Window and display device including same
By adopting a specific layer structure in the display device, including a metal fluoride low refractive layer, a silicon-aluminum oxide functional layer and a perfluorinated compound layer, the deterioration of visibility and insufficient wear resistance caused by external light reflection in the display device is solved. Problem, better wear resistance and joint force are achieved.
Patent Information
- Application Number
- CN202380032672.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-08
- Filing Date
- 2023-04-07
- Publication Date
- 2024-11-22
AI Technical Summary
During use, the existing display devices are prone to deterioration in visibility due to external light reflection and lack of wear resistance.
A window structure including a substrate, a low refractive layer, a first functional layer and a second functional layer, wherein the low refractive layer is made of metal fluoride, the first functional layer is composed of silicon aluminum oxide and aluminum oxide, and the second functional layer is The layer is composed of a perfluorinated compound, and an oxide third functional layer is provided between the substrate and the low refractive layer to reduce reflectivity and increase bonding force.
Effectively prevent or reduce the deterioration of the visibility of the display device, improve the bonding force between layers, and thereby improve the wear resistance of the window.
Smart Images

Figure CN119014143A_ABST
Abstract
Description
Technical Field
[0001] One or more embodiments relate to a window and a display device including the window, and more particularly, to a window having reduced reflectivity and a display device including the window. Background Art
[0002] The use of display devices has been diversified. In addition, as display devices become thinner and lighter, their use range is gradually expanding.
[0003] As the display device is variously used, there may be various methods of designing the shape of the display device, and functions that may be combined or associated with the display device increase. Summary of the invention
[0004] Technical issues
[0005] One or more embodiments include a display device configured to prevent or reduce visibility deterioration. However, this technical problem is an example, and the present disclosure is not limited thereto.
[0006] Technical Solutions
[0007] According to one or more embodiments, the window includes: a substrate; a low-refractive layer disposed on the substrate and including a metal fluoride; a first functional layer disposed on the low-refractive layer, having a thickness of about 5 nanometers (nm) to about 25 nm and including an oxide; and a second functional layer disposed on the first functional layer and including a perfluorinated compound.
[0008] The low-refractive layer may include magnesium fluoride.
[0009] The low-refractive layer may have a refractive index of about 1.2 to about 1.4.
[0010] The low refractive layer may have a thickness of about 50 nm to about 150 nm.
[0011] The low-refractive layer may have a crystalline structure.
[0012] The first functional layer may include silicon aluminum oxide.
[0013] The first functional layer may include silicon oxide in which aluminum atoms are employed.
[0014] The first functional layer may include a substitutional solid solution in which some of silicon atoms of silicon oxide are substituted with aluminum atoms.
[0015] The first functional layer may include a penetrating solid solution in which aluminum atoms penetrate through a crystal lattice of silicon oxide.
[0016] The first functional layer may include aluminum oxide in which silicon atoms are employed.
[0017] The first functional layer may include a substitutional solid solution in which some of aluminum atoms of aluminum oxide are substituted with silicon atoms.
[0018] The first functional layer may have a refractive index of about 1.4 to about 1.6.
[0019] The second functional layer may have a thickness of about 5 nm to about 30 nm.
[0020] The window may further include a third functional layer disposed between the substrate and the low-refractive layer and including an oxide.
[0021] The third functional layer may include one of yttrium oxide, magnesium oxide, and aluminum oxide.
[0022] The refractive index of the third functional layer may be greater than the refractive index of the low-refractive layer.
[0023] The third functional layer may have a refractive index of about 1.6 to about 1.8.
[0024] The third functional layer may have a thickness of about 5 nm to about 30 nm.
[0025] After applying a load of 1 kilogram (Kg) to the surface of the window using a rubber and reciprocating a distance of 15 millimeters (mm) 6000 times at a speed of 40 cycles per minute (cycles / minute), the contact angle of the window surface with respect to water can be about 95° or greater.
[0026] According to one or more embodiments, a display device includes a display panel and a window disposed on the display panel, wherein the display panel includes a display substrate, a light emitting element disposed above the display substrate, and a filter layer disposed on the light emitting element and including a color filter layer and a light blocking layer. The window includes: a substrate; a low refractive layer disposed on the substrate and including a metal fluoride; a first functional layer disposed on the low refractive layer, having a thickness of about 5 nm to about 25 nm and including an oxide; and a second functional layer disposed on the first functional layer and including a perfluorinated compound.
[0027] The light emitting element may include a pixel electrode, an emission layer, and an opposite electrode, and the display device may further include a pixel defining layer defining a first opening exposing at least a portion of the pixel electrode.
[0028] A second opening may be defined in the light blocking layer, wherein the second opening overlaps the first opening.
[0029] At least a portion of the color filter layer may be located within the second opening.
[0030] The low-refractive layer may include magnesium fluoride, have a refractive index of 1.2 to 1.4, and have a thickness of 50 nm to 150 nm.
[0031] The first functional layer may include silicon aluminum oxide.
[0032] The first functional layer may include silicon oxide in which aluminum atoms are employed.
[0033] The first functional layer may include a substitutional solid solution in which some of silicon atoms of silicon oxide are substituted with aluminum atoms, or a penetrating solid solution in which aluminum atoms penetrate through a crystal lattice of silicon oxide.
[0034] The window may further include a third functional layer disposed between the substrate and the low-refractive layer and including an oxide.
[0035] The refractive index of the third functional layer may be greater than the refractive index of the low-refractive layer.
[0036] After applying a load of 1 Kg to the surface of the window using a rubber and reciprocating a distance of 15 mm at a speed of 40 cycles / min 6000 times, the contact angle of the surface of the window with respect to water may be about 95° or more.
[0037] These and / or other aspects will become apparent and more readily understood from the following description of embodiments, the accompanying drawings, and the claims.
[0038] Beneficial Effects
[0039] According to the embodiment, the visibility of the display device can be prevented or reduced from being deteriorated due to external light reflection. In addition, the bonding force between the layers included in the window can be improved, and thus, the wear resistance of the window can be improved. However, the scope of the present disclosure is not limited by this effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 is a schematic plan view of a display device according to an embodiment.
[0041] Figure 2 is a schematic cross-sectional view of a display device according to an embodiment.
[0042] Figure 3 is a schematic cross-sectional view of a display device according to an embodiment.
[0043] Figure 4 is a schematic cross-sectional view of a window included in a display device according to an embodiment.
[0044] Figure 5 3 is a graph showing the results of the wear resistance evaluation of the first embodiment.
[0045] Figure 6 3 is a graph showing the results of the wear resistance evaluation of the first embodiment.
[0046] Figure 7is a graph showing the results of wear resistance evaluation of comparative examples.
[0047] Figure 8 is a graph showing the results of wear resistance evaluation of comparative examples.
[0048] Fig. 9 is a schematic cross-sectional view of a window included in a display device according to an embodiment.
[0049] Fig.10 This is a graph showing the results of the wear resistance evaluation of the second embodiment.
[0050] Fig.11 This is a graph showing the results of the wear resistance evaluation of the second embodiment. DETAILED DESCRIPTION
[0051] Reference will now be made in detail to embodiments, examples of which are shown in the accompanying drawings, wherein like reference numerals denote like elements throughout. In this regard, the embodiments may have different forms and should not be construed as being limited to the descriptions set forth herein. Therefore, embodiments are described below only by reference to the accompanying drawings to explain various aspects of the specification.
[0052] Since the present disclosure allows various changes and multiple embodiments, certain embodiments will be shown in the drawings and described in the written description. The effects and features of the present disclosure and methods for achieving them will be explained with reference to the embodiments described in detail below with reference to the drawings. However, the present disclosure is not limited to the following embodiments and can be implemented in various forms.
[0053] Although terms such as "first" and "second" may be used to describe various components, these components should not be limited to the above terms. The above terms are used to distinguish one component from another.
[0054] As used herein, the singular forms “a”, “an” and “the” are intended to include the plural forms as well, unless the context clearly indicates otherwise.
[0055] It will be understood that the terms “comprising,” “including,” “includes,” and / or “comprising” as used herein specify the presence of stated features or components, but do not preclude the addition of one or more other features or components.
[0056] It will also be understood that when a layer, region or component is referred to as being "on" another layer, region or component, it can be directly or indirectly on the other layer, region or component. That is, for example, intervening layers, regions or components may be present.
[0057] For convenience of explanation, the size of the elements in the drawings may be exaggerated or reduced. As an example, for convenience of description, the size and thickness of each element shown in the drawings are arbitrarily represented, and therefore, the present disclosure is not necessarily limited thereto.
[0058] In the present specification, "or" means "and / or". "A and / or B" means A or B, or A and B. In the present specification, "at least one of A and B" means A or B, or A and B.
[0059] As used herein, when a wiring is referred to as “extending in the first direction or the second direction”, this means that the wiring extends not only in a straight line shape but also in a zigzag shape or a curved line in the first direction or the second direction.
[0060] As used herein, "on a plan view" means observing the target portion from above, and "on a cross-sectional view" means observing a vertically intercepted cross section of the target portion from the side. As used herein, "overlap" includes overlap in a "plan view" and overlap in a "cross-sectional view".
[0061] In view of the measurements discussed and the errors associated with the measurement of a particular quantity (i.e., the limitations of the measurement system), "about" or "approximately" as used herein includes the stated value and means within an acceptable deviation range for a particular value as determined by one of ordinary skill in the art. For example, "about" may mean within one or more standard deviations, or within ±30%, ±20%, ±10%, or ±5% of the stated value. Hereinafter, embodiments of the present disclosure are described in detail with reference to the accompanying drawings. When described with reference to the accompanying drawings, the same reference numerals are used for the same or corresponding elements.
[0062] Figure 1 is a schematic plan view of a display device 1 according to an embodiment.
