Perovskite solar cell for preparing high-quality optical active layer based on assistance of additive
By introducing fluorine-containing additives in the preparation process of perovskite solar cells, the morphology of lead iodide films is solved, and the problem of low quality of perovskite films in traditional methods is achieved, and high efficiency and stable perovskite solar is achieved. Battery performance.
Patent Information
- Application Number
- CN202310556305.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-05-17
AI Technical Summary
The perovskite film prepared by the traditional two-step spin coating method is too smooth, resulting in difficulty in penetration of monovalent halide solution, resulting in PbI2 residue, low crystallinity of low-quality perovskite film, irregular surface morphology, poor repeatability, and grain boundary Or the interface defect state is high, affecting the photoelectric performance and stability of perovskite solar cells.
Introducing fluorine-containing additives, such as hexafluorobenzene, changes the morphology of lead iodide films, makes them rough and porous, promotes the penetration and reaction of organic solutions, and prepares high-quality perovskite films through two-step spin coating or scraping coating.
It improves the photoelectric efficiency and environmental stability of perovskite solar cells, increases grain size, improves surface morphology, reduces defect states, and improves device performance and storage stability.
Smart Images

Figure CN119012718A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar cells, and in particular to a perovskite solar cell based on additive-assisted preparation of a high-quality photoactive layer. Background Art
[0002] Perovskite solar cells have developed rapidly in recent years due to their excellent photoelectric performance, and their maximum efficiency has exceeded 26% by 2023. Perovskite materials have gradually become the most promising choice for solar energy systems due to their superior light absorption coefficient, low cost, easy manufacturing and weak light effect. The morphology and quality of perovskite films seriously affect the photoelectric performance of the device, and the preparation of excellent perovskite films has become an important research hotspot. At present, the popular methods for obtaining perovskite films include vapor deposition, spraying, spin coating (including one or two steps), etc. The two-step spin coating method has more opportunities to affect the crystallization of the perovskite layer and has become a typical and widely used laboratory method.
[0003] Usually, lead iodide (PbI 2 ) and a mixed solution of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) to prepare PbI 2 Then, a monovalent halide solution such as formamidine iodide (FAI) is spin-coated onto the PbI 2 However, the conventional two-step spin coating method for preparing PbI 2 The film is too smooth, which is not conducive to the penetration and reaction of monovalent halide solution, resulting in the PbI 2 A large amount of residues and disappointing microstructure of perovskite film. Low-quality perovskite film has low crystallinity, irregular surface morphology, poor reproducibility, and high defect states at grain boundaries or interfaces, which are the main pathways for ion migration. Ion movement causes hysteresis and phase separation in the photovoltage-current curve of the perovskite active layer. Low-quality perovskite film and large amount of PbI 2 The residue also accelerates the corrosion of perovskite film by water and oxygen, reducing the performance and stability of the device. Summary of the invention
[0004] The purpose of the present invention is to provide a perovskite solar cell with a high-quality photoactive layer prepared with the aid of additives. The present invention improves the film quality of the perovskite layer by introducing fluorine-containing additives, thereby improving the photoelectric efficiency, environmental stability and other properties of the perovskite solar cell.
[0005] The present invention is achieved through the following technical solutions:
[0006] A perovskite solar cell with a high-quality photoactive layer prepared with the aid of additives, which consists of a substrate, an electron transport layer, an organic-inorganic perovskite structure photoactive layer, a hole transport layer and a back electrode layer from bottom to top. The organic-inorganic perovskite structure photoactive layer is prepared by preparing a lead iodide film with the aid of doping with a fluorine-containing additive, and then reacting on the lead iodide film to prepare a perovskite film. The doping volume fraction of the fluorine-containing additive is 1% to 25%.
[0007] Preferably, the organic-inorganic perovskite structure photoactive layer is prepared by a two-step spin coating method or a two-step scraping method, that is, a lead iodide film is first prepared and then a perovskite film is prepared by chemical reaction. The fluorine-containing additive is used to change the morphology of the lead iodide film in the first step, and does not remain in the film after the lead iodide film is prepared.
[0008] Preferably, the fluorine-containing additive is a fluorine-containing aromatic hydrocarbon or a fluorine-containing alkane having a boiling point below 100°C.
[0009] More preferably, the fluorinated aromatic hydrocarbon is hexafluorobenzene or octafluoronaphthalene, and the fluorinated alkane is perfluoropentane, perfluorohexane or perfluoroheptane.
