Adsorbent for purifying tetramethylsilane, preparation method thereof and purification device
By preparing the adsorbent for tetramethylsilane purification, the problems of difficulty and energy consumption in tetramethylsilane in the prior art are solved, and efficient isopentane separation and Purification reduces energy consumption.
Patent Information
- Application Number
- CN202411121555.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art is difficult and consumes energy when isolantane contained in tetramethylsilane, resulting in low separation efficiency.
A tetramethylsilane purification adsorbent is prepared by mixing seed crystals, silicon sources, iron sources, copper sources, structure guide agents and crystal form control agents, and then grinding, crystallization treatment and calcining. The adsorbent of isopentane is realized at normal pressure of 35 to 40°C.
It realizes efficient separation and purification of isopentane in tetramethylsilane, reduces energy consumption, and has good adsorption effect without heating and distillation.
Smart Images

Figure CN119016023A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of adsorbents, and in particular relates to an adsorbent for purifying tetramethylsilane, a preparation method thereof and a purification device. Background Art
[0002] Tetramethylsilane (TMS) is an important organic silicon material, which is widely used in the fields of medicine, aerospace construction and mechanical materials. TMS can be used as a precursor for chemical vapor deposition (CVD) or plasma enhanced chemical vapor deposition (PECVD) in the electronics industry to prepare high-quality silicon carbide films. TMS is a precursor material for low dielectric constant film deposition in the process of very large-scale integrated circuits. It is an emerging material in the market and is mainly used in the process of integrated circuit copper chips below 90nm as an etching barrier and copper barrier.
[0003] At present, the main methods for producing TMS are organosilicon conversion method and organosilicon low-boiling separation method. The organosilicon low-boiling separation method refers to the separation of TMS from low-boiling residues obtained from industrial production. For example, a large amount of low-boiling residues will be produced during the industrial production of methylchlorosilane, and the low-boiling residues contain both TMS and isopentane. Since the boiling points of TMS and isopentane are similar, it is difficult and energy-consuming to separate isopentane from TMS raw materials by distillation.
[0004] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0005] The object of the present invention is to provide an adsorbent for purifying tetramethylsilane, a preparation method thereof and a purification device. The adsorbent for purifying tetramethylsilane can specifically adsorb isopentane contained in tetramethylsilane and can effectively separate and purify tetramethylsilane.
[0006] In order to achieve the above object, a technical solution provided by a specific embodiment of the present invention is as follows:
[0007] A method for preparing an adsorbent for purifying tetramethylsilane comprises the following steps:
[0008] S1, mixing seed crystals, silicon source, iron source, copper source, structure directing agent, and crystal shape controlling agent to obtain a mixed material;
[0009] S2, grinding the mixed material;
[0010] S3, adding a cation source to the ground mixture, crystallizing, filtering, and calcining to obtain an adsorbent for purifying tetramethylsilane;
[0011] The molar ratio of the iron source to the copper source is 1:(0.03-0.7) based on iron-copper atoms.
[0012] In one or more embodiments of the present invention, the crystal shape controlling agent is urea, and the molar ratio of the iron source to urea is 1:(0.1-0.7) based on iron atom to urea.
[0013] In one or more embodiments of the present invention, the molar ratio of the iron source to urea is 1:(0.3-0.7) calculated as iron atom to urea.
[0014] In one or more embodiments of the present invention, the silicon source is selected from one or more of silica sol, silicon dioxide and tetraethyl orthosilicate; and / or,
[0015] The iron source is selected from one or both of ferric nitrate nonahydrate and ferric acetate; and / or,
[0016] The copper source is selected from one or more of copper nitrate nonahydrate, copper nitrate trihydrate and copper acetate; and / or,
[0017] The structure directing agent is selected from one or more of tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, tetramethylammonium hydroxide, triethylamine and n-propylamine; and / or,
[0018] The molar ratio of the silicon source, the iron source and the structure directing agent is (49-51):1:(2.2-2.7) based on silicon atoms, iron atoms and structure directing agent; and / or,
[0019] The cation source is ammonia water with a concentration of 22-25 wt %, and the mass ratio of the silicon source to ammonia water is 1:(0.5-0.7).
[0020] In one or more embodiments of the present invention, the seed crystal is a ZSM-5 molecular sieve loaded with iron and copper, and the mass ratio of the seed crystal to the silicon source is (0.8-1.2):20.