[0063] refer to Figure 1 , the display device 1 includes a display area DA configured to display an image and a peripheral area PA arranged around the display area DA. The display device 1 can display an image to the outside by using light emitted from the display area DA. Alternatively, since the display device 1 includes the display substrate 100, it can be understood that the display substrate 100 includes the display area DA and the peripheral area PA.
[0064] The display substrate 100 may include various materials such as glass, metal or plastic. In an embodiment, the display substrate 100 may include a flexible material. Here, the flexible material may be a material that is easily warped, bendable, foldable or rollable. The display substrate 100 of the flexible material may include ultra-thin glass, metal or plastic.
[0065] The pixels PX may be arranged in a display area DA of the display substrate 100, wherein each of the pixels PX includes a light emitting element, such as an organic light emitting diode OLED. The pixels PX may be arranged in a plurality. The plurality of pixels PX may be arranged in various configurations, such as a stripe configuration, a pentile configuration, a mosaic configuration, etc., to display an image. Hereinafter, although it is described that the display device 1 according to the embodiment includes a light emitting element, and the light emitting element is an organic light emitting diode, the embodiment is not limited thereto. As an example, the light emitting element may be an inorganic light emitting diode, a quantum dot light emitting diode, etc.
[0066] Despite Figure 1 , the planar shape of the display area DA is shown to be a rectangle, but the embodiment is not limited thereto. As an example, the display area DA may be set to a polygonal shape such as a triangle, a pentagon, a hexagon, a circular shape, an elliptical shape, an irregular shape, etc.
[0067] The peripheral area PA of the display substrate 100 is an area arranged around the display area DA and may be an area in which an image is not displayed. Pads may be arranged in the peripheral area PA, wherein various wirings, printed circuit boards, or driver integrated circuit ("IC") chips configured to transmit electrical signals to the display area DA are attached to the pads.
[0068] Figure 2 is a schematic cross-sectional view of a display device 1 according to an embodiment.
[0069] refer to Figure 2 , the display device 1 may include a display panel 10 and a window 600. The window 600 may be provided on the display panel 10. The display panel 10 may include a display substrate 100, a display layer 200, an encapsulation layer 300, an input sensing layer 400, and an optical filter layer 500 stacked in sequence. Since the display device 1 includes the display panel 10, it can be understood that the display device 1 includes a display substrate 100, a display layer 200, an encapsulation layer 300, an input sensing layer 400, and an optical filter layer 500 stacked in sequence.
[0070] The display substrate 100 may include a glass material, a ceramic material, a metal, or a flexible or bendable material. In the case where the display substrate 100 is flexible or bendable, the display substrate 100 may include a polymer resin such as polyethersulfone, polyacrylate, polyetherimide, polyethylene naphthalate, polyethylene terephthalate, polyphenylene sulfide, polyarylate, polyimide, polycarbonate, and cellulose acetate propionate.
[0071] The display substrate 100 may have a single layer structure or a multi-layer structure of the above materials, and may further include an inorganic layer in the case of a multi-layer structure. Alternatively, the display substrate 100 may have a structure of organic material / inorganic material / organic material / inorganic material.
[0072] The display layer 200 may be disposed on the display substrate 100. The display layer 200 may include a thin film transistor, a light emitting element, an inorganic insulating layer, and an organic insulating layer.
[0073] The encapsulation layer 300 may be disposed on the display layer 200. The encapsulation layer 300 may include at least one inorganic layer and at least one organic layer. Alternatively, the encapsulation layer 300 may include an encapsulation substrate including glass. In the case where the encapsulation layer 300 includes glass, a sealant including glass frit or the like may be disposed between the display substrate 100 and the encapsulation layer 300. The sealant may be disposed in the peripheral area PA (see Figure 1 The sealant disposed in the peripheral area PA may surround the display area DA and prevent or reduce moisture from penetrating through the side surface of the display device 1.
[0074] The input sensing layer 400 may be disposed on the encapsulation layer 300. The input sensing layer 400 may obtain coordinate information corresponding to an external input (e.g., a touch event). The input sensing layer 400 may be formed separately on a touch substrate and then adhered to the encapsulation layer 300 through an adhesive layer such as an optically transparent adhesive OCA. Alternatively, the input sensing layer 400 may be directly formed on the encapsulation layer 300. In this case, the adhesive layer may not be disposed between the input sensing layer 400 and the encapsulation layer 300.
[0075] In an embodiment, the filter layer 500 may be disposed on the input sensing layer 400. Figure 3 As described, the filter layer 500 may include a light blocking layer 510 (see Figure 3 ), color filter layer 520 (see Figure 3 ) and outer coating 530 (see Figure 3 ). Figure 3 Described in more detail in .
[0076] In an embodiment, the window 600 may be disposed on the filter layer 500. Figure 4 As described, the window 600 may include a substrate 610 (see Figure 4 ), low refractive layer 620 (see Figure 4 ), the first functional layer 630 (see Figure 4 ) and a second functional layer 640 (see Figure 4 ). Figure 4 Described in more detail in .
[0077] Figure 6 is a schematic cross-sectional view of a display device according to an embodiment. Specifically, Figure 3 is arranged in the display area DA (see Figure 1 ) is a cross-sectional view of an element in FIG.
[0078] refer to Figure 3 , the display device 1 may include a display substrate 100, a light emitting element OLED and a filter layer 500. In this case, the light emitting element OLED may be an organic light emitting diode.
[0079] In addition, the pixel circuit PC may be disposed over the display substrate 100. Figure 3 Pixel circuit PC is shown to include two transistors, but the embodiment is not limited thereto. Pixel circuit PC may include three or more transistors. As an example, pixel circuit PC may include seven transistors or nine transistors.
[0080] The display substrate 100 may have a structure in which a layer including an organic material and a layer including an inorganic material are alternately stacked. As an example, the display substrate 100 may include a first base layer 101, a first barrier layer 102, a second base layer 103, and a second barrier layer 104 stacked in sequence. However, the embodiment is not limited thereto. The display substrate 100 may include glass.
[0081] The first base layer 101 and the second base layer 103 may each include an organic material. As an example, the first base layer 101 and the second base layer 103 may each include one of polyimide, polyethylene naphthalate, polyethylene terephthalate, polyarylate, polycarbonate, polyetherimide, and polyethersulfone. The first base layer 101 and the second base layer 103 may include the same material or different materials.
[0082] The first barrier layer 102 may be disposed between the first base layer 101 and the second base layer 103. In addition, the second barrier layer 104 may be disposed on the second base layer 103. The first barrier layer 102 and the second barrier layer 104 may each include an inorganic material. As an example, the first barrier layer 102 and the second barrier layer 104 may each include silicon oxide, silicon oxynitride, silicon nitride, amorphous silicon, etc. In an embodiment, the first barrier layer 102 may include two layers including different materials. In this case, the refractive indexes of the two layers may be different from each other. As an example, the first barrier layer 102 may include two layers including silicon oxynitride and silicon oxide having a refractive index less than that of silicon oxynitride. However, the embodiment is not limited thereto.
[0083] The buffer layer 111 may be disposed on the display substrate 100. The buffer layer 111 may reduce or prevent penetration of foreign materials, moisture, or external air from under the display substrate 100. The buffer layer 111 may include an inorganic material such as silicon nitride, silicon oxynitride, and silicon oxide, and include a single layer or a multilayer including the above inorganic material.
[0084] The semiconductor pattern may be disposed on the buffer layer 111. Hereinafter, the semiconductor pattern directly disposed on the buffer layer 111 is defined as a first semiconductor pattern. The first semiconductor pattern may include a silicon semiconductor. The first semiconductor pattern may include polycrystalline silicon. However, the embodiment is not limited thereto. As an example, the first semiconductor pattern may include amorphous silicon. Alternatively, the first semiconductor pattern may include an oxide semiconductor. In this case, the oxide semiconductor may include a crystalline or amorphous oxide semiconductor.
[0085] The first semiconductor pattern may include a doped region and a non-doped region. The doped region may be doped with an N-type dopant or a P-type dopant. The P-type transistor may include a doped region doped with a P-type dopant.
[0086] The first transistor T1 may include a source S1, an active portion A1, and a drain D1. The source S1, the active portion A1, and the drain D1 of the first transistor T1 may include a first semiconductor pattern. The source S1 may be separated from the drain D1 of the first transistor T1 with the active portion A1 of the first transistor T1 therebetween.
[0087] The first insulating layer 113 may be disposed on the buffer layer 111. The first insulating layer 113 may cover the first semiconductor pattern. In an implementation, the first insulating layer 113 may include an inorganic material such as silicon nitride, silicon oxynitride, and silicon oxide, and include a single layer or multiple layers including the above inorganic material.
[0088] The gate G1 of the first transistor T1 may be disposed on the first insulating layer 113. The gate G1 may be a portion of a metal pattern. The gate G1 of the first transistor T1 may overlap at least a portion of a first semiconductor pattern disposed thereunder. As an example, the gate G1 may overlap an active portion A1 disposed thereunder. The gate G1 may include a low-resistance conductive material such as molybdenum (Mo), aluminum (Al), copper (Cu), and / or titanium (Ti), and may have a single-layer structure or a multi-layer structure including the above materials.
[0089] The second insulating layer 115 may be disposed on the first insulating layer 113. The second insulating layer 115 may cover the gate G1 of the first transistor T1 disposed on the first insulating layer 113. The second insulating layer 115 may include an inorganic material such as silicon nitride, silicon oxynitride, and silicon oxide, and include a single layer or multiple layers including the above inorganic materials.
[0090] The upper electrode UE may be disposed on the second insulating layer 115. The upper electrode UE may overlap at least a portion of the gate G1 of the first transistor T1 disposed thereunder. The upper electrode UE may be a portion of a metal pattern or a portion of a doped semiconductor pattern. The portions where the gate G1 and the upper electrode UE overlap each other may constitute a storage capacitor. However, the upper electrode UE may be omitted.