[0010] The present invention also protects the above-mentioned method for preparing a perovskite solar cell with a high-quality photoactive layer assisted by an additive, comprising the following steps:
[0011] S1, cleaning the substrate;
[0012] S2, preparing an electron transport layer on a transparent substrate by a solution method;
[0013] S3. Uniformly coating a fluorine-containing lead iodide precursor solution on the electron transport layer obtained in step S2 to obtain a lead iodide film, wherein the fluorine-containing lead iodide precursor solution is prepared according to the following steps: adding a fluorine-containing additive to a lead iodide precursor solution having a molar concentration of 1.2 to 1.5 mmol / mL to obtain a fluorine-containing lead iodide precursor solution having a fluorine-containing additive volume fraction of 1% to 25%;
[0014] S4, uniformly coating a monovalent halide solution with a molar concentration of 1.2 to 1.5 mmol / mL on the lead iodide film obtained in step S3 to obtain a perovskite film, i.e., an organic-inorganic perovskite structure photoactive layer;
[0015] S5. A hole transport layer and a back electrode layer are sequentially prepared on the perovskite film obtained in step S4 to finally obtain the perovskite solar cell.
[0016] Preferably, the coating method in step S3 or S4 is a blade coating method or a spin coating method. The organic-inorganic perovskite structure photoactive layer is prepared by a two-step spin coating method or a two-step blade coating method.
[0017] The electron transport layer described in step S2 is a tin dioxide electron transport layer, which is prepared by the following steps: SnO 2 The precursor solution is evenly dropped on the transparent substrate, and the spin coating is carried out at a speed of 3500-4500 r / min for 15-25 s. After the spin coating is completed, the wafer is removed from the spin coater and annealed on a constant temperature heating table at 140°C-160°C for 25-35 min to obtain SnO 2 ETL film (ie tin dioxide electron transport layer).
[0018] Further preferably, the specific steps of steps S3 and S4 are:
[0019] S3, on the tin dioxide electron transport layer obtained in step S2, spin-coating a fluorine-containing lead iodide precursor solution at a rotation speed of 1500-2000 rpm for 20-40 seconds, and after the spin coating is completed, thermal annealing is performed at less than 80° C. for 10-80 seconds to obtain a lead iodide film;
[0020] S4. Spin coating a monovalent halide solution on the lead iodide film obtained in step S3 at a rotation speed of 1500-2000 rpm for 20-40 seconds. After the spin coating is completed, annealing is performed at 140° C.-160° C. for 10-20 minutes in an atmosphere with a humidity of 30%-45% to obtain a perovskite film.
[0021] Further preferably, the specific steps of steps S3 and S4 are:
[0022] S3, on the tin dioxide electron transport layer obtained in step S2, scraping to obtain a lead iodide thin film at a scraping speed of 80 to 120 mm / min, a transparent substrate heating temperature of less than 80° C., and a gap of 90 to 110 μm between the scraper and the substrate surface;
[0023] S4. On the lead iodide film obtained in step S3, a monovalent halide solution is scraped at a speed of 80 to 120 mm / min. The substrate is not heated. The gap between the scraper and the substrate surface is 90 to 110 μm. The wet film obtained by scraping is annealed at 140° C. to 160° C. for 10 to 20 min in an atmospheric environment with a humidity of 30% to 45% to obtain a perovskite film.
[0024] Preferably, the volume fraction of the fluorine-containing additive is 5% to 20%, and more preferably, the volume fraction of the fluorine-containing additive is 10% to 20%.
[0025] Preferably, the monovalent halide in step S4 has a general formula of AX, where A is a +1 valent cation and includes FA + 、MA + , Cs + , Rb + , X is a halogen ion, including Cl - Br- 、I-.
[0026] Preferably, the substrate described in step S1 is fluorine-doped tin oxide transparent conductive glass (FTO) or indium tin oxide transparent conductive film glass (ITO) or indium tin oxide transparent polyethylene naphthalate film (PEN-ITO) or indium tin oxide transparent polyethylene terephthalate film (PET-ITO).
[0027] Preferably, the thickness of the electron transport layer is 20-40 nm, the thickness of the organic-inorganic perovskite structure photoactive layer is 580-620 nm, the thickness of the hole transport layer is 100-200 nm, and the thickness of the back electrode layer is 50-100 nm. The hole transport layer is a 2,2',7,7'-tetra-N,N-di(4-methoxyphenyl)amino-9,9'-spirobifluorene (Spiro-OMeTAD) layer. The back electrode layer is a metal electrode layer, and the metal electrode is a gold electrode.
[0028] The preparation steps of the hole transport layer are as follows: after spreading the hole transport layer precursor solution on a substrate provided with an organic-inorganic perovskite structure photoactive layer, spin coating at a spin coating speed of 3500-4500 r / min for 20-40s to obtain the hole transport layer.
[0029] The back electrode is prepared by vacuum coating.