[0021] In one or more embodiments of the present invention, in step S2, the mixed material is ground to a particle size of 170 mesh to 200 mesh.
[0022] In one or more embodiments of the present invention, in step S3, the crystallization treatment temperature is 150-200° C. and the time is 20-26 hours; and / or,
[0023] In step S3, the calcination temperature is 500-600° C. and the calcination time is 3-5 hours.
[0024] In one or more embodiments of the present invention, a regeneration process is also included: the used adsorbent is kept at 250-350° C. for 1.5-2.5 hours, cooled to room temperature, and the regeneration process is completed.
[0025] Another specific embodiment of the present invention provides a technical solution as follows:
[0026] An adsorbent for purifying tetramethylsilane is prepared by adopting the preparation method of the adsorbent for purifying tetramethylsilane.
[0027] Another specific embodiment of the present invention provides a technical solution as follows:
[0028] A purification device includes a separation body, wherein the separation body includes a cavity for carrying an adsorbent, and the cavity is connected to an air inlet for receiving cavity raw gas and an air outlet for discharging purified gas after passing through the adsorbent; wherein the adsorbent is prepared by the above-mentioned preparation method of the adsorbent for purifying tetramethylsilane.
[0029] Compared with the prior art, the adsorbent for purifying tetramethylsilane prepared by the present invention can effectively adsorb isopentane in the tetramethylsilane raw material with a similar boiling point and difficult to separate by distillation at 35-40° C. under normal pressure, without the need for temperature-raising distillation, thus reducing energy consumption and achieving good adsorption effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] Figure 1 The figure is a flow chart of a method for preparing an adsorbent for purifying tetramethylsilane according to an embodiment of the present invention. DETAILED DESCRIPTION
[0032] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0033] like Figure 1 As shown, a specific embodiment of the present invention provides a method for preparing an adsorbent for purifying tetramethylsilane, comprising steps 1-3.
[0034] Step 1, mixing seed crystals, silicon source, iron source, copper source, structure directing agent, and crystal shape controlling agent to obtain a mixed material.
[0035] Specifically, in step 1, the seed crystal is a ZSM-5 molecular sieve loaded with iron and copper, and the mass ratio of the seed crystal to the silicon source is (0.8-1.2): 20. Specifically, adding the seed crystal is conducive to the nucleation and growth of the crystal, and selecting the same type of ZSM-5 molecular sieve loaded with iron and copper as the target adsorbent is helpful to obtain the target adsorbent, and can ensure that the obtained adsorbent has a good crystal shape and uniformly distributed particle size.
[0036] The iron source is selected from one or both of ferric nitrate nonahydrate and ferric acetate; the copper source is selected from one or more of copper nitrate nonahydrate, copper nitrate trihydrate and copper acetate; the structure directing agent is selected from one or more of tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, tetramethylammonium hydroxide, triethylamine and n-propylamine. The molar ratio of the silicon source, the iron source and the structure directing agent is (49-51) : 1 : (2.2-2.7) based on silicon atoms, iron atoms and structure directing agent; the molar ratio of the iron source and the copper source is 1 : (0.1-0.7) based on iron and copper atoms. Through the usage ratio of the silicon source, the iron source, the copper source and the structure directing agent, the prepared adsorbent can specifically adsorb isopentane in the TMS raw material, thereby achieving the purpose of effectively separating and purifying TMS.
[0037] Furthermore, the crystal shape controlling agent is urea, and the molar ratio of the iron source to urea is 1:(0.1-0.7) based on the iron atom and the urea. Adding a specific proportion of urea can effectively adjust the crystal shape of the adsorbent, reduce crystal defects, and significantly enhance the adsorption performance of the adsorbent.
[0038] Step 2, grinding the mixed material.
[0039] Specifically, the mixed material is ground to a particle size of 170-200 meshes. The particle size of the raw material will affect the crystal growth. By controlling the particle size of the raw material, an adsorbent with a suitable particle size can be prepared so that the adsorbent can effectively adsorb isopentane.
[0040] Step 3, adding a cation source to the ground mixture, performing crystallization treatment, filtering, and calcining to obtain an adsorbent for purifying tetramethylsilane.