[0091] The third insulating layer 117 may be disposed on the second insulating layer 115. The third insulating layer 117 may cover the upper electrode UE disposed on the second insulating layer 115. The third insulating layer 117 may include an inorganic material such as silicon nitride, silicon oxynitride, and silicon oxide, and include a single layer or multiple layers including the above inorganic materials. In an embodiment, the third insulating layer 117 may include a plurality of silicon oxide layers and silicon nitride layers alternately stacked.
[0092] The semiconductor pattern may be disposed on the third insulating layer 117. Hereinafter, the semiconductor pattern directly disposed on the third insulating layer 117 is defined as a second semiconductor pattern. The second semiconductor pattern may include an oxide semiconductor. The oxide semiconductor may include a crystalline or amorphous oxide semiconductor. However, the embodiment is not limited thereto. The second semiconductor pattern may include a silicon semiconductor. As an example, the second semiconductor pattern may include polycrystalline silicon or amorphous silicon.
[0093] The oxide semiconductor may include at least one of indium (In), gallium (Ga), tin (Sn), zirconium (Zr), vanadium (V), hafnium (Hf), cadmium (Cd), germanium (Ge), chromium (Cr), titanium (Ti), and zinc (Zn). Alternatively, the oxide semiconductor may include at least one of indium tin oxide ("ITO"), indium gallium zinc oxide ("IGZO"), zinc oxide (ZnO), indium zinc oxide (IZnO), indium zinc oxide ("ZIO"), indium oxide (InO), titanium oxide (TiO), indium zinc tin oxide ("IZTO"), zinc tin oxide ("ZTO"), etc.
[0094] The second transistor T2 may include a source S2, an active portion A2, and a drain D2. The source S2, the active portion A2, and the drain D2 of the second transistor T2 may include a second semiconductor pattern. The source S2 and the drain D2 of the second transistor T2 may include a metal reduced from a metal oxide semiconductor. The source S2 and the drain D2 of the second transistor T2 may include a metal layer having a predetermined thickness from an upper surface of the second semiconductor pattern and including the reduced metal.
[0095] The fourth insulating layer 119 may be disposed on the third insulating layer 117. The fourth insulating layer 119 may cover the second semiconductor pattern disposed on the third insulating layer 117. The fourth insulating layer 119 may include an inorganic material such as silicon nitride, silicon oxynitride, and silicon oxide, and include a single layer or multiple layers including the above inorganic material.
[0096] Although not shown, the fourth insulating layer 119 may be patterned to correspond to the gate G2 of the second transistor T2 disposed on the fourth insulating layer 119. That is, in a plan view, the gate G2 and the fourth insulating layer 119 may be provided in the same shape. However, embodiments are not limited thereto.
[0097] The gate G2 of the second transistor T2 may be disposed on the fourth insulating layer 119. The gate G2 may be a portion of a metal pattern. The gate G2 of the second transistor T2 may overlap at least a portion of a second semiconductor pattern disposed below the gate G2. As an example, the gate G2 may overlap an active portion A2 disposed below the gate G2. The gate G2 may include a conductive material such as a low-resistance material of molybdenum (Mo), aluminum (Al), copper (Cu), and / or titanium (Ti), and may have a single-layer structure or a multi-layer structure including the above materials.
[0098] The fifth insulating layer 121 may be disposed on the fourth insulating layer 119. The fifth insulating layer 121 may cover the gate G2 disposed on the fourth insulating layer 119. The fifth insulating layer 121 may include an inorganic material such as silicon nitride, silicon oxynitride, and silicon oxide, and include a single layer or multiple layers including the above inorganic materials. In an embodiment, the fifth insulating layer 121 may include a plurality of silicon oxide layers and silicon nitride layers alternately stacked.
[0099] Despite Figure 3 117, but the embodiment is not limited thereto. The second semiconductor pattern may be omitted. In this case, the source S2, the active portion A2, and the drain D2 of the second transistor T2 may include the first semiconductor pattern. That is, the source S2, the active portion A2, and the drain D2 of the second transistor T2 may be disposed on the same layer on which the source S1, the active portion A1, and the drain D1 of the first transistor T1 are disposed.
[0100] At least one organic insulating layer may be disposed on the fifth insulating layer 121. A first organic insulating layer 160 and a second organic insulating layer 170 may be disposed on the fifth insulating layer 121. The first organic insulating layer 160 and the second organic insulating layer 170 may include a single layer of at least one of a polyimide-based resin, an acrylic resin, a methacrylic resin, polyisoprene, an ethylene-based resin, an epoxy-based resin, a urethane-based resin, a cellulose-based resin, a siloxane-based resin, a polyamide-based resin, and a perylene-based resin.
[0101] In an embodiment, the first organic insulating layer 160 and the second organic insulating layer 170 may include different materials. As an example, the first organic insulating layer 160 may include a siloxane-based resin, and the second organic insulating layer 170 may include a polyimide-based resin. Alternatively, the first organic insulating layer 160 may include a polyimide-based resin, and the second organic insulating layer 170 may include a siloxane-based resin. However, embodiments are not limited thereto. As an example, the first organic insulating layer 160 may include the same material as that of the second organic insulating layer 170.
[0102] The first connection electrode CNE1 may be disposed on the fifth insulating layer 121. The second connection electrode CNE2 may be disposed on the first organic insulating layer 160. The second connection electrode CNE2 may be connected to the first connection electrode CNE1 through a first through hole VIA1 defined in the first organic insulating layer 160.
[0103] The light emitting element OLED may be disposed on the second organic insulating layer 170. In an embodiment, the light emitting element OLED may be an organic light emitting diode. The light emitting element OLED may include a pixel electrode 210, an intermediate layer 220, and an opposite electrode 230 stacked in sequence. The pixel electrode 210 may be disposed on the second organic insulating layer 170.
[0104] The pixel defining layer 180 may be disposed on the second organic insulating layer 170 and the pixel electrode 210, wherein a first opening 180OP exposing at least a portion of the pixel electrode 210 is defined in the pixel defining layer 180. An emission area EA of light emitted from the first opening 180OP of the pixel defining layer 180 may be defined by the first opening 180OP of the pixel defining layer 180. As an example, a width of the first opening 180OP may correspond to a width of the emission area EA. Surrounding the emission area EA is a non-emission area NEA, which may surround the emission area EA.
[0105] The pixel defining layer 180 may include an organic insulating material. Alternatively, the pixel defining layer 180 may include an inorganic insulating material, such as silicon oxide, silicon oxynitride, and silicon nitride. Alternatively, the pixel defining layer 180 may include an organic insulating material and an inorganic insulating material. In an embodiment, the pixel defining layer 180 may include a light blocking material. The light blocking material may include carbon black, carbon nanotubes, a resin or paste including a black dye, metal particles such as nickel, aluminum, molybdenum, and alloys thereof, metal oxide particles (e.g., chromium oxide) or metal nitride particles (e.g., chromium nitride). In the case where the pixel defining layer 180 includes a light blocking material, external light reflection caused by a metal structure arranged below the pixel defining layer 180 may be reduced.
[0106] Although not shown, a spacer may be disposed on the pixel defining layer 180. The spacer may include an organic insulating material such as polyimide. Alternatively, the spacer may include an inorganic insulating material such as silicon nitride or silicon oxide, or include an organic insulating material and an inorganic insulating material.
[0107] In an embodiment, the spacer may include the same material as that of the pixel defining layer 180. In this case, the pixel defining layer 180 and the spacer may be formed together during a mask process using a half-tone mask or the like. However, embodiments are not limited thereto. As an example, the spacer may include a material different from that of the pixel defining layer 180.
[0108] The pixel electrode 210 may be disposed on the second organic insulating layer 170. The pixel electrode 210 may be electrically connected to the second connection electrode CNE2 through a second through hole VIA2 defined in the second organic insulating layer 170. The pixel electrode 210 may include an indium tin oxide (ITO), indium zinc oxide (IZO), zinc oxide (ZnO), indium oxide (In 2 O 3 ), indium gallium oxide (IGO), or aluminum zinc oxide (AZO). In an embodiment, the pixel electrode 210 may include a reflective layer including silver (Ag), magnesium (Mg), aluminum (Al), platinum (Pt), palladium (Pd), gold (Au), nickel (Ni), neodymium (Nd), iridium (Ir), chromium (Cr), or a compound thereof. In an embodiment, the pixel electrode 210 may further include a layer above / below the reflective layer, the layer including ITO, IZO, ZnO x or In 2 O 3 As an example, the pixel electrode 210 may have a multi-layer structure of ITO / Ag / ITO.
[0109] The intermediate layer 220 may be disposed on the pixel electrode 210. The intermediate layer 220 may include a first auxiliary layer 220a, an emission layer 220b, and a second auxiliary layer 220c sequentially stacked. The first auxiliary layer 220a and the second auxiliary layer 220c may be collectively referred to as an organic functional layer 220e.
[0110] The emission layer 220b may be disposed within the first opening 180OP of the pixel defining layer 180. The emission layer 220b may include a polymer organic material or a low molecular weight organic material that emits light having a preset color.
[0111] The organic functional layer 220e may include at least one of a first auxiliary layer 220a and a second auxiliary layer 220c, wherein the first auxiliary layer 220a is located between the pixel electrode 210 and the emission layer 220b, and the second auxiliary layer 220c is located between the emission layer 220b and the opposite electrode 230. As an example, the first auxiliary layer 220a may be located between the pixel electrode 210 and the emission layer 220b, and the second auxiliary layer 220c may not be located between the emission layer 220b and the opposite electrode 230. That is, the second auxiliary layer 220c may be omitted.
[0112] In an implementation, the first auxiliary layer 220a may not be located between the pixel electrode 210 and the emission layer 220b, and the second auxiliary layer 220c may be located between the emission layer 220b and the opposite electrode 230. That is, the first auxiliary layer 220a may be omitted.
