropylene film; Step 2: water-plating a 1.5μm copper layer on the surface of the magnetron sputtered film to make a composite current collector.

[0037] Comparative Example 2 (the frequency of the ultrasonic embossing equipment was changed to 10 kHz, and the other method steps were consistent with Example 1): S1: Take an alumina ultra-thin porous nanoplate with a nanopore size of 130 nm and a 100 μm thick metal copper foil, first wash them with deionized water for 10 min, then wash them with isopropanol for 10 min, and finally wash them with ethanol for 10 min; cut them into square chips with a side length of 5 mm; S2: Coat a solid lubricant in the ultra-thin porous nanoplate of aluminum oxide, place it on top of the metal foil, and perform ultrasonic embossing using a Branson 2000X ultrasonic embossing device with a frequency of 10 kHz to obtain an ultra-thin porous nanoplate of aluminum oxide / substrate with copper metal rods of 130 nm in size; S3: immersing the alumina ultrathin porous nanoplate / substrate stack obtained in step S2 in a 1M NaOH solution for 2 h to obtain a metal substrate with nanowires exposed; S4: using nano laser cutting technology to cut away the nanowires on the metal substrate to obtain nanowires; S5: Evenly scrape a conductive glue with a thickness of 1 μm on the surface of the polypropylene film, and spray the nanowires. When spraying the nanowires, a nanowire dispersion is used, and the nanowire dispersion is a 6 mg / ml nanowire ethanol dispersion; the spraying speed is 15 mm / s; the atomization pressure is 20 MPa; the nozzle diameter is 100 μm; after the spraying is completed, it is cured under ultraviolet light and 120°C for 5 minutes to obtain a current collector.

[0038] Comparative Example 3 (the addition amount of hydroxyethyl methacrylate and bis(4-nitrophenyl)phosphate was changed, and the other method steps were consistent with Example 7): S1: Take an alumina ultra-thin porous nanoplate with a nanopore size of 300 nm and a 100 μm thick metal copper foil, first wash it with deionized water for 10 min, then wash it with isopropanol for 10 min, and finally wash it with ethanol for 10 min; cut it into a square chip with a side length of 5 mm; S2: Coating a solid lubricant in the ultra-thin porous nanoplate of aluminum oxide, placing it on top of the metal foil, and ultrasonically imprinting it using a Branson 2000X ultrasonic imprinting device with a frequency of 20 kHz to obtain an ultra-thin porous nanoplate of aluminum oxide / substrate with a copper metal rod of 300 nm in size; S3: immersing the alumina ultrathin porous nanoplate / substrate stack obtained in step S2 in a 1M NaOH solution for 2 h to obtain a metal substrate with nanowires exposed; S4: using nano laser cutting technology to cut away the nanowires on the metal substrate to obtain nanowires; S5: 25 parts of hydroxyethyl methacrylate, 100 parts of polypropylene and 1 part of benzoyl peroxide were mixed, heated to 210°C, and reacted for 3 hours to obtain an intermediate; 100 parts of the intermediate were added to 150 parts of N,N-dimethylformamide, stirred evenly, 2 parts of anhydrous sodium carbonate and 35 parts of bis(4-nitrophenyl)phosphate were added, heated to 185°C under a nitrogen atmosphere, reacted for 12 hours, and refluxed under reduced pressure to obtain modified polypropylene; The modified polypropylene is melt-extruded; the obtained melt is cast into a sheet by a cooling roller and a high-pressure air knife, and then longitudinally stretched and transversely stretched by a longitudinal stretching machine and a transverse stretching machine in sequence; the temperature of the cooling roller is 90°C, the gas temperature of the high-pressure air knife is 60°C, and the blowing speed is 150m / s; the stretching temperature of the longitudinal stretching is 150°C, the setting temperature is 150°C, preferably 150°C, and the stretching ratio is 7; the stretching temperature of the transverse stretching is 160°C, the setting temperature is 175°C, and the stretching ratio is 12; the temperature is kept at 120°C for 5 minutes, and a corona treatment is performed; the corona power is 80kW, and the line speed is 200m / min; a modified polypropylene film is obtained; S6: Evenly scrape a conductive glue with a thickness of 1 μm on the surface of the modified polypropylene film, and spray the nanowires. When spraying the nanowires, a nanowire dispersion is used, and the nanowire dispersion is 6 mg / ml nanowire ethanol dispersion; the spraying speed is 15 mm / s; the atomization pressure is 20 MPa; the nozzle diameter is 100 μm; after the spraying is completed, it is cured under ultraviolet light and 120°C for 5 minutes to obtain a current collector.