[0041] Specifically, in step 3, the cation source is ammonia water with a concentration of 22 to 25 wt%, and the mass ratio of the silicon source to ammonia water is 1:(0.5 to 0.7). The crystallization treatment temperature is 150 to 200°C, the time is 20 to 26 hours, and the calcination temperature is 500 to 600°C, and the time is 3 to 5 hours. By controlling the crystallization temperature and time, an adsorbent with uniform morphology and microporous structure can be prepared; the calcination temperature and time will affect the crystallinity and microporous structure of the adsorbent. By controlling the calcination temperature and time, the crystallinity and the number of micropores of the adsorbent can be increased, thereby further ensuring the specificity of the adsorbent in adsorbing isopentane.
[0042] Furthermore, the used adsorbent can be regenerated, specifically, the used adsorbent is kept at 250-350°C for 1.5-2.5 hours, cooled to room temperature, and regenerated. Specifically, the material in the adsorption column is emptied, the adsorption column is evacuated, and the temperature of the adsorption column is simultaneously raised, and after reaching 300°C, it is kept for 2 hours, and then cooled to room temperature to complete the adsorbent regeneration.
[0043] Another specific embodiment of the present invention provides an adsorbent for purifying tetramethylsilane, which is prepared by the above-mentioned method for preparing the adsorbent for purifying tetramethylsilane.
[0044] Another specific embodiment of the present invention provides a purification device, including a separation body, the separation body includes a cavity for carrying an adsorbent, the cavity is connected to provide an air inlet for receiving cavity raw gas and an air outlet for discharging purified gas after passing through the adsorbent; wherein the adsorbent is prepared by the above-mentioned preparation method of the adsorbent for purifying tetramethylsilane.
[0045] Specifically, the adsorbent for purifying tetramethylsilane can specifically adsorb isopentane contained in the raw material, so as to achieve the purpose of efficiently separating tetramethylsilane and isopentane. The adsorbent can be loaded into the cavity in the form of particles or powder, or can be stacked in the cavity in the form of blocks.
[0046] The present invention is further described in detail below in conjunction with specific embodiments.
[0047] Seed preparation
[0048] Take 20g of silica powder, 2.69g of Fe(NO3)3·9H2O, 0.16g of Cu(NO3)2·9H2O, 3.38g of tetramethylammonium hydroxide and 0.12g of urea, mix them, ball mill for 4h to get a 200-mesh mixture, add 11.98g of 25wt% ammonia water to the mixture, and then crystallize it in a hydrothermal autoclave for 24h at a crystallization temperature of 180°C. After crystallization, filter it and calcine it at 550°C for 4h to get ZSM-5 molecular sieve seeds loaded with iron and copper.
[0049] Example 1
[0050] The adsorbent for purifying tetramethylsilane is prepared as follows:
[0051] Take 1g of ZSM-5 molecular sieve seed loaded with iron and copper, 20g of silicon dioxide powder, 2.69g of Fe(NO3)3·9H2O, 0.16g of Cu(NO3)2·9H2O, 3.38g of tetramethylammonium hydroxide and 0.12g of urea, mix well to obtain a mixture, ball mill the mixture for 4h, and the particle size of the mixture after ball milling is 200 mesh. Add 11.98g of 25wt% ammonia water to the ball milled mixture, then add the material to a hydrothermal autoclave and crystallize at 180℃ for 24h. After crystallization, filter and calcine at 550℃ for 4h to obtain an adsorbent for purifying tetramethylsilane.
[0052] Example 2
[0053] The adsorbent for purifying tetramethylsilane is prepared as follows:
[0054] Take 1g of ZSM-5 molecular sieve seed loaded with iron and copper, 20g of silicon dioxide powder, 2.69g of Fe(NO3)3·9H2O, 0.48g of Cu(NO3)2·9H2O, 3.38g of tetramethylammonium hydroxide and 0.12g of urea, mix them well to obtain a mixture, and ball mill the mixture for 4h. The particle size of the mixture after ball milling is 200 mesh. Add 11.98g of 25wt% ammonia water to the ball milled mixture, and then add the material to a hydrothermal autoclave and crystallize at 180℃ for 24h. After crystallization, filter it and calcine it at 550℃ for 4h to obtain an adsorbent for purifying tetramethylsilane.
[0055] Example 3
[0056] The adsorbent for purifying tetramethylsilane is prepared as follows:
[0057] Take 1g of ZSM-5 molecular sieve seed loaded with iron and copper, 20g of silicon dioxide powder, 2.69g of Fe(NO3)3·9H2O, 0.80g of Cu(NO3)2·9H2O, 3.38g of tetramethylammonium hydroxide and 0.12g of urea, mix well to obtain a mixture, ball mill the mixture for 4h, and the particle size of the mixture after ball milling is 200 mesh. Add 11.98g of 25wt% ammonia water to the ball milled mixture, then add the material to a hydrothermal autoclave and crystallize at 180℃ for 24h. After crystallization, filter and calcine at 550℃ for 4h to obtain an adsorbent for purifying tetramethylsilane.