[0113] In an embodiment, the first auxiliary layer 220a may be located between the pixel electrode 210 and the emission layer 220b, and the second auxiliary layer 220c may be located between the emission layer 220b and the opposite electrode 230. Hereinafter, the case where the first auxiliary layer 220a and the second auxiliary layer 220c are included is mainly described in detail.
[0114] The first auxiliary layer 220a may include, for example, a hole transport layer ("HTL") and / or a hole injection layer ("HIL"). The second auxiliary layer 220c may include an electron transport layer ("ETL") and / or an electron injection layer ("EIL"). The first auxiliary layer 220a and / or the second auxiliary layer 220c may be a common layer that completely covers the display substrate.
[0115] The relative electrode 230 may include a conductive material having a low work function. As an example, the relative electrode 230 may include a (semi) transparent layer including silver (Ag), magnesium (Mg), aluminum (Al), platinum (Pt), palladium (Pd), gold (Au), nickel (Ni), neodymium (Nd) and iridium (Ir), chromium (Cr), lithium (Li), calcium (Ca) or an alloy thereof. Alternatively, the relative electrode 230 may also include a layer on the (semi) transparent layer including ITO, IZO, ZnO or In 2 O 3 Although not shown, a capping layer may be further disposed on the opposite electrode 230. The capping layer may include lithium fluoride (LiF), an inorganic material, and / or an organic material.
[0116] The encapsulation layer 300 may be disposed on the light emitting element OLED. The encapsulation layer 300 may include a thin film encapsulation layer or an encapsulation substrate. Hereinafter, the case where the encapsulation layer 300 includes a thin film encapsulation layer is mainly described in detail.
[0117] In an implementation, the encapsulation layer 300 may include at least one inorganic layer and at least one organic layer. For example, the thin film encapsulation layer 300 may include a first inorganic layer 310, an organic layer 320, and a second inorganic layer 330 sequentially stacked.
[0118] The first inorganic layer 310 may be disposed on the opposite electrode 230. The first inorganic layer 310 may prevent or reduce external moisture or oxygen from penetrating the light emitting element OLED. The organic layer 320 may be disposed on the first inorganic layer 310. The organic layer 320 may provide a flat surface on the first inorganic layer 310. Since the curved portion or particles formed on the upper surface of the first inorganic layer 310 may be covered by the organic layer 320, the surface state of the upper surface of the first inorganic layer 310 may be blocked from affecting the elements disposed on the organic layer 320. The second inorganic layer 330 may be disposed on the organic layer 320.
[0119] The first inorganic layer 310 and the second inorganic layer 330 may include at least one inorganic material of aluminum oxide, titanium oxide, tantalum oxide, hafnium oxide, zinc oxide, silicon oxide, silicon nitride, and silicon oxynitride. The first inorganic layer 310 and the second inorganic layer 330 may include a single layer or multiple layers containing the above materials. The organic layer 320 may include a polymer-based material. The polymer-based material may include an acrylic-based resin, an epoxy-based resin, a polyimide, and polyethylene. In an embodiment, the organic layer 320 may include an acrylate.
[0120] The input sensing layer 400 may be disposed on the encapsulation layer 300. The input sensing layer 400 may include a first sensing insulating layer 410, a first conductive pattern 420, a second sensing insulating layer 430, a second conductive pattern 440, and a third sensing insulating layer 450.
[0121] The first sensing insulating layer 410 may be disposed on the encapsulation layer 300. In addition, the first conductive pattern 420 may be disposed on the first sensing insulating layer 410 and covered by the second sensing insulating layer 430. In addition, the second conductive pattern 440 may be disposed on the second sensing insulating layer 430 and covered by the third sensing insulating layer 450. The first sensing insulating layer 410, the second sensing insulating layer 430, and the third sensing insulating layer 450 may each include at least one of an inorganic material and an organic material.
[0122] The first conductive pattern 420 and the second conductive pattern 440 may each have conductivity. The first conductive pattern 420 and the second conductive pattern 440 may each be set as a single layer or a multilayer. In addition, in a plan view, at least one of the first conductive pattern 420 and the second conductive pattern 440 may be set as a grid line. In a plan view, the grid lines constituting the first conductive pattern 420 and the second conductive pattern 440 may not overlap with the emission layer 220b. Therefore, even if the input sensing layer 400 is formed on the light emitting element OLED, the light emitted from the emission layer 220b of the light emitting element OLED can be provided to the user without being interfered by the input sensing layer 400.
[0123] In the case where the light blocking layer 510 is directly formed on the second conductive pattern 440, at least a portion of the second conductive pattern 440 may be damaged during the process of patterning the light blocking layer 510. Therefore, since the third sensing insulating layer 450 is disposed on the second conductive pattern 440, damage to the second conductive pattern 440 may be prevented or reduced.
[0124] The filter layer 500 may be disposed on the input sensing layer 400. The filter layer 500 may include a light blocking layer 510, a color filter layer 520, and an outer coating layer 530. In an embodiment, the color filter layer 520 may be disposed on the input sensing layer 400. The color filter layer 520 may overlap at least a portion of the emission layer 220b disposed below the color filter layer 520. The color filter layer 520 may be configured to selectively transmit light corresponding to the light provided from the emission layer 220b. As an example, in the case where the emission layer 220b is configured to provide blue light, the color filter layer 520 may be a blue filter that transmits blue light. Alternatively, in the case where the emission layer 220b is configured to provide green light, the color filter layer 520 may be a green filter that transmits green light. Alternatively, in the case where the emission layer 220b is configured to provide red light, the color filter layer 520 may be a red filter that transmits red light.
[0125] The color filter layer 520 may include a polymer photosensitive resin, a pigment, or a dye. As an example, the color filter layer 520 overlapping the emission layer 220b configured to provide blue light may include a blue pigment or dye, the color filter layer 520 overlapping the emission layer 220b configured to provide green light may include a green pigment or dye, and the color filter layer 520 overlapping the emission layer 220b configured to provide red light may include a red pigment or dye.
[0126] However, the embodiment is not limited thereto, and the color filter layer 520 overlapped with the emission layer 220b configured to provide blue light may not include a pigment or a dye. In this case, the color filter layer 520 may be transparent and may include a transparent photosensitive resin.
[0127] The light blocking layer 510 may be arranged between the color filter layers 520 configured to provide different lights. The light blocking layer 510 is a pattern having black color and is a matrix having a lattice shape. The light blocking layer 510 may include a black colorant. The black colorant may include a black dye and a black pigment. The black colorant may include carbon black, a metal such as chromium, or an oxide thereof. In an embodiment, the light blocking layer 510 may include the same material as the material of the pixel defining layer 180.
[0128] In an embodiment, a second opening 510OP may be defined in the light blocking layer 510. The second opening 510OP may overlap with the first opening 180OP defined in the pixel defining layer 180. In addition, the second opening 510OP may overlap with the emission area EA. In an embodiment, the color filter layer 520 may be disposed in the second opening 510OP defined in the light blocking layer 510.
[0129] An overcoat layer 530 may be disposed on the light blocking layer 510 and the color filter layer 520. The overcoat layer 530 is a light-transmitting layer having no color in the visible light band, and may provide a flat upper surface covering uneven portions occurring in a process of forming the light blocking layer 510 and the color filter layer 520. As an example, the overcoat layer 530 may include a light-transmitting organic material such as an acrylic-based resin.
[0130] In an embodiment, the window 600 may be disposed on the filter layer 500. This will refer to Figure 4 Describe in more detail.
[0131] Figure 4 is a schematic cross-sectional view of a window included in a display device according to an embodiment.
[0132] refer to Figure 4, the window 600 may include a substrate 610, a low-refractive layer 620, a first functional layer 630, and a second functional layer 640. In this case, the low-refractive layer 620, the first functional layer 630, and the second functional layer 640 may be sequentially stacked on the substrate 610.
[0133] In an embodiment, the substrate 610 may include glass. However, the embodiment is not limited thereto. In another embodiment, the substrate 610 may include a polymer resin. The refractive index n1 of the substrate 610 may be about 1.51. Specifically, the refractive index n1 of the substrate 610 relative to a wavelength of about 550 nanometers (nm) may be about 1.51.
[0134] In an embodiment, the low-refractive layer 620 may be disposed on the substrate 610. The low-refractive layer 620 may include a low-refractive material. The low-refractive layer 620 may include a metal fluoride. The low-refractive layer 620 may include magnesium fluoride (MgF 2 ), calcium fluoride (CaF 2 ), aluminum fluoride (AlF 3 ) and ytterbium fluoride (YbF 3 As an example, the low-refractive layer 620 may include magnesium fluoride (MgF 2 The magnesium fluoride (MgF) included in the low refractive layer 620 2 ) may have a crystalline structure.
[0135] In an embodiment, the refractive index n2 of the low-refractive layer 620 may be about 1.2 to about 1.4. Specifically, the refractive index n2 of the low-refractive layer 620 with respect to a wavelength of about 550 nm may be about 1.38.
[0136] In an embodiment, the thickness t1 of the low-refractive layer 620 may be 50nm to 150nm. Alternatively, the thickness t1 of the low-refractive layer 620 may be about 60nm to about 80nm. Specifically, the thickness t1 of the low-refractive layer 620 may be about 68nm. In the case where the thickness t1 of the low-refractive layer 620 is too thin (e.g., less than 50nm), the reflectivity of the window 600 including the low-refractive layer 620 may not be reduced because the reflectivity varies greatly for each wavelength. In addition, in the case where the thickness t1 of the low-refractive layer 620 is too thick (e.g., greater than 150nm) compared to other layers, the reflectivity of the window 600 including the low-refractive layer 620 may not be reduced.
[0137] In the case where refractive layers having different refractive indices are formed on the substrate 610, a plurality of chambers may be used in the process of manufacturing the window 600. In the window 600 according to the embodiment, since only the low-refractive layer 620 is provided to the substrate 610, the low-refractive layer 620 may be formed on the substrate 610 in one chamber. Therefore, the process time of the window 600 may be reduced, and thus the productivity of the window 600 may be effectively improved and the manufacturing cost of the window 600 may be reduced.