[0030] Compared with the prior art, the present invention has the following beneficial effects: the present invention introduces a green and environmentally friendly additive hexafluorobenzene (HFB) into the first step lead iodide precursor solution of the perovskite film prepared by the two-step spin coating or scraping coating method, thereby obtaining a lead iodide film morphology different from the smooth first step of the traditional two-step method. The lead iodide film morphology introduced with hexafluorobenzene becomes rough and porous, which is beneficial to the second step organic solution penetration intercalation reaction, thereby obtaining a high-quality perovskite film with increased grain size, improved surface morphology, and reduced defect state density, thereby improving the photoelectric efficiency, environmental stability and other performances of the perovskite solar cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a schematic diagram of the structure of the perovskite solar cell prepared by the present invention;
[0032] Figure 2 The JV curve of the perovskite solar cell prepared in Example 1 of the present invention;
[0033] Figure 3 This is a JV curve diagram of the perovskite solar cell prepared in Example 2 of the present invention.
[0034] Figure 4This is a storage stability test graph of the perovskite solar cells prepared in Example 1 of the present invention and Comparative Example 1 under the protocol test ID: ISOS-D-lshelf that meets the International Organic Photovoltaic Stability Summit. DETAILED DESCRIPTION
[0035] The present invention is further described in detail below with reference to the examples. These examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples where specific conditions are not specified are generally based on conventional conditions in the art or conditions recommended by the manufacturer; the raw materials, reagents, etc. used, unless otherwise specified, are considered to be raw materials and reagents that can be obtained through commercial channels such as conventional markets.
[0036] like Figure 1 As shown, a perovskite solar cell based on additive-assisted preparation of a high-quality photoactive layer is composed of a substrate, an electron transport layer (tin dioxide), an organic-inorganic perovskite structure photoactive layer (Perovskite), a hole transport layer and a back electrode layer from bottom to top. In the following embodiments, the substrate is preferably fluorine-doped tin oxide transparent conductive glass (FTO), the electron transport layer is tin dioxide (SnO 2 )Electron transport layer (SnO 2 ETL layer), the hole transport layer is 2,2',7,7'-tetrakis N,N-di(4-methoxyphenyl)amino-9,9'-spirobifluorene (Spiro-OMeTAD) layer (HTL layer), the back electrode layer is a metal electrode layer, and the metal electrode is a gold electrode.
[0037] In the following Examples 1 and 2, the precursor solution is prepared by the following steps:
[0038] SnO 2 ETL layer precursor solution configuration: 15wt% SnO commercially available from Alfa Asear was used. 2 The nanocrystalline hydrocolloid dispersion (particle size of 3-5 nm) was diluted to 3.75 wt% (1:3) by adding deionized water and filtered to obtain SnO 2 The precursor solution is reserved;
[0039] PbI 2 Precursor solution preparation: prepare a lead iodide precursor solution with a molar concentration of 1.3 mmol / mL, heat and stir on a constant temperature heating table until it is completely dissolved, add hexafluorobenzene as a fluorine-containing additive, keep it in a heated state, and obtain a fluorine-containing lead iodide precursor solution with a fluorine-containing additive volume ratio of 15%;
[0040] Preparation of FAMA precursor solution: Based on the preparation of 1.5 mL of precursor solution, 90 mg of FAI, 9 mg of MACl and 9 mg of MABr were accurately weighed using an analytical balance in a glove box and added to a clean brown empty bottle. Then, 1.5 mL of IPA solvent was added and stirred for 30 min until the solute was completely dissolved. Filtered with a polytetrafluoroethylene filter (0.22 μm) before spin coating;
[0041] Preparation of Spiro-OMeTAD HTL layer precursor solution: Based on the preparation of 1 mL of Spiro solution, accurately weigh 72.3 mg of Spiro-OMeTAD powder using an analytical balance in a nitrogen glove box, and add 1 mL of chlorobenzene, 28.8 μL of TBP, 17.5 μL of 520 mg / mL lithium salt acetonitrile solution, and 20 μL of 300 mg / mL Co salt (FK209) acetonitrile solution in sequence. Mix in a brown light-proof bottle, and filter with a polytetrafluoroethylene filter (0.22 μm) after complete dissolution for later use.