[0039] Comparative Example 4 (polypropylene with a melt index of 3 g / 10 min was selected, and the remaining steps were consistent with those of Example 7): S1: an ultra-thin porous nanoplate of aluminum oxide with a nanopore size of 300 nm and a 100 μm thick copper foil were first washed with deionized water for 10 min, then with isopropanol for 10 min, and finally with ethanol for 10 min; and cut into square chips with a side length of 5 mm; S2: Coating a solid lubricant in the ultra-thin porous nanoplate of aluminum oxide, placing it on top of the metal foil, and ultrasonically imprinting it using a Branson 2000X ultrasonic imprinting device with a frequency of 20 kHz to obtain an ultra-thin porous nanoplate of aluminum oxide / substrate with a copper metal rod of 300 nm in size; S3: immersing the alumina ultrathin porous nanoplate / substrate stack obtained in step S2 in a 1M NaOH solution for 2 h to obtain a metal substrate with nanowires exposed; S4: using nano laser cutting technology to cut away the nanowires on the metal substrate to obtain nanowires; S5: 16 parts of hydroxyethyl methacrylate, 100 parts of polypropylene and 1 part of benzoyl peroxide were mixed, heated to 210°C, and reacted for 3 hours to obtain an intermediate; 100 parts of the intermediate were added to 150 parts of N,N-dimethylformamide, stirred evenly, 2 parts of anhydrous sodium carbonate and 25 parts of bis(4-nitrophenyl) phosphate were added, heated to 185°C under a nitrogen atmosphere, reacted for 12 hours, and refluxed under reduced pressure to obtain modified polypropylene; The modified polypropylene is melt-extruded; the obtained melt is cast into a sheet by a cooling roller and a high-pressure air knife, and then longitudinally stretched and transversely stretched by a longitudinal stretching machine and a transverse stretching machine in sequence; the temperature of the cooling roller is 90°C, the gas temperature of the high-pressure air knife is 60°C, and the blowing speed is 150m / s; the stretching temperature of the longitudinal stretching is 150°C, the setting temperature is 150°C, preferably 150°C, and the stretching ratio is 7; the stretching temperature of the transverse stretching is 160°C, the setting temperature is 175°C, and the stretching ratio is 12; the temperature is kept at 120°C for 5 minutes, and a corona treatment is performed; the corona power is 80kW, and the line speed is 200m / min; a modified polypropylene film is obtained; S6: Evenly scrape a conductive glue with a thickness of 1 μm on the surface of the modified polypropylene film, and spray the nanowires. When spraying the nanowires, a nanowire dispersion is used, and the nanowire dispersion is 6 mg / ml nanowire ethanol dispersion; the spraying speed is 15 mm / s; the atomization pressure is 20 MPa; the nozzle diameter is 100 μm; after the spraying is completed, it is cured under ultraviolet light and 120°C for 5 minutes to obtain a current collector.

[0040] In the above embodiments, the test methods used are conventional methods unless otherwise specified; the raw materials used are commercially available unless otherwise specified, and the sources of the raw materials are as follows: ultra-thin porous alumina nanoplates (commercially available anodized aluminum oxide AAO templates); solid lubricants (carbon 60); conductive adhesives (LOCTITE ABLESTIK ICP 3850); hydroxyethyl methacrylate (S24381, Shanghai Yuanye); benzoyl peroxide (CAS: 94-36-0); N,N-dimethylformamide (CAS: 68-12-2); anhydrous sodium carbonate (S24152, Shanghai Yuanye); bis(4-nitrophenyl) phosphate (S30868, Shanghai Yuanye); ethanol (CAS: 64-17-5).

[0041] Experiment: The current collectors prepared in Examples 1 to 7 and Comparative Examples 1 to 4 were tested for coating peeling force with reference to ASTM B533: Standard Test Method for Peel Strength of Metal-Plated Plastics of the American Society for Testing and Materials; specifically, a universal testing machine was used to cut a sample with a width of (25.0±0.25) mm from the composite current collector material, and the prepared sample was mounted on the fixture of the testing equipment. The peeling angle was 90°, and the test speed was 100 mm / min. The peeling force was divided by the width of the sample to obtain the peeling force per unit width (N / m); the specific data are shown in the table below;

[0042] Conclusion: The current collector prepared by ultrasonic embossing nanowires and spraying them on the surface of the polymer film has good bonding strength between layers, which can significantly improve the safety performance of the battery and increase the cycle life of the battery. From Example 7, when the polymer film is modified polypropylene film, the peeling force is further enhanced due to the improvement of mechanical properties and crystallinity; from Comparative Example 3, it can be seen that the amount of hydroxyethyl methacrylate grafted on the side chain needs to be controlled, otherwise it will lead to a decrease in performance; from Comparative Example 4, the choice of polypropylene also has an important influence; In summary, the modified polypropylene film prepared by the present invention has good surface adhesion, good storage stability, good mechanical properties, and the prepared current collector has good peeling strength.