[0138] In an embodiment, a layer including magnesium fluoride (MgF) may be formed on the substrate 610 by using an electron beam deposition apparatus. 2 ) of the low-refractive layer 620. As an example, the low-refractive layer 620 may be formed on the substrate 610 in one chamber by using an electron beam deposition device.
[0139] In an implementation, the first functional layer 630 may be disposed on the low-refractive layer 620. The first functional layer 630 may be directly disposed on the low-refractive layer 620.
[0140] In an embodiment, the first functional layer 630 may include a low refractive material. The first functional layer 630 may include an oxide. The first functional layer 630 may include at least one inorganic material of aluminum oxide, titanium oxide, tantalum oxide, hafnium oxide, zinc oxide, silicon oxide, silicon nitride, and silicon oxynitride. As an example, the first functional layer 630 may include silicon oxide (SiO 2 ) and / or aluminum oxide (Al 2 O 3 ).
[0141] Alternatively, the first functional layer 630 may include silicon aluminum oxide (Si x Al y O z ). In this case, x, y, and z may each be a natural number greater than 1. For example, x, y, and z may be 9, 2, and 10, respectively. That is, the first functional layer 630 may include silicon aluminum oxide (Si 9 Al 2 O 10 ). However, the embodiment is not limited thereto.
[0142] The first functional layer 630 may include silicon oxide in which aluminum atoms are employed. In this case, the first functional layer 630 may be provided as a substitutional solid solution in which some of the silicon atoms of the silicon oxide are replaced by aluminum atoms. In other words, the first functional layer 630 may include a substitutional solid solution in which some of the silicon atoms of the silicon oxide are replaced by aluminum atoms. Alternatively, the first functional layer 630 may be provided as a penetrating solid solution in which aluminum atoms penetrate the crystal lattice of silicon oxide. In other words, the first functional layer 630 may include a penetrating solid solution in which aluminum atoms penetrate the crystal lattice of silicon oxide.
[0143] Alternatively, the first functional layer 630 may include aluminum oxide in which silicon atoms are employed. In this case, the first functional layer 630 may be provided as a substitutional solid solution in which some of the aluminum atoms of the aluminum oxide are replaced by silicon atoms. In other words, the first functional layer 630 may include a substitutional solid solution in which some of the aluminum atoms of the aluminum oxide are replaced by silicon atoms. Alternatively, the first functional layer 630 may be provided as a penetrating solid solution in which silicon atoms penetrate the crystal lattice of the aluminum oxide. In other words, the first functional layer 630 may include a penetrating solid solution in which silicon atoms penetrate the crystal lattice of the aluminum oxide.
[0144] In an embodiment, in the case where the first functional layer 630 is provided as a substitutional solid solution, silicon atoms, aluminum atoms, and / or oxygen atoms may be chemically bonded to each other and exist within the first functional layer 630. Therefore, in the case where the first functional layer 630 is provided as a substitutional solid solution, when the first functional layer 630 is coated, the coating speed may be stable (or uniform), and a high-density first functional layer 630 may be formed.
[0145] In an embodiment, the first functional layer 630 may include silicon aluminum oxide (Si 9 Al 2 O 10 ), and silicon aluminum oxide (Si 9 Al 2 O 10 ) can be provided as a substitutional solid solution. In this case, silicon aluminum oxide (Si 9 Al 2 O 10 ) may have a cubic structure in which oxygen atoms, silicon atoms, and aluminum atoms are chemically combined. In addition, the content of aluminum atoms in the first functional layer 630 may be within about five percent (5%). As an example, silicon aluminum oxide (Si 9 Al 2 O 10 ) may contain aluminum atoms in an amount within about 5%.
[0146] In an embodiment, the first functional layer 630 may be made of silicon oxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) is a simple mixture of
[0147] In an embodiment, the refractive index n3 of the first functional layer 630 may be about 1.4 to about 1.6. Specifically, the refractive index n3 of the first functional layer 630 with respect to a wavelength of about 550 nm may be about 1.48.
[0148] In an embodiment, the thickness t2 of the first functional layer 630 may be 5nm to 25nm. Specifically, the thickness t2 of the first functional layer 630 may be about 15nm. The window 600 may include a substrate 610, a low-refractive layer 620, a first functional layer 630, and a second functional layer 640. The reflectivity of the window 600 may be reduced by adjusting the material, refractive index, and thickness of the layer. Therefore, in the case where the thickness t2 of the first functional layer 630 is less than 5nm or exceeds 25nm, the optical characteristics change, and the reflectivity of the window 600 including the first functional layer 630 may not be reduced. Therefore, in the case where the thickness t2 of the first functional layer 630 satisfies 5nm to 25nm, the reflectivity of the window 600 including the first functional layer 630 may be reduced.
[0149] In an embodiment, the second functional layer 640 may be disposed on the first functional layer 630. The second functional layer 640 may include a low refractive material. The second functional layer 640 may include a perfluorinated compound. As an example, the second functional layer 640 may include perfluoropolyether ("PFPE"). However, the embodiment is not limited thereto.
[0150] In an embodiment, the refractive index n4 of the second functional layer 640 may be about 1.2 to about 1.4. Specifically, the refractive index n4 of the second functional layer 640 with respect to a wavelength of about 550 nm may be about 1.32.
[0151] In an embodiment, the thickness t3 of the second functional layer 640 may be 5nm to 30nm. Specifically, the thickness t3 of the second functional layer 640 may be about 25nm. The second functional layer 640 is included to improve the wear resistance and / or alcohol resistance of the window 600. In the case where the thickness t3 of the second functional layer 640 is less than 5nm, the thickness t3 of the second functional layer 640 is too thin, and therefore, the wear resistance and / or alcohol resistance of the second functional layer 640 and / or the window 600 including the second functional layer 640 may deteriorate. In addition, when the thickness t3 of the second functional layer 640 is less than 5nm, the bonding force (adhesive force or attachment force) between the second functional layer 640 and the first functional layer 630 is small, and the second functional layer 640 may be peeled off from the first functional layer 630. On the contrary, when the thickness t3 of the second functional layer 640 exceeds 30nm, the thickness t3 of the second functional layer 640 is too thick, the uppermost layer of the second functional layer 640 may peel off, and the wear resistance and / or alcohol resistance of the second functional layer 640 and / or the window 600 including the second functional layer 640 may deteriorate.
[0152] In an embodiment, the low-refractive layer 620 may include magnesium fluoride (MgF 2 However, magnesium fluoride (MgF 2) has low bonding strength (adhesion or adhesion) with other materials. Therefore, the second functional layer 640 is directly disposed on the magnesium fluoride (MgF 2 ), the bonding force (adhesive force or adhesive force) between the low-refractive layer 620 and the second functional layer 640 is small, and the second functional layer 640 may be easily peeled off from the low-refractive layer 620.
[0153] In an embodiment, the window 600 may include a substrate 610, a low-refractive layer 620, a first functional layer 630, and a second functional layer 640. The reflectivity of the window 600 may be reduced by optical interference. By adjusting the thickness, refractive index, and material of the substrate 610, the low-refractive layer 620, the first functional layer 630, and the second functional layer 640, the light reflected by the plane between the layers destructively interferes with each other. Therefore, the reflectivity of the window 600 including the substrate 610, the low-refractive layer 620, the first functional layer 630, and the second functional layer 640 may be reduced. Specifically, two of the light reflected by the plane between the substrate 610 and the low-refractive layer 620, the light reflected by the plane between the low-refractive layer 620 and the first functional layer 630, the light reflected by the plane between the first functional layer 630 and the second functional layer 640, and the light reflected by the surface of the second functional layer 640 may destructively interfere with each other, and therefore, the reflection of the window 600 may be reduced.
[0154] In an embodiment, the first functional layer 630 may be disposed between the low-refractive layer 620 and the second functional layer 640. The first functional layer 630 may improve the bonding force (adhesive force or attachment force) between the low-refractive layer 620 and the second functional layer 640. That is, since the first functional layer 630 is disposed between the low-refractive layer 620 and the second functional layer 640, the adhesion between the low-refractive layer 620 and the second functional layer 640 is improved, and therefore, the second functional layer may be prevented or reduced from peeling off from the low-refractive layer 620.
[0155] In an embodiment, the sum of the thicknesses of the elements disposed on the substrate 610 may be about 60 nm to about 205 nm. Specifically, the sum (t1+t2+t3) of the thickness t1 of the low-refractive layer 620 disposed on the substrate 610, the thickness t2 of the first functional layer 630, and the thickness t3 of the second functional layer 640 may be about 60 nm to about 205 nm. Alternatively, the sum (t1+t2+t3) of the thickness t1 of the low-refractive layer 620 disposed on the substrate 610, the thickness t2 of the first functional layer 630, and the thickness t3 of the second functional layer 640 may be about 70 nm to about 135 nm.
[0156] Table 1
[0157]
[0158] Table 1 is a table showing the reflectivity and reflection color evaluation results of the window according to Embodiment 1 and Comparative Example. In Table 1, Embodiment 1 corresponds to the case where the window 600 includes a substrate 610, a low-refractive layer 620, a first functional layer 630 and a second functional layer 640. The substrate 610, the low-refractive layer 620, the first functional layer 630 and the second functional layer 640 respectively include glass, magnesium fluoride (MgF 2 ), silicon aluminum oxide (Si 9 Al 2 O 10 ) and perfluoropolyether (PFPE). In this case, silicon aluminum oxide (Si 9 Al 2 O 10 ) may include a substitutional solid solution. In addition, the comparative example corresponds to a case where the window 600 includes a substrate 610, a low-refractive layer 620, a first functional layer 630, and a second functional layer 640. The substrate 610, the low-refractive layer 620, the first functional layer 630, and the second functional layer 640 respectively include glass, magnesium fluoride (MgF 2 ), silicon oxide (SiO 2 ) and perfluoropolyether (PFPE). That is, the difference between Embodiment 1 and the comparative example is that the first functional layer 630 includes silicon aluminum oxide (Si 9 Al 2 O 10 ), while the comparative example includes silicon oxide (SiO 2 ). In addition, the elements of Embodiment 1 and Comparative Example can be provided as the above reference Figure 4 The refractive index and thickness described.