[0058] Example 4
[0059] The adsorbent for purifying tetramethylsilane is prepared as follows:
[0060] Take 1g of ZSM-5 molecular sieve seed loaded with iron and copper, 20g of silica powder, 2.69g of Fe(NO3)3·9H2O, 1.13g of Cu(NO3)2·9H2O, 3.38g of tetramethylammonium hydroxide and 0.12g of urea, mix well to obtain a mixture, ball mill the mixture for 4h, and the particle size of the mixture after ball milling is 200 mesh. Add 11.98g of 25wt% ammonia water to the ball milled mixture, then add the material to a hydrothermal autoclave and crystallize at 180℃ for 24h. After crystallization, filter and calcine at 550℃ for 4h to obtain an adsorbent for purifying tetramethylsilane.
[0061] Example 5
[0062] The adsorbent for purifying tetramethylsilane is prepared as follows:
[0063] Take 1g of ZSM-5 molecular sieve seed loaded with iron and copper, 20g of silicon dioxide powder, 2.69g of Fe(NO3)3·9H2O, 1.60g of Cu(NO3)2·9H2O, 3.38g of tetramethylammonium hydroxide and 0.12g of urea, mix them well to obtain a mixture, ball mill the mixture for 4h, and the particle size of the mixture after ball milling is 200 mesh. Add 11.98g of 25wt% ammonia water to the ball milled mixture, then add the material to a hydrothermal autoclave and crystallize at 180℃ for 24h. After crystallization, filter and calcine at 550℃ for 4h to obtain an adsorbent for purifying tetramethylsilane.
[0064] Example 6
[0065] The adsorbent for purifying tetramethylsilane is prepared as follows:
[0066] Take 1g of ZSM-5 molecular sieve seed loaded with iron and copper, 20g of silicon dioxide powder, 2.69g of Fe(NO3)3·9H2O, 0.07g of Cu(NO3)2·9H2O, 3.38g of tetramethylammonium hydroxide and 0.12g of urea, mix well to obtain a mixture, ball mill the mixture for 4h, and the particle size of the mixture after ball milling is 200 mesh. Add 11.98g of 25wt% ammonia water to the ball milled mixture, then add the material to a hydrothermal autoclave and crystallize at 180℃ for 24h. After crystallization, filter and calcine at 550℃ for 4h to obtain an adsorbent for purifying tetramethylsilane.
[0067] Example 7
[0068] The adsorbent for purifying tetramethylsilane is prepared as follows:
[0069] Take 1g of ZSM-5 molecular sieve seed loaded with iron and copper, 20g of silicon dioxide powder, 2.69g of Fe(NO3)3·9H2O, 0.48g of Cu(NO3)2·9H2O, 3.38g of tetramethylammonium hydroxide and 0.04g of urea, mix them well to obtain a mixture, and ball mill the mixture for 4h. The particle size of the mixture after ball milling is 200 mesh. Add 11.98g of 25wt% ammonia water to the ball milled mixture, and then add the material to a hydrothermal autoclave and crystallize at 180℃ for 24h. After crystallization, filter it and calcine it at 550℃ for 4h to obtain an adsorbent for purifying tetramethylsilane.
[0070] Example 8
[0071] The adsorbent for purifying tetramethylsilane is prepared as follows:
[0072] Take 1g of ZSM-5 molecular sieve seed loaded with iron and copper, 20g of silicon dioxide powder, 2.69g of Fe(NO3)3·9H2O, 0.48g of Cu(NO3)2·9H2O, 3.38g of tetramethylammonium hydroxide and 0.20g of urea, mix well to obtain a mixture, ball mill the mixture for 4h, and the particle size of the mixture after ball milling is 200 mesh. Add 11.98g of 25wt% ammonia water to the ball milled mixture, then add the material to a hydrothermal autoclave and crystallize at 180℃ for 24h. After crystallization, filter and calcine at 550℃ for 4h to obtain an adsorbent for purifying tetramethylsilane.
