Method for increasing yield of fine-fraction titanium concentrate
By adopting multi-stage magnetic separation and grading processes in the process of vanadium titanium magnetite, the grinding parameters are optimized, the problem of low titanium resource utilization is solved, the yield and grade of fine-grained titanium concentrate is improved, and energy saving is achieved Emission reduction and economic benefits improvement.
Patent Information
- Application Number
- CN202411408993.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-11-26
AI Technical Summary
The utilization rate of vanadium titanium magnetite in Panxi is low, especially the recovery rate of titanium resources, which leads to waste of resources. The existing technology is difficult to meet the fine-grain titanium concentrate in the case of low influx grade and low recovery rate. Insufficient production.
The process flow of one-stage weak magnetic separation, strong magnetic separation, cyclone classification, ball milling and re-grinding, high-frequency vibration screen classification, deferromagnetic separation, two-stage strong magnetic separation and fine particle flotation is adopted to optimize the grinding graded parameters. and equipment configuration to improve the fine-grain yield and grade of titanium concentrate.
It significantly improves the yield and grade of fine-grained titanium concentrate, improves the recovery rate of titanium concentrate, reduces energy consumption and equipment load, improves economic benefits, and achieves more full utilization of resources and low-carbon and environmentally friendly production.
Smart Images

Figure CN119016188A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ore dressing, and in particular relates to a method for increasing the yield of fine-grained titanium concentrate. Background Art
[0002] The Panxi area is rich in vanadium-titanium magnetite resources with proven reserves of 93.933×10 8 t, and the predicted reserves are 30 billion tons, of which iron reserves account for 20% of the country, ranking second in the country; the proven reserves of titanium resources (in terms of TiO2) are 428 million tons, accounting for 93% of the country's reserves, ranking first in the world; the proven reserves of vanadium resources (in terms of V2O5) are 10.4786 million tons, accounting for 63% of the country's reserves, ranking third in the world. After decades of efforts, the development and utilization of vanadium-titanium magnetite resources in Panxi area have achieved a series of major scientific research results. However, in the comprehensive utilization of vanadium-titanium magnetite in Panxi area, there is also a problem of low resource utilization rate. The recovery rates of iron, vanadium and titanium elements are about 60%, 39% and 10% respectively. In particular, the precious titanium resources have a relative utilization rate of about 10% to 20% of the original ore, resulting in a large waste of resources. This is the most prominent problem in the comprehensive utilization of Panxi vanadium-titanium magnetite.
[0003] Crushing and grinding is the leading process of the ore dressing plant and the last process of material preparation. The quality of the selection operation index depends largely on the quality of the grinding products. According to statistics, the energy consumption of crushing and grinding in the ore dressing plant accounts for about 65% to 75% of the total energy consumption of the ore dressing plant, and the cost accounts for 50% to 70% of the total cost of the ore dressing plant. Therefore, it has great economic and social benefits to correctly select the grinding process, optimize the grinding process parameters, and improve the grinding and classification efficiency.
[0004] CN103706463A discloses a titanium selection method, comprising the following steps: dissociating titanium selection ore to separate ilmenite with a particle size of less than 0.25m from gangue minerals in the titanium selection ore; classifying the dissociated ore to obtain fine-grained ore with a particle size of less than 0.074mm and coarse-grained ore with a particle size of more than 0.074m; performing coarse separation treatment on the coarse-grained ore to remove ore with a particle size of more than 1.0mm; performing a first stage of iron removal and a first stage of strong magnetic separation on the separated ore to obtain strong magnetic concentrate and tailings; performing cyclone classification and vibrating screen classification on the strong magnetic concentrate, and sending the ore with a particle size of less than 0.18m obtained by cyclone classification to the vibrating screen for further classification to remove the ore with a particle size of more than 0. The ore with a particle size of more than 18m, the ore with a particle size of more than 0.18m obtained by cyclone classification and vibrating screen classification is returned to the cyclone classification step for further selection after grinding treatment; the ore with a particle size of less than 0.18m obtained by vibrating screen classification is successively subjected to two-stage iron removal, two-stage strong magnetic separation, concentration and flotation to obtain titanium concentrate, wherein the content of ore with a particle size of more than 0.18mm in the ore to be floated is 10-20wt%, the content of ore with a particle size of 0.100-0.18mm is 20-30%, the content of ore with a particle size of 0.074-0.100mm is 20-25wt%, the content of ore with a particle size of less than 0.074mm is 30-40wt%, and the content of TiO2 is 20-24wt%. This method is mainly used to produce coarse-grained titanium concentrate, and the output of fine-grained titanium concentrate is relatively low. In addition, with the passage of time, the properties of the ore have changed significantly, resulting in the current titanium concentrate flotation grade being reduced to 12-14%, and the recovery rate being reduced to below 80%. This method obtains high-grade ore to be floated, which is difficult to meet the current low flotation grade production situation.
[0005] Therefore, under the current conditions of low flotation grade and low recovery rate, it is urgent to develop a new process to promote the recovery of fine-grained titanium concentrate and increase the output of titanium concentrate. Summary of the invention
[0006] The purpose of the present invention is to provide a method for increasing the output of fine-grained titanium concentrate, so as to solve the problems of low utilization rate of vanadium and titanium resources and low output of titanium concentrate in Panzhihua area, and to achieve energy conservation and emission reduction, green production, and solve the problems of low-carbon environmental protection, energy consumption reduction, cost reduction, efficiency improvement and development promotion.
[0007] The present invention provides a method for increasing the yield of fine-grained titanium concentrate, which comprises the following steps:
[0008] A. Perform a weak magnetic separation to remove iron from the titanium ore, with a magnetic field strength of 1800-2000GS, to obtain weak magnetic separation tailings and sub-iron concentrate (the sub-iron concentrate is incorporated into the upstream iron concentrate);
[0009] B. The weak magnetic separation tailings obtained in step A are subjected to a stage of strong magnetic separation operation, and the magnetic field strength is 