[0159] In Table 1, the reflectance means the reflectance measured in a mode including the specular component of SCI (SCI), and a* and b* respectively represent a* and b* in the L*a*b* color system of the light measured in a mode not including the specular component (SCE). When the reflectance of window 600 is 6.3% or less, it corresponds to a case that satisfies the required conditions. In addition, since a* of display panel 10 satisfies -2 < a* < 2, it is preferable that a* of window 600 has an equivalent level of the a* value. Therefore, when a* of window 600 has a value within the range of -2 < a* < 2, it corresponds to a case that satisfies the required conditions (SPEC IN). In addition, when a* of window 600 has a value deviating from the above range, it corresponds to a case that does not satisfy the required conditions (SPEC OUT). In addition, since b* of display panel 10 satisfies -1.5 < b* < 0.5, it is preferable that b* of window 600 also has an equivalent level of the b* value. Therefore, when b* of window 600 has a value within the range of -1.5 < b* < 0.5, it corresponds to a case that satisfies the required conditions (SPECIN). In addition, when b* of window 600 has a value deviating from the above range, it corresponds to a case that does not satisfy the required conditions (SPECOUT).
[0160] Referring to Table 1, both Embodiment 1 and the Comparative Example have a reflectance of 6.3% or less, and it can be determined that both Embodiment 1 and the Comparative Example have the required reflectance. In addition, the reflectance of Embodiment 1 is about 5.85%, and the reflectance of the Comparative Example is about 5.97%, and it can be determined that the reflectance of Embodiment 1 is less than that of the Comparative Example.
[0161] a* and b* of Embodiment 1 are 0.06 and -0.32 respectively, and it can be determined that a* and b* of Embodiment 1 respectively satisfy the required conditions. On the contrary, a* and b* of the Comparative Example are 0.27 and -2.25 respectively, and it can be determined that b* of the Comparative Example does not satisfy the required conditions. That is, it can be determined that both a* and b* of Embodiment 1 satisfy the required reflected color sense, but b* of the Comparative Example does not satisfy the required reflected sense.
[0162] Therefore, it can be determined that, compared with the case where the first functional layer 630 includes silicon oxide (SiO 2 ), the case where the first functional layer 630 includes silicon aluminoxide (Si 9 Al 2 O 10 ) having a substitutional solid solution structure has a lower reflectance and a reflected color sense that satisfy the required conditions.
[0163] Figure 5 is a diagram showing the abrasion resistance evaluation results of Embodiment 1. Figure 5is a diagram showing the results of measuring the contact angle of the surface of the window 600 of Embodiment 1 with respect to water before and after performing the wear resistance evaluation. Figure 5 In Table 1, abrasion resistance evaluation was performed, wherein: after applying a load of about 1 Kg to the surface of the window 600 of Embodiment 1 having the above structure using an eraser and reciprocating a distance of about 15 mm at a speed of about 40 cycles / minute for 5000 times and 10,000 times, the contact angle was measured. In this case, the protrusion amount of the eraser was 5 mm from the end of the fixture.
[0164] The surface of the window 600 treated with antifouling has hydrophobicity. In the case where the surface of the window 600 has hydrophobicity, the contact angle relative to water can be increased. However, the surface of the window 600 may be hydrophilized due to repeated external stress and / or strong impact. In the case where the surface of the window 600 is hydrophilized, the contact angle relative to water may be reduced. In this case, after the wear resistance evaluation, when the contact angle relative to water is 95° or more, this may indicate that the surface of the window 600 has well withstood external stress and impact. When the contact angle relative to water is less than 95°, this may indicate that the surface of the window 600 has not well withstood external stress and impact. Therefore, when the contact angle of the surface of the window 600 relative to water is 95° or more after 6,000 times of wear resistance evaluation, it corresponds to the case where the window 600 meets the required wear resistance (SPEC IN). When the contact angle of the surface of the window 600 relative to water is less than 95° after 6,000 times, it corresponds to the case where the window 600 does not meet the required wear resistance (SPEC OUT).
[0165] refer to Figure 5 , it can be determined that the contact angles of the surface of the window 600 with respect to water are 115.7°, 110.3°, and 104.7° before, after 5,000 times, and after 10,000 times of the wear resistance evaluation using the rubber, respectively. Therefore, since the contact angle of the surface of the window 600 with respect to water is 95° or more after 10,000 times of the wear resistance evaluation, it can be determined that the embodiment 1 has the desired wear resistance.
[0166] Figure 6 3 is a graph showing the results of the wear resistance evaluation of the first embodiment. Figure 6 is a diagram showing the results of measuring the contact angle of the surface of the window 600 of Embodiment 1 with respect to water before and after performing the wear resistance evaluation. Figure 6 In Table 1, a wear resistance evaluation was performed, wherein: after a load of about 1 Kg was applied to the surface of the window 600 of Embodiment 1 having the above structure using steel wool and reciprocated a distance of about 15 mm at a speed of about 40 cycles / min for 5000 times and 10,000 times, the contact angle was measured.
[0167] As mentioned above Figure 5 As described above, in the wear resistance evaluation using steel wool, when the contact angle of the surface of the window 600 with respect to water is 95° or more after 5,000 times of the wear resistance evaluation, it corresponds to the case where the window 600 satisfies the required wear resistance (SPEC IN). When the contact angle of the surface of the window 600 with respect to water is less than 95° after 5,000 times of the wear resistance evaluation, it corresponds to the case where the window 600 does not satisfy the required wear resistance (SPEC OUT).
[0168] refer to Figure 6 , it can be determined that the contact angles of the surface of the window 600 with respect to water are 115.7°, 106.5°, and 98°, respectively, before, after 5,000 times, and after 10,000 times of the wear resistance evaluation using steel wool. Therefore, since the contact angle of the surface of the window 600 with respect to water is 95° or more after 10,000 times of the wear resistance evaluation, it can be determined that Embodiment 1 has the wear resistance of the desired condition. In addition, since the contact angle of the surface of the window 600 with respect to water is about 106.5° after 5,000 times of the wear resistance evaluation, it can be determined that the contact angle of the surface of the window 600 with respect to water is 100° or more even in the case where the wear resistance evaluation is performed 5,000 times.
[0169] Figure 7 is a graph showing the results of wear resistance evaluation of comparative examples. Figure 7 is a graph showing the results of measuring the contact angle of the surface of the window 600 of the comparative example with respect to water before and after performing the wear resistance evaluation. Figure 7 In Table 1, abrasion resistance evaluation was performed, wherein: after applying a load of about 1 Kg to the surface of the window 600 of the comparative example having the above structure using an eraser and reciprocating a distance of about 20 mm at a speed of about 40 cycles / minute for 5000 times and 10,000 times, the contact angle was measured. In this case, the protrusion amount of the eraser was 5 mm from the end of the fixture.
[0170] As mentioned above Figure 5 As described above, in the abrasion resistance evaluation using a rubber, when the contact angle of the surface of the window 600 with respect to water is 95° or more after 6,000 times of the abrasion resistance evaluation, it corresponds to a case where the window 600 satisfies the required abrasion resistance (SPEC IN). When the contact angle of the surface of the window 600 with respect to water is less than 95° after 6,000 times of the abrasion resistance evaluation, it corresponds to a case where the window 600 does not satisfy the required abrasion resistance (SPEC OUT).
[0171] refer to Figure 7, it can be determined that the contact angles of the surface of the window 600 with respect to water are 116.8°, 89.4°, and 89.4°, respectively, before, after 5,000 times, and after 10,000 times of the wear resistance evaluation using the rubber. Therefore, since the contact angle of the surface of the window 600 with respect to water is less than 95° after 10,000 times of the wear resistance evaluation, it can be determined that the comparative example does not have the desired condition of wear resistance.
[0172] Figure 8 is a graph showing the results of wear resistance evaluation of comparative examples. Figure 8 is a graph showing the results of measuring the contact angle of the surface of the window 600 of the comparative example with respect to water before and after performing the wear resistance evaluation. Figure 8 In Table 1, a wear resistance evaluation was performed, wherein: after a load of about 1 Kg was applied to the surface of the window 600 of the comparative example having the above structure using steel wool and reciprocated a distance of about 20 mm at a speed of about 40 cycles / min for 5000 times and 10,000 times, the contact angle was measured.
[0173] As mentioned above Figure 5 As described above, in the wear resistance evaluation using steel wool, when the contact angle of the surface of the window 600 with respect to water is 95° or more after 5,000 times of the wear resistance evaluation, it corresponds to the case where the window 600 satisfies the required wear resistance (SPEC IN). When the contact angle of the surface of the window 600 with respect to water is less than 95° after 5,000 times of the wear resistance evaluation, it corresponds to the case where the window 600 does not satisfy the required wear resistance (SPEC OUT).
[0174] refer to Figure 8 , although the contact angle of the surface of the window 600 with respect to water was 116.8° before the wear resistance evaluation was performed, the contact angle of the surface of the window 600 with respect to water was not measured when the wear resistance evaluation was performed by using steel wool. Therefore, since the contact angle of the surface of the window 600 with respect to water was less than 95° after the wear resistance evaluation was performed 10,000 times, it can be determined that the comparative example does not have the required condition of wear resistance.
[0175] Therefore, it can be determined that the first functional layer 630 includes silicon oxide (SiO 2 ) compared to the case where the first functional layer 630 includes silicon aluminum oxide (Si 9 Al 2 O 10 ) has a higher level of wear resistance.