[0042] Example 1
[0043] A method for preparing a perovskite solar cell with a high-quality photoactive layer assisted by an additive, wherein the photoactive layer is prepared by a two-step spin coating method, specifically comprising the following steps:
[0044] S1. Rigid substrate cleaning: Place the FTO substrate on a customized cleaning rack, and clean the FTO conductive glass with FTO cleaning solution (FTO cleaning agent: deionized water = 1:20), deionized water (DI), anhydrous ethanol, and isopropanol in turn to remove adhesives and residual cleaning agents on the substrate surface. Each round of cleaning requires the glass to be ultrasonically cleaned in an ultrasonic cleaner for 15 minutes. After the last round of isopropanol cleaning, use a nitrogen blow gun to blow dry the isopropanol on the surface of the FTO conductive glass, and then place the substrate in a clean culture dish for later use;
[0045] S2、SnO 2 Preparation of ETL layer: The FTO conductive glass cleaned in step S1 is fed into the UV-O 3 UV treatment in the machine for 20 minutes. After the slice cools to room temperature, place it on the spin coater suction cup, blow air on the surface with an ear-cleaning bulb, and then use a 100μL pipette to draw 100μL of the prepared SnO 2 The precursor solution was evenly dropped on the substrate and the spin coating was carried out at a speed of 4000 r / min for 20 s. After the spin coating was completed, the wafer was removed from the spin coater and annealed at 150 °C for 30 min on a constant temperature heating table to obtain a SnO with a thickness of 30 nm. 2 ETL film.
[0046] S3. Preparation of lead iodide film: After spin coating SnO2 The fluorine-containing lead iodide precursor solution was spin-coated on the ETL film substrate at a rotation speed of 1700 rpm for 30 seconds, and after the spin coating was completed, it was thermally annealed on a 70°C constant temperature heating table for 10 seconds to obtain a lead iodide film with a thickness of 580 nm;
[0047] S4, FAMACs perovskite film preparation: spin-coated PbI 2 After the substrate of the film is placed on the spin coater suction cup, the surface is blown with an ear bulb, and dynamic spin coating is used. When the substrate is rotated at a constant speed of 1700r / min, 70mL of FAMA precursor solution is spin-coated for 30s. After the spin coating is completed, the substrate is immediately transferred from the glove to an atmosphere at room temperature (25±2)℃ and a humidity of 40%, and annealed at 150℃ for 15min to obtain a FAMACs perovskite film with a thickness of 600nm;
[0048] S5. Preparation of HTL layer: Place the substrate cooled to room temperature on the chuck of the spin coater, blow air on the surface with an ear bulb, and then use a 100μL pipette to draw 50μL of filtered Spiro-OMeTAD precursor solution and evenly drop it on the substrate. After the Spiro solution spreads on the entire substrate, spin coat at a speed of 4000r / min for 30s to obtain a HTL layer with a thickness of 150nm.
[0049] S6. Transfer the substrate with the HTL layer spin-coated from the glove box to a room with a temperature of (25±2)℃ and a humidity of 40%. Use a surgical blade to scrape a 3-4mm gap along the edge of the film in parallel. Transfer the substrate to the vacuum coating evaporation chamber of the glove box. Use the first 1nm Evaporation rate, 1~5nm use Evaporation rate, 5~10nm use Evaporation rate, 10~80nm use The evaporation rate was 2.004 % to obtain a 80 nm thick gold electrode. After the evaporation was completed, the device was transferred to a dry air box with a humidity of 5% to 10% to avoid light oxidation for 12 hours. The final device efficiency was 23.01%. The JV curve is shown in Figure 2 shown.
[0050] Example 2
[0051] A method for preparing a perovskite solar cell with a high-quality photoactive layer assisted by an additive, wherein the photoactive layer is coated by a two-step scraping method, specifically comprising the following steps:
[0052] S1. Rigid substrate cleaning: Place the FTO substrate on a customized cleaning rack, and clean the FTO conductive glass with FTO cleaning solution (FTO cleaning agent: deionized water = 1:20), deionized water (DI), anhydrous ethanol, and isopropanol in turn to remove adhesives and residual cleaning agents on the substrate surface. Each round of cleaning requires the glass to be ultrasonically cleaned in an ultrasonic cleaner for 15 minutes. After the last round of isopropanol cleaning, use a nitrogen blow gun to blow dry the isopropanol on the surface of the FTO conductive glass, and then place the substrate in a clean culture dish for later use;
[0053] S2、SnO 2 Preparation of ETL layer: The FTO conductive glass cleaned in step S1 is fed into the UV-O 3 UV treatment in the machine for 20 minutes. After the substrate cools to room temperature, place it on the spin coater suction cup, blow air on the surface with an ear-cleaning bulb, and then use a 100μL pipette to draw 100μL of the prepared SnO 2 The precursor solution was evenly dropped on the substrate and the spin coating was carried out at a speed of 4000 r / min for 20 s. After the spin coating was completed, the wafer was removed from the spin coater and annealed at 150 °C for 30 min on a constant temperature heating table to obtain a SnO with a thickness of 30 nm. 2 ETL film.