[0073] Example 9
[0074] The adsorbent for purifying tetramethylsilane is prepared as follows:
[0075] Take 1g of ZSM-5 molecular sieve seed loaded with iron and copper, 20g of silicon dioxide powder, 2.69g of Fe(NO3)3·9H2O, 0.48g of Cu(NO3)2·9H2O, 3.38g of tetramethylammonium hydroxide and 0.28g of urea, mix them well to obtain a mixture, and ball mill the mixture for 4h. The particle size of the mixture after ball milling is 200 mesh. Add 11.98g of 25wt% ammonia water to the ball milled mixture, then add the material to a hydrothermal autoclave and crystallize at 180℃ for 24h. After crystallization, filter it and calcine it at 550℃ for 4h to obtain an adsorbent for purifying tetramethylsilane.
[0076] Comparative Example 1
[0077] The adsorbent for purifying tetramethylsilane is prepared as follows:
[0078] Take 1g of ZSM-5 molecular sieve seed loaded with iron and copper, 20g of silica powder, 2.69g of Fe(NO3)3·9H2O, 3.38g of tetramethylammonium hydroxide and 0.12g of urea, mix well to obtain a mixture, ball mill the mixture for 4h, and the particle size of the mixture after ball milling is 200 mesh. Add 11.98g of 25wt% ammonia water to the ball milled mixture, then add the material to a hydrothermal kettle and crystallize at 180℃ for 24h. After crystallization, filter and calcine at 550℃ for 4h to obtain an adsorbent for purifying tetramethylsilane.
[0079] Comparative Example 2
[0080] The adsorbent for purifying tetramethylsilane is prepared as follows:
[0081] Take 1g of ZSM-5 molecular sieve seed loaded with iron and copper, 20g of silicon dioxide powder, 0.16g of Cu(NO3)2·9H2O, 3.38g of tetramethylammonium hydroxide and 0.12g of urea, mix them well to obtain a mixture, and ball mill the mixture for 4h. The particle size of the mixture after ball milling is 200 mesh. Add 11.98g of 25wt% ammonia water to the ball milled mixture, and then add the material to a hydrothermal kettle and crystallize at 180℃ for 24h. After crystallization, filter it and calcine it at 550℃ for 4h to obtain an adsorbent for purifying tetramethylsilane.
[0082] Comparative Example 3
[0083] The adsorbent for purifying tetramethylsilane is prepared as follows:
[0084] Take 1g of ZSM-5 molecular sieve seed loaded with iron and copper, 20g of silicon dioxide powder, 2.69g of Fe(NO3)3·9H2O, 3.49g of Cu(NO3)2·9H2O, 3.38g of tetramethylammonium hydroxide and 0.12g of urea, mix well to obtain a mixture, ball mill the mixture for 4h, and the particle size of the mixture after ball milling is 200 mesh. Add 11.98g of 25wt% ammonia water to the ball milled mixture, then add the material to a hydrothermal autoclave and crystallize at 180℃ for 24h. After crystallization, filter and calcine at 550℃ for 4h to obtain an adsorbent for purifying tetramethylsilane.
[0085] Comparative Example 4
[0086] The adsorbent for purifying tetramethylsilane is prepared as follows:
[0087] Take 1g of ZSM-5 molecular sieve seed loaded with iron and copper, 20g of silicon dioxide powder, 2.69g of Fe(NO3)3·9H2O, 0.16g of Cu(NO3)2·9H2O and 3.38g of tetramethylammonium hydroxide, mix them well to obtain a mixture, and ball mill the mixture for 4h. The particle size of the mixture after ball milling is 200 mesh. Add 11.98g of 25wt% ammonia water to the ball milled mixture, and then add the material to a hydrothermal autoclave and crystallize at 180℃ for 24h. After crystallization, filter it and calcine it at 550℃ for 4h to obtain an adsorbent for purifying tetramethylsilane.
[0088] The adsorbent prepared above was tested: 80% tetramethylsilane and 20% isopentane were used as raw materials for adsorption test. The raw materials became gaseous after passing through a 40°C vaporizer. The gas flow rate was 6L / h. The gas was passed into an adsorption column with an inner diameter of 2.3cm and a length of 70cm. The adsorption column contained 0.29L of adsorbent and the air velocity was 21h -1 During the test, samples were taken and analyzed every 20 minutes to confirm the isopentane content after the adsorption column. When the isopentane content exceeded 10 ppm, it was considered as breakthrough. The test results are shown in Table 1.