[0176] Fig. 9 is a schematic cross-sectional view of a window included in a display device according to an embodiment. Specifically, Fig. 9 The implementation method and Figure 4 The difference between the embodiments is that the window 600 further includes a third functional layer 650. Fig. 9 In, with Figure 4 The same reference numerals as in the accompanying drawings denote the same components, and thus, repeated descriptions thereof are omitted.
[0177] refer to Fig. 9 , the window 600 may include a substrate 610 , a low-refractive layer 620 , a first functional layer 630 , a second functional layer 640 , and a third functional layer 650 .
[0178] In an implementation, the third functional layer 650 may be disposed on the substrate 610, and the low-refractive layer 620 may be disposed on the third functional layer 650. That is, the third functional layer 650 may be disposed between the substrate 610 and the low-refractive layer 620.
[0179] In an embodiment, the third functional layer 650 may include an intermediate refractive material. The third functional layer 650 may include an oxide. The third functional layer 650 may include yttrium oxide (Y 2 O 3 ), magnesium oxide (MgO) and aluminum oxide (Al 2 O 3 As an example, the third functional layer 650 may include yttrium oxide (Y 2 O 3 ).
[0180] In an embodiment, the refractive index n5 of the third functional layer 650 may be about 1.6 to about 1.8. Specifically, the refractive index n5 of the third functional layer 650 with respect to a wavelength of about 550 nm may be about 1.66.
[0181] Since the third functional layer 650 having a refractive index n5 of about 1.6 to about 1.8 is disposed below the low refractive layer 620 having a refractive index n2 of about 1.2 to about 1.4, the reflectivity of the window 600 including the low refractive layer 620 and the third functional layer 650 can be further reduced by optical interference. Specifically, since the third functional layer 650 having a refractive index of about 1.66 (e.g., an intermediate refractive index) is disposed below the low refractive layer 620 having a refractive index of about 1.38 (e.g., a low refractive index), at least two of the light reflected by the plane (i.e., boundary surface) between the first functional layer 630 and the low refractive layer 620, the light reflected by the plane (i.e., boundary surface) between the low refractive layer 620 and the third functional layer 650, and the light reflected by the plane (i.e., boundary surface) between the third functional layer 650 and the substrate 610 destructively interfere with each other, and therefore, the reflectivity of the window 600 can be further reduced.
[0182] In an embodiment, the thickness t4 of the third functional layer 650 may be 5nm to 30nm. The window 600 may include a substrate 610, a third functional layer 650, a low refractive layer 620, a first functional layer 630, and a second functional layer 640. The reflectivity of the window 600 may be reduced by adjusting the material, refractive index, and thickness of the layer. In the case where the thickness t4 of the third functional layer 650 is less than 5nm or exceeds 30nm, the optical characteristics change, and the reflectivity of the window 600 including the third functional layer 650 may not be reduced. Therefore, in the case where the thickness t4 of the third functional layer 650 satisfies 5nm to 30nm, the reflectivity of the window 600 including the third functional layer 650 may be effectively reduced.
[0183] As mentioned above, magnesium fluoride (MgF 2 ) can be formed on the substrate 610 by using an electron beam deposition device (see Figure 4 ). In the case where the low-refractive layer 620 is formed on the substrate 610 at a temperature of about 200 degrees Celsius (°C) to about 300°C, the bonding force (adhesive force or attachment force) between the substrate 610 and the low-refractive layer 620 may be high. That is, as the layer formation temperature of the low-refractive layer 620 increases, the bonding force (adhesive force, attachment force) between the substrate 610 and the low-refractive layer 620 may increase. In the case where the low-refractive layer 620 is formed on the substrate 610 at a temperature of about 200°C to about 300°C, one cycle for forming the low-refractive layer 620 on the substrate 610 may take about 90 minutes. That is, in the case where the layer formation temperature of the low-refractive layer 620 is high, the process time required to form the layer of the low-refractive layer 620 may increase.
[0184] In addition, in the case where the low-refractive layer 620 is formed on the substrate 610 at a temperature of about 50°C to about 200°C, the bonding force (adhesive force or attachment force) between the substrate 610 and the low-refractive layer 620 may be low. That is, in the case where the low-refractive layer 620 is formed at low temperature, the bonding force (adhesive force, attachment force) between the substrate 610 and the low-refractive layer 620 may be low. However, in the case where the low-refractive layer 620 is formed on the substrate 610 at a temperature of about 50°C to about 200°C, one cycle may take about 60 minutes. That is, in the case where the layer formation temperature of the low-refractive layer 620 is low, the process time required to form the layer of the low-refractive layer 620 can be reduced.
[0185] In an embodiment, the third functional layer 650 may be disposed between the substrate 610 and the low-refractive layer 620. The third functional layer 650 may improve the bonding force (adhesive force or attachment force) between the substrate 610 and the low-refractive layer 620. That is, since the third functional layer 650 is disposed between the substrate 610 and the low-refractive layer 620, the adhesion between the substrate 610 and the low-refractive layer 620 is improved, and therefore, the peeling of the low-refractive layer 620 from the substrate 610 may be effectively prevented or reduced.
[0186] In an embodiment, since the third functional layer 650 is disposed between the substrate 610 and the low-refractive layer 620, the low-refractive layer 620 may be formed at a temperature of about 50° C. to about 200° C. That is, since the third functional layer 650 is disposed between the substrate 610 and the low-refractive layer 620, the magnesium fluoride (MgF 2 ) can be formed at a temperature of about 50°C to about 200°C. In this case, in the case where the layer formation temperature of the low-refractive layer 620 is less than 50°C, the layer formation temperature of the low-refractive layer 620 is too low and the adhesion of the low-refractive layer 620 may be too low. Therefore, the low-refractive layer 620 may be peeled off from the third functional layer 650. In addition, in the case where the layer formation temperature of the low-refractive layer 620 exceeds 200°C, the layer formation temperature of the low-refractive layer 620 is too high, and the process time may increase. Therefore, when the layer of the low-refractive layer 620 is formed at a temperature of about 50°C to about 200°C, the low-refractive layer 620 may have an appropriate level of adhesion, and at the same time, the process time may be reduced.
[0187] In an embodiment, in the magnesium fluoride (MgF 2 ) is formed into a layer at a temperature of about 50° C. to about 200° C., the formed magnesium fluoride (MgF 2 ) may have an amorphous or partially crystalline structure.
[0188] Table 2
[0189]
[0190] Table 2 is a table showing the reflectivity and reflection color evaluation results of the window according to Embodiment 2. In Table 2, Embodiment 2 corresponds to the case where the window 600 includes a substrate 610, a third functional layer 650, a low-refractive layer 620, a first functional layer 630, and a second functional layer 640. The substrate 610, the third functional layer 650, the low-refractive layer 620, the first functional layer 630, and the second functional layer 640 respectively include glass, yttrium oxide (Y 2 O 3 ), magnesium fluoride (MgF 2 ), silicon aluminum oxide (Si 9 Al 2 O10 ) and perfluoropolyether (PFPE). In this case, the silicon aluminum oxide (Si 9 Al 2 O 10 ) may include a substitutional solid solution. In addition, the element of Embodiment 2 may be provided with the refractive index and thickness described above with reference to Figure 4 and Fig. 9 .
[0191] As shown in Table 1, when the reflectance of the window 600 is 6.3% or less, this corresponds to a case where the required conditions are satisfied. In addition, a* of the window 600 has a value in the range of -2 < a* < 2, which corresponds to a case where the required conditions are satisfied (SPEC IN), and b* of the window 600 has a value in the range of -1.5 < b* < 0.5, which corresponds to a case where the required conditions are satisfied (SPEC IN).
[0192] Referring to Table 2, since Embodiment 2 has a reflectance of 6.3% or less, it can be determined that Embodiment 2 has the reflectance of the required conditions. The a* and b* of Embodiment 2 are -0.02 and -0.36, respectively. It is determined that the a* and b* of Embodiment 2 satisfy the required conditions, respectively.
[0193] Therefore, when the window 600 has the structure of Embodiment 2, it can be determined that the window 600 has the reflectance and reflection color sense of the required conditions.
[0194] Fig.10 is a graph showing the abrasion resistance evaluation results of Embodiment 2. Fig.10 is a graph showing the results of measuring the contact angle of the surface of the window 600 of Embodiment 2 with respect to water before and after performing the abrasion resistance evaluation. The abrasion resistance evaluation is performed on the surface of the window 600 of Embodiment 2 having the above structure in Table 2 under the same conditions as in Figure 5 .
[0195] Referring to Fig.10 , it can be determined that the contact angles of the surface of the window 600 with respect to water are 117.5°, 107.8°, and 103.6° before, after 5,000 times, and after 10,000 times of the abrasion resistance evaluation using a rubber, respectively. Therefore, since the contact angle of the surface of the window 600 with respect to water is 95° or more after 10,000 times of the abrasion resistance evaluation, it can be determined that Embodiment 2 has the abrasion resistance of the required conditions.
[0196] Fig.11 is a graph showing the abrasion resistance evaluation results of Embodiment 2. Fig.11 is a graph showing the results of measuring the contact angle of the surface of the window 600 of Embodiment 2 with respect to water before and after performing the abrasion resistance evaluation. Under the same conditions as in Figure 6 A wear resistance evaluation was performed on the surface of the window 600 of Embodiment 2 having the above structure in Table 2 under the same conditions as in FIG.
[0197] refer to Fig.11 , it can be determined that the contact angles of the surface of the window 600 with respect to water are 117.5°, 102.7°, and 99.7° before, after 5,000 times, and after 10,000 times of the wear resistance evaluation using steel wool, respectively. Therefore, since the contact angle of the surface of the window 600 with respect to water is 95° or more after 10,000 times of the wear resistance evaluation, it can be determined that Embodiment 2 has the desired wear resistance.