[0054] S3. Preparation of lead iodide film: After spin coating SnO 2 On the ETL film substrate, the scraper was coated at a speed of 100 mm / min, the substrate was heated at 70°C, the gap between the scraper and the substrate surface was 100 μm, and the fluorine-containing lead iodide precursor solution was dripped into the gap, and the lead iodide film with a thickness of 580 nm was obtained by scraping;
[0055] S4, preparation of FAMACs perovskite film: on the lead iodide film obtained in step S3, the coating speed is 100 mm / min, the substrate is not heated, the gap between the scraper and the substrate surface is 100 μm, and the wet film obtained by scraping is annealed at 150° C. for 15 min in an atmospheric environment with a humidity of 30% to 45%, to obtain a perovskite film with a thickness of 600 nm;
[0056] S5. Preparation of HTL layer: Place the substrate cooled to room temperature on the chuck of the spin coater, blow air on the surface with an ear bulb, and then use a 100μL pipette to draw 50μL of filtered Spiro-OMeTAD precursor solution and evenly drop it on the substrate. After the Spiro solution spreads on the entire substrate, spin coat at a speed of 4000r / min for 30s to obtain a HTL layer with a thickness of 150nm.
[0057] S6. Transfer the substrate with the HTL layer spin-coated from the glove box to a room with a temperature of (25±2)℃ and a humidity of 40%. Use a surgical blade to scrape a 3-4mm gap along the edge of the wafer in parallel. Transfer the wafer to the vacuum coating evaporation chamber of the glove box. Use the first 1nm Evaporation rate, 1~5nm use Evaporation rate, 5~10nm use Evaporation rate, 10~80nm use The evaporation rate was 2.5 % to obtain a 80 nm thick gold electrode. After the evaporation was completed, the device was transferred to a dry air box with a humidity of 5% to 10% to avoid light oxidation for 12 hours. The final device efficiency was 21.23%. The JV curve is shown in Figure 3 shown.
[0058] Comparative Example 1
[0059] In this comparative example, a perovskite solar cell was prepared according to the steps of Example 1. Compared with Example 1, the only difference was that no fluorine-containing additive was added to the lead iodide precursor solution in step S3, and the efficiency of the device finally prepared was 20.95%.
[0060] The stability comparison test of Example 1 and Comparative Example 1 is as follows Figure 4 As shown, after adding the fluorine-containing additive in Example 1, the storage stability of the perovskite solar cell is significantly improved.
[0061] Comparative Example 2
[0062] In this comparative example, a perovskite solar cell was prepared according to the steps of Example 2. Compared with Example 2, the only difference was that no fluorine-containing additive was added to the lead iodide precursor solution in step S3, and the efficiency of the device finally prepared was 19.16%.
[0063] Example 3
[0064] This embodiment prepares a perovskite solar cell according to the steps of Example 1. Compared with Example 1, the only difference is that the fluorine-containing additive added to the lead iodide precursor solution in step S3 is replaced by octafluoronaphthalene instead of hexafluorobenzene. The efficiency of the device finally obtained is 22.34%.
[0065] Example 4
[0066] This embodiment prepares a perovskite solar cell according to the steps of Example 2. Compared with Example 2, the only difference is that the fluorine-containing additive added to the lead iodide precursor solution in step S3 is replaced by octafluoronaphthalene instead of hexafluorobenzene. The efficiency of the device finally prepared is 20.27%.
[0067] Example 5
[0068] This embodiment prepares a perovskite solar cell according to the steps of Example 1. Compared with Example 1, the only difference is that the fluorine-containing additive added to the lead iodide precursor solution in step S3 is replaced by perfluoropentane instead of hexafluorobenzene. The efficiency of the device finally obtained is 22.56%.
[0069] Example 6
[0070] This embodiment prepares a perovskite solar cell according to the steps of Example 2. Compared with Example 2, the only difference is that the fluorine-containing additive added to the lead iodide precursor solution in step S3 is replaced by perfluoropentane instead of hexafluorobenzene. The efficiency of the device finally obtained is 20.65%.
[0071] Example 7
[0072] This embodiment prepares a perovskite solar cell according to the steps of Example 1. Compared with Example 1, the only difference is that the fluorine-containing additive added to the lead iodide precursor solution in step S3 is replaced by perfluorohexane instead of hexafluorobenzene. The efficiency of the device finally obtained is 21.87%.
[0073] Example 8
[0074] This embodiment prepares a perovskite solar cell according to the steps of Example 2. Compared with Example 2, the only difference is that the fluorine-containing additive added to the lead iodide precursor solution in step S3 is replaced by perfluorohexane instead of hexafluorobenzene. The efficiency of the final device is 19.95%.
[0075] Example 9
[0076] This embodiment prepares a perovskite solar cell according to the steps of Example 1. Compared with Example 1, the only difference is that the fluorine-containing additive added to the lead iodide precursor solution in step S3 is replaced by perfluoroheptane instead of hexafluorobenzene. The efficiency of the device finally obtained is 21.56%.