[0089] Table 1 Adsorbent test results
[0090]
[0091]
[0092] It can be seen from Table 1 that the amount of isopentane adsorbed by the adsorbent in Comparative Examples 1-2 is much smaller than that in Example 1, and the penetration time is greatly shortened, indicating that the removal of the iron source or the copper source will reduce the specific adsorption of isopentane by the adsorbent; at the same time, in combination with Examples 2 to 6 and Comparative Example 3, the addition of the copper source and the iron source in the molar ratio disclosed in the present invention can effectively ensure the specific adsorption of isopentane by the adsorbent, and it can also be seen from the amount of isopentane adsorbed by the adsorbent per unit weight that the adsorbent prepared by the present invention has a high adsorption efficiency for isopentane.
[0093] Comparison of Example 1 and Comparative Example 4 shows that adding urea as a crystal shape control agent can improve the adsorption performance of the adsorbent for isopentane. At the same time, combined with Examples 7-9, it can be seen that in the dosage disclosed in the present invention, the iron source and urea are preferably added in a molar ratio of 1: (0.3-0.7), which can better ensure that the adsorbent has a higher adsorption performance.
[0094] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0095] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for preparing an adsorbent for purifying tetramethylsilane, It is characterized in that The steps include: S1, mixing seed crystals, silicon source, iron source, copper source, structure directing agent, and crystal shape controlling agent to obtain a mixed material; S2, grinding the mixed material; S3, adding a cation source to the ground mixture, crystallizing, filtering, and calcining to obtain an adsorbent for purifying tetramethylsilane; The molar ratio of the iron source to the copper source is 1:(0.03-0.7) based on iron-copper atoms.
2. The method for preparing the adsorbent for purifying tetramethylsilane according to claim 1, It is characterized in that The crystal shape controlling agent is urea, and the molar ratio of the iron source to urea is 1:(0.1-0.7) based on iron atom to urea.
3. The method for preparing the adsorbent for purifying tetramethylsilane according to claim 2, It is characterized in that The molar ratio of the iron source to urea is 1:(0.3-0.7) based on iron atom to urea.
4. The method for preparing the adsorbent for purifying tetramethylsilane according to claim 1, It is characterized in that The silicon source is selected from one or more of silica sol, silicon dioxide and tetraethyl orthosilicate; and / or, The iron source is selected from one or both of ferric nitrate nonahydrate and ferric acetate; and / or, The copper source is selected from one or more of copper nitrate nonahydrate, copper nitrate trihydrate and copper acetate; and / or, The structure directing agent is selected from one or more of tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, tetramethylammonium hydroxide, triethylamine and n-propylamine; and / or, The molar ratio of the silicon source, the iron source and the structure directing agent is (49-51):1:(2.2-2.7) based on silicon atoms, iron atoms and structure directing agent; and / or, The cation source is ammonia water with a concentration of 22-25 wt %, and the mass ratio of the silicon source to ammonia water is 1:(0.5-0.7).
5. The method for preparing the adsorbent for purifying tetramethylsilane according to claim 1, It is characterized in that The seed crystal is a ZSM-5 molecular sieve loaded with iron and copper, and the mass ratio of the seed crystal to the silicon source is (0.8-1.2):
20.
6. The method for preparing the adsorbent for purifying tetramethylsilane according to claim 1, It is characterized in that In step S2, the mixed material is ground to a particle size of 170 mesh to 200 mesh.
7. The method for preparing the adsorbent for purifying tetramethylsilane according to claim 1, It is characterized in that In step S3, the crystallization treatment temperature is 150-200° C. and the time is 20-26 hours; and / or, In step S3, the calcination temperature is 500-600° C. and the calcination time is 3-5 hours.
8. The method for preparing the adsorbent for purifying tetramethylsilane according to claim 1, It is characterized in that It also includes a regeneration process: the used adsorbent is kept at 250-350°C for 1.5-2.5 hours, then cooled to room temperature to complete the regeneration process.
9. An adsorbent for purifying tetramethylsilane, It is characterized in that The tetramethylsilane purifying adsorbent is prepared by the preparation method of the adsorbent for purifying tetramethylsilane according to any one of claims 1 to 8.
10. A purification device, It is characterized in that The separation body comprises a cavity for carrying an adsorbent, wherein the cavity is provided with an air inlet for receiving cavity raw gas and an air outlet for discharging purified gas after passing through the adsorbent; Wherein, the adsorbent is prepared by the preparation method of the adsorbent for purifying tetramethylsilane according to any one of claims 1 to 8.