[0198] As above reference Figure 4 As described above, the window 600 may include a substrate 610, a low-refractive layer 620, a first functional layer 630, and a second functional layer 640. In this case, the low-refractive layer 620, the first functional layer 630, and the second functional layer 640 may be sequentially stacked on the substrate 610. In addition, the substrate 610, the low-refractive layer 620, the first functional layer 630, and the second functional layer 640 may include glass, magnesium fluoride (MgF 2 ), silicon aluminum oxide (Si 9 Al 2 O 10 ) and perfluoropolyether (PFPE).
[0199] As mentioned above, when magnesium fluoride (MgF 2 ) when the layer forming temperature of the low-refractive layer 620 is high, the bonding force (adhesive force or attachment force) between the substrate 610 and the low-refractive layer 620 may increase. However, when the layer forming temperature of the low-refractive layer 620 is high, the process time required for forming the layer of the low-refractive layer 620 may increase. In addition, when the low-refractive layer 620 is formed at low temperatures, the bonding force (adhesive force, attachment force) between the substrate 610 and the low-refractive layer 620 may be low.
[0200] In an embodiment, a magnesium fluoride (MgF)-containing 2 ) of the low-refractive layer 620. In the case of using IAD, when deposited particles of the low-refractive material are attached to the substrate 610, ionized argon, oxygen, etc. may collide together, increase the kinetic energy of the deposited particles, and increase the bonding force (adhesive force or attachment force) of the deposited layer.
[0201] In this case, a layer including magnesium fluoride (MgF 2) of the low-refractive layer 620. The reaction gas may include oxygen, nitrogen, etc., and the inert gas may include argon (Ar), helium (He), etc. As an example, an inert gas may be used as the inert gas. The reaction gas and the inert gas may activate the surface of the low-refractive layer 620, accelerate the surface oxidation of the low-refractive layer 620, or help the chemical stability of the low-refractive layer 620 without affecting the internal crystal structure of the low-refractive layer 620.
[0202] In an embodiment, the reaction gas may include oxygen (or oxygen ions), and the inert gas may include argon (or argon ions). In this case, the flow rate of oxygen (or oxygen ions) may be about 5 standard cubic centimeters per minute (sccm) to about 30 sccm, and the flow rate of argon (or argon ions) may be about 30 sccm to about 5 sccm. The low-refractive layer 620 formed by IAD may be formed as an amorphous and crystalline mixture. In addition, magnesium oxide (MgO) and / or argon atoms may be present in a portion of the low-refractive layer 620. Therefore, because magnesium oxide (MgO) and / or argon atoms fill the space inside the low-refractive layer 620, the density of the low-refractive layer 620 may be increased, and water molecules may be prevented or reduced from being absorbed into the low-refractive layer 620.
[0203] In an embodiment, the reaction gas may include nitrogen (or nitrogen ions), and the inert gas may include argon (or argon ions). In this case, the flow rate of nitrogen (or nitrogen ions) may be about 5 sccm to about 30 sccm, and the flow rate of argon (or argon ions) may be about 30 sccm to about 5 sccm. The low-refractive layer 620 formed by IAD may be formed as an amorphous and crystalline mixture. In addition, nitrogen atoms and / or argon atoms may be present in a portion of the low-refractive layer 620. Therefore, because nitrogen atoms and / or argon atoms fill the space inside the low-refractive layer 620, the density of the low-refractive layer 620 may be increased, and water molecules may be prevented or reduced from being absorbed into the low-refractive layer 620.
[0204] In an embodiment, the reaction gas may include oxygen (or oxygen ions), and the inert gas may include helium (or helium ions). In this case, the flow rate of oxygen (or oxygen ions) may be about 5 sccm to about 30 sccm, and the flow rate of helium (or helium ions) may be about 30 sccm to about 5 sccm. The low-refractive layer 620 formed by IAD may be formed as an amorphous and crystalline mixture. In addition, magnesium oxide (MgO) and / or helium atoms may be present in a portion of the low-refractive layer 620. Therefore, since magnesium oxide (MgO) and / or helium atoms fill the space inside the low-refractive layer 620, the density of the low-refractive layer 620 may be increased, and water molecules may be prevented or reduced from being absorbed into the low-refractive layer 620.
[0205] In an embodiment, a molten-liquid crystal including magnesium fluoride (MgF) may be formed by using IAD at a temperature of about 50° C. to about 200° C. 2 ) of the low-refractive layer 620. Therefore, the process time required to form the low-refractive layer 620 on the substrate 610 can be reduced.
[0206] In an embodiment, since a layer including magnesium fluoride (MgF 2 ), the bonding force (adhesive force or attachment force) between the substrate 610 and the low-refractive layer 620 can be improved even when a separate layer is not formed between the substrate 610 and the low-refractive layer 620. In addition, since a layer including magnesium fluoride (MgF 2 ), the low-refractive layer 620 can be formed at a low temperature (eg, a temperature of about 50° C. to about 200° C.). Therefore, the process time spent on manufacturing the window 600 can be reduced.
[0207] It should be understood that the embodiments described herein should be considered to be illustrative only and not for limiting purposes. The description of features or aspects within each embodiment should generally be considered to be applicable to other similar features or aspects in other embodiments. Although one or more embodiments have been described with reference to the accompanying drawings, it will be understood by those of ordinary skill in the art that various changes in form and detail may be made therein without departing from the spirit and scope defined by the appended claims.
Claims
1. A window, include: substrate; a low-refractive layer disposed on the substrate and comprising a metal fluoride; a first functional layer disposed on the low refractive layer, having a thickness of 5 nm to 25 nm and including an oxide; and The second functional layer is disposed on the first functional layer and includes a perfluorinated compound.
2. The window according to claim 1, in, The low-refractive layer includes magnesium fluoride.
3. The window according to claim 1, in, The low-refractive layer has a refractive index of about 1.2 to about 1.
4.
4. The window according to claim 1, in, The low refractive layer has a thickness of 50 nanometers (nm) to 150 nm.
5. The window according to claim 1, in, The low-refractive layer has a crystalline structure.
6. The window according to claim 1, in, The first functional layer includes silicon aluminum oxide.
7. The window according to claim 1, in, The first functional layer includes silicon oxide incorporating aluminum atoms.
8. The window according to claim 7, in, The first functional layer includes a substitutional solid solution in which some of silicon atoms of the silicon oxide are substituted with the aluminum atoms.
9. The window according to claim 7, in, The first functional layer includes a penetrating solid solution in which the aluminum atoms penetrate through a crystal lattice of the silicon oxide.
10. The window according to claim 1, in, The first functional layer includes aluminum oxide using silicon atoms.
11. The window according to claim 10, in, The first functional layer includes a substitutional solid solution in which some of aluminum atoms of the aluminum oxide are substituted with the silicon atoms.
12. The window according to claim 1, in, The first functional layer has a refractive index of about 1.4 to about 1.
6.
13. The window according to claim 1, in, The second functional layer has a thickness of 5 nm to 30 nm.
14. The window according to claim 1, further comprising a third functional layer disposed between the substrate and the low-refractive layer and comprising an oxide.
15. The window according to claim 14, in, The third functional layer includes one of yttrium oxide, magnesium oxide and aluminum oxide.
16. The window according to claim 14, in, The refractive index of the third functional layer is greater than the refractive index of the low-refractive layer.
17. The window according to claim 16, in, The third functional layer has a refractive index of about 1.6 to about 1.
8.
18. The window according to claim 14, in, The third functional layer has a thickness of 5 nm to 30 nm.
19. The window according to claim 1, in, After a load of 1 Kg was applied to the surface of the window using a rubber and reciprocated a distance of 15 millimeters (mm) 6000 times at a speed of 40 cycles per minute (cycles / min), the contact angle of the surface of the window with respect to water was 95 degrees (°) or greater.
20. A display device, include: Display panel; as well as A window is provided on the display panel, Wherein, the display panel comprises: Display substrate; a light emitting element, disposed above the display substrate; and a filter layer disposed on the light emitting element and comprising a color filter layer and a light blocking layer, and Wherein, the window comprises: substrate; a low-refractive layer disposed on the substrate and comprising a metal fluoride; a first functional layer disposed on the low refractive layer, having a thickness of 5 nm to 25 nm and including an oxide; and The second functional layer is disposed on the first functional layer and includes a perfluorinated compound.
21. The display device according to claim 20, in, The light emitting element includes a pixel electrode, an emission layer and a counter electrode, and The display device further includes a pixel defining layer defining a first opening exposing at least a portion of the pixel electrode.
22. The display device according to claim 21, in, A second opening is defined in the light blocking layer, wherein the second opening overlaps the first opening.
23. The display device according to claim 22, in, At least a portion of the color filter layer is located within the second opening.
24. The display device according to claim 20, in, The low-refractive layer includes magnesium fluoride, has a refractive index of about 1.2 to about 1.4, and has a thickness of 50 nm to 150 nm.
25. The display device according to claim 20, in, The first functional layer includes silicon aluminum oxide.
26. The display device according to claim 20, in, The first functional layer includes silicon oxide incorporating aluminum atoms.
27. The display device according to claim 26, in, The first functional layer includes a substitutional solid solution in which some of the silicon atoms of the silicon oxide are replaced by the aluminum atoms or a penetrating solid solution in which the aluminum atoms penetrate through a crystal lattice of the silicon oxide. 28 . The display device according to claim 20 , further comprising a third functional layer disposed between the substrate and the low-refractive layer and comprising an oxide.
29. The display device according to claim 28, in, The refractive index of the third functional layer is greater than the refractive index of the low-refractive layer.
30. The display device according to claim 20, in, After a load of 1 Kg was applied to the surface of the window using a rubber and reciprocated a distance of 15 mm at a speed of 40 cycles / min 6000 times, the contact angle of the surface of the window with respect to water was 95° or more.