[0077] Example 10
[0078] This embodiment prepares a perovskite solar cell according to the steps of Example 2, and the only difference compared with Example 2 is that the fluorine-containing additive added to the lead iodide precursor solution in step S3 is replaced by perfluoroheptane instead of hexafluorobenzene, and the efficiency of the final device is 19.67%.
[0079] The comparison of device efficiencies obtained by using different fluorine-containing additives in Examples 1-10 and Comparative Examples 1-2 is shown in Table 1.
[0080] Table 1
[0081]
[0082]
[0083] Embodiment 11
[0084] Same as Example 1, except that:
[0085] S2, spin coating at a speed of 3500r / min for 25s. After the spin coating is completed, the wafer is removed from the spin coater and annealed on a constant temperature heating table at 140℃ for 35min to obtain a SnO with a thickness of 20nm. 2 ETL film (ie tin dioxide electron transport layer).
[0086] S3. Spin coating a fluorine-containing lead iodide precursor solution on the electron transport layer obtained in step S2 at a rotation speed of 1500 rpm for 40 seconds, and thermally annealing at 70° C. for 10 seconds after spin coating to obtain a lead iodide film with a thickness of 570 nm. The fluorine-containing lead iodide precursor solution is prepared by the following steps: preparing a lead iodide precursor solution with a molar concentration of 1.2 mmol / mL, heating and stirring on a constant temperature heating table until completely dissolved, adding hexafluorobenzene as a fluorine-containing additive, and keeping it in a heated state to obtain a fluorine-containing lead iodide precursor solution with a volume fraction of 10% of the fluorine-containing additive;
[0087] S4, on the lead iodide film obtained in step S3, a monovalent halide solution is spin-coated at a rotation speed of 1500 rpm for 40 seconds, and after the spin coating is completed, annealing is performed at 140° C. for 20 minutes in an atmosphere with a humidity of 30% to 45%, to obtain a perovskite film with a thickness of 590 nm;
[0088] S5, spin coating at a spin coating speed of 3500 r / min for 40 s to obtain a hole transport layer with a thickness of 100 nm;
[0089] S6. Transfer the substrate with the HTL layer spin-coated from the glove box to a room with a temperature of (25±2)℃ and a humidity of 40%. Use a surgical blade to scrape a 3-4mm gap along the edge of the wafer in parallel. Transfer the wafer to the vacuum coating evaporation chamber of the glove box. Use the first 1nm Evaporation rate, 1~5nm use Evaporation rate, 5~10nm use Evaporation rate, 10~50nm use The evaporation rate was 50 nm to obtain a gold electrode with a thickness of 50 nm.
[0090] Example 12
[0091] Same as Example 1, except that:
[0092] S2, spin coating at a speed of 4500r / min for 15s. After the spin coating is completed, the wafer is removed from the spin coater and annealed on a constant temperature heating table at 160℃ for 25min to obtain a SnO with a thickness of 40nm. 2ETL film (ie tin dioxide electron transport layer).
[0093] S3. Spin coating a fluorine-containing lead iodide precursor solution on the electron transport layer obtained in step S2 at a rotation speed of 2000 rpm for 20 seconds, and thermally annealing at 50° C. for 80 seconds after the spin coating is completed to obtain a lead iodide film with a thickness of 590 nm. The fluorine-containing lead iodide precursor solution is prepared by the following steps: preparing a lead iodide precursor solution with a molar concentration of 1.5 mmol / mL, heating and stirring on a constant temperature heating table until it is completely dissolved, adding hexafluorobenzene as a fluorine-containing additive, and keeping it in a heated state to obtain a fluorine-containing lead iodide precursor solution with a volume fraction of 20% of the fluorine-containing additive;
[0094] S4, on the lead iodide film obtained in step S3, a monovalent halide solution is spin-coated at a rotation speed of 2000 rpm for 20 seconds, and after the spin coating is completed, annealing is performed at 160° C. for 10 minutes in an atmosphere with a humidity of 30% to 45%, to obtain a perovskite film with a thickness of 610 nm;
[0095] S5, spin coating at a spin coating speed of 4500 r / min for 20 s to obtain a hole transport layer with a thickness of 200 nm;
[0096] S6. Transfer the substrate with the HTL layer spin-coated from the glove box to a room with a temperature of (25±2)℃ and a humidity of 40%. Use a surgical blade to scrape a 3-4mm gap along the edge of the wafer in parallel. Transfer the wafer to the vacuum coating evaporation chamber of the glove box. Use the first 1nm Evaporation rate, 1~5nm use Evaporation rate, 5~10nm use Evaporation rate, 10~100nm use The evaporation rate was 100 nm to obtain a gold electrode with a thickness of 100 nm.