[0043] Finally, it should be noted that the above is only a preferred embodiment of the present invention, but the protection scope of this application is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the spirit and principle of the present invention and within the technical scope disclosed in this application should be included in the protection scope of this application; in the absence of conflict, the embodiments of this application and the features in the embodiments can be combined with each other. Therefore, the protection scope of this application shall be based on the protection scope of the claims.

Claims

1. A method for preparing a current collector with high binding force, characterized in that: The method comprises the following steps: S1: taking an ultra-thin porous alumina nanoplate and a metal foil, washing them, and cutting them into square chips with a side length of 1 to 5 mm; S2: evenly coating the solid lubricant in the ultra-thin porous nanoplate of aluminum oxide, placing it on the metal foil, and ultrasonically imprinting it with an ultrasonic embossing device at a frequency of 15-25kHz to obtain an ultra-thin porous nanoplate of aluminum oxide / substrate with a metal rod; S3: immersing the alumina ultrathin porous nanoplate / substrate stack obtained in step S2 in a 1M NaOH solution for 2 h to obtain a metal substrate with nanowires exposed; S4: using nano laser cutting technology to cut away the nanowires on the metal substrate to obtain nanowires; S5: Evenly apply conductive glue on the surface of the polymer film, control the surface temperature to 70°C, and spray nanowires; A nanowire dispersion is used when spraying the nanowires, wherein the nanowire dispersion is a 2-10 mg / ml nanowire ethanol dispersion; Injection speed 10~20mm / s; Atomization pressure is 5~30MPa; nozzle diameter is 50~200μm; After the spraying is completed, the current collector is cured for 5 minutes under the conditions of UV intensity of 50~200mW / cm² and temperature of 110~120℃.

2. The method for preparing a current collector with high binding force according to claim 1, characterized in that: The nanopore size of the alumina ultra-thin porous nanoplate is 100-300 nm.

3. The method for preparing a current collector with high binding force according to claim 1, characterized in that: The metal foil is a copper metal foil with a thickness of 100 μm.

4. The method for preparing a current collector with high binding force according to claim 1, characterized in that: The solid lubricant is carbon 60, and the coating thickness is 80-120 nm.

5. The method for preparing a current collector with high binding force according to claim 1, characterized in that: The polymer film is a BOPP polypropylene film with a thickness of 4 to 10 μm.

6. The method for preparing a current collector with high binding force according to claim 1, characterized in that: The thickness of the conductive adhesive is 0.8-1 μm.

7. The method for preparing a current collector with high binding force according to claim 5, characterized in that: The polymer film is a modified polypropylene film, and the specific preparation method is The following steps are involved: S1: Mix hydroxyethyl methacrylate, polypropylene and benzoyl peroxide, heat to 200-210°C, react for 2-3 hours to obtain an intermediate; take the intermediate, add it to N,N-dimethylformamide, stir evenly, add anhydrous sodium carbonate and bis(4-nitrophenyl) phosphate, heat to 180-190°C under nitrogen atmosphere, react for 10-12 hours, and reflux under reduced pressure to obtain modified polypropylene; S2: Melting and extruding the modified polypropylene; The obtained melt casting sheet is formed, and longitudinal stretching and transverse stretching, heat preservation and corona treatment are performed in sequence to obtain a modified polypropylene film.

8. The method for preparing a current collector with high binding force according to claim 7, characterized in that: The intermediate comprises the following raw materials, calculated by weight: 15-20 parts of hydroxyethyl methacrylate, 100 parts of polypropylene, and 1-2 parts of benzoyl peroxide; The modified polypropylene comprises the following raw materials, calculated by mass: 100 parts of an intermediate, 150-180 parts of N,N-dimethylformamide, 1-2 parts of anhydrous sodium carbonate, and 25-30 parts of bis(4-nitrophenyl)phosphate.

9. A current collector prepared according to the method for preparing a current collector with high binding force according to any one of claims 1 to 8.

10. A battery, characterized in that: Comprising the current collector as claimed in claim 9.

Citation Information

Patent Citations

  • Ceramic surface ultrasonic impressing metallization device and method

    CN108746912A

  • A flexible porous current collector and a preparation method thereof

    CN109216703A

  • Composite copper-based current collector and preparation method thereof, battery electrode and lithium ion battery

    CN115172761A

  • Method for embossing microstructures in flat thermoplastic plastic semi-finished products, such as plates or films, involves melting plastic surface area by coupling of ultrasonic energy

    DE102008048298A1

  • Preparation method for composite current collector

    WO2023142320A1

Cited By

  • Multi-metal three-dimensional array current collector and application thereof in sodium battery

    CN122338081A