[0097] Example 13
[0098] Same as Example 1, except that:
[0099] S2, spin coating at a speed of 3500r / min for 25s. After the spin coating is completed, the wafer is removed from the spin coater and annealed on a constant temperature heating table at 140℃ for 35min to obtain a SnO with a thickness of 20nm. 2 ETL film (ie tin dioxide electron transport layer).
[0100] S3, on the electron transport layer obtained in step S2, on the already spin-coated SnO 2The ETL film substrate is coated at a scraping speed of 80 mm / min, the substrate heating temperature is 70°C, the gap between the scraper and the substrate surface is 90 μm, and a fluorine-containing lead iodide precursor solution is dripped into the gap, and a lead iodide film with a thickness of 570 nm is obtained by scraping; the fluorine-containing lead iodide precursor solution is prepared by the following steps: preparing a lead iodide precursor solution with a molar concentration of 1.2 mmol / mL, heating and stirring on a constant temperature heating table until it is completely dissolved, adding hexafluorobenzene as a fluorine-containing additive, and keeping it in a heated state to obtain a fluorine-containing lead iodide precursor solution with a volume fraction of 10% of the fluorine-containing additive;
[0101] S4, on the lead iodide film obtained in step S3, the wet film obtained by scraping was annealed at 140° C. for 20 min in an atmosphere with a humidity of 30% to 45%, with a scraping speed of 80 mm / min, the substrate was not heated, the gap between the scraper and the substrate surface was 90 μm, and a perovskite film with a thickness of 590 nm was obtained;
[0102] S5, spin coating at a spin coating speed of 3500 r / min for 40 s to obtain a hole transport layer with a thickness of 100 nm;
[0103] S6. Transfer the substrate with the HTL layer spin-coated from the glove box to a room with a temperature of (25±2)℃ and a humidity of 40%. Use a surgical blade to scrape a 3-4mm gap along the edge of the wafer in parallel. Transfer the wafer to the vacuum coating evaporation chamber of the glove box. Use the first 1nm Evaporation rate, 1~5nm use Evaporation rate, 5~10nm use Evaporation rate, 10~50nm use The evaporation rate was 50 nm to obtain a gold electrode with a thickness of 50 nm.
[0104] Embodiment 14
[0105] Same as Example 1, except that:
[0106] S2, spin coating at a speed of 4500r / min for 15s. After the spin coating is completed, the wafer is removed from the spin coater and annealed on a constant temperature heating table at 160℃ for 25min to obtain a SnO with a thickness of 40nm. 2 ETL film (ie tin dioxide electron transport layer).
[0107] S3, on the electron transport layer obtained in step S2, on the already spin-coated SnO 2The ETL film substrate is coated at a scraping speed of 120 mm / min, the substrate heating temperature is 70° C., the gap between the scraper and the substrate surface is 110 μm, and a fluorine-containing lead iodide precursor solution is dripped into the gap, and a lead iodide film with a thickness of 590 nm is obtained by scraping; the fluorine-containing lead iodide precursor solution is prepared by the following steps: preparing a lead iodide precursor solution with a molar concentration of 1.5 mmol / mL, heating and stirring on a constant temperature heating table until it is completely dissolved, adding hexafluorobenzene as a fluorine-containing additive, and keeping it in a heated state to obtain a fluorine-containing lead iodide precursor solution with a volume fraction of 20% of the fluorine-containing additive;
[0108] S4, on the lead iodide film obtained in step S3, the wet film obtained by scraping was annealed at 160° C. for 10 min in an atmosphere with a humidity of 30% to 45%, with a scraping speed of 120 mm / min, the substrate was not heated, the gap between the scraper and the substrate surface was 110 μm, and a perovskite film with a thickness of 610 nm was obtained;
[0109] S5, spin coating at a spin coating speed of 4500 r / min for 20 s to obtain a hole transport layer with a thickness of 200 nm;
[0110] S6. Transfer the substrate with the HTL layer spin-coated from the glove box to a room with a temperature of (25±2)℃ and a humidity of 40%. Use a surgical blade to scrape a 3-4mm gap along the edge of the wafer in parallel. Transfer the wafer to the vacuum coating evaporation chamber of the glove box. Use the first 1nm Evaporation rate, 1~5nm use Evaporation rate, 5~10nm use Evaporation rate, 10~100nm use The evaporation rate was 100 nm to obtain a gold electrode with a thickness of 100 nm.
[0111] The description of the above embodiments is only used to help understand the technical solution and core ideas of the present invention. It should be pointed out that for technicians in this technical field, several improvements and modifications can be made to the present invention without departing from the principles of the present invention. These improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A perovskite solar cell based on additive-assisted preparation of a high-quality photoactive layer, characterized in that: From bottom to top, it is composed of a substrate, an electron transport layer, an organic-inorganic perovskite structure photoactive layer, a hole transport layer and a back electrode layer. The organic-inorganic perovskite structure photoactive layer is prepared by doping a fluorine-containing additive to assist in preparing a lead iodide film, and then reacting on the lead iodide film to prepare a perovskite film. The fluorine-containing additive doping volume fraction is 1% to 25%.
2. The perovskite solar cell according to claim 1, characterized in that: The organic-inorganic perovskite structure photoactive layer is prepared by a two-step spin coating method or a two-step scraping method.
3. The perovskite solar cell according to claim 1 or 2, characterized in that: The fluorine-containing additive is a fluorine-containing aromatic hydrocarbon or a fluorine-containing alkane with a boiling point below 100°C.
4. The perovskite solar cell according to claim 3, characterized in that: The fluorine-containing aromatic hydrocarbon is hexafluorobenzene or octafluoronaphthalene, and the fluorine-containing alkane is perfluoropentane, perfluorohexane or perfluoroheptane.
5. The method for preparing a perovskite solar cell with a high-quality photoactive layer assisted by additives according to claim 1, characterized in that: The steps include: S1, cleaning the substrate; S2, preparing an electron transport layer on the substrate by a solution method; S3. Uniformly coating a fluorine-containing lead iodide precursor solution on the electron transport layer obtained in step S2 to obtain a lead iodide film, wherein the fluorine-containing lead iodide precursor solution is prepared according to the following steps: adding a fluorine-containing additive to a lead iodide precursor solution having a molar concentration of 1.2 to 1.5 mmol / mL to obtain a fluorine-containing lead iodide precursor solution having a fluorine-containing additive volume fraction of 1% to 25%; S4, uniformly coating a monovalent halide solution with a molar concentration of 1.2 to 1.5 mmol / mL on the lead iodide film obtained in step S3 to obtain a perovskite film, i.e., an organic-inorganic perovskite structure photoactive layer; S5. A hole transport layer and a back electrode layer are sequentially prepared on the perovskite film obtained in step S4 to finally obtain the perovskite solar cell.
6. The preparation method according to claim 5, characterized in that: The coating method in step S3 or S4 is scraping coating or spin coating.
7. The preparation method according to claim 6, characterized in that: The specific steps of steps S3 and S4 are: S3, on the electron transport layer obtained in step S2, spin-coating a fluorine-containing lead iodide precursor solution at a rotation speed of 1500-2000 rpm for 20-40 seconds, and after the spin coating is completed, thermal annealing is performed at less than 80° C. for 10-80 seconds to obtain a lead iodide film; S4. Spin coating a monovalent halide solution on the lead iodide film obtained in step S3 at a rotation speed of 1500-2000 rpm for 20-40 seconds. After the spin coating is completed, annealing is performed at 140° C.-160° C. for 10-20 minutes in an atmosphere with a humidity of 30%-45% to obtain a perovskite film.
8. The preparation method according to claim 6, characterized in that: The specific steps of steps S3 and S4 are: S3, on the electron transport layer obtained in step S2, the coating speed is 80-120 mm / min, the heating temperature of the transparent substrate is less than 80° C., the gap between the scraper and the substrate surface is 90-110 μm, and the lead iodide film is obtained by coating; S4. On the lead iodide film obtained in step S3, a monovalent halide solution is scraped at a speed of 80 to 120 mm / min. The substrate is not heated. The gap between the scraper and the substrate surface is 90 to 110 μm. The wet film obtained by scraping is annealed at 140° C. to 160° C. for 10 to 20 min in an atmospheric environment with a humidity of 30% to 45% to obtain a perovskite film.
9. The preparation method according to claim 5, characterized in that: The monovalent halide in step S4 has the general formula AX, where A is a +1 cation, including FA + 、MA + , Cs + , Rb + , X is a halogen ion, including Cl-, Br - ,I - .
10. The preparation method according to claim 5, characterized in that: The thickness of the electron transport layer is 20-40 nm, the thickness of the organic-inorganic perovskite structure photoactive layer is 580-620 nm, the thickness of the hole transport layer is 100-200 nm, and the thickness of the back electrode layer is 50-100 nm.
Citation Information
Patent Citations
Perovskite film for effectively fixing organic cations and preparation method of solar cell
CN110085744A
Perovskite solar cell doped with multifunctional additive and preparation method of perovskite solar cell
CN111525038A
Perovskite solar cell based on 1, 4-diiodotetrafluorobenzene doped hole transport layer and preparation method thereof
CN114583065A
Cited By
Application of compound in manufacturing perovskite thin-film solar cell and perovskite thin-film solar cell manufactured by using compound
CN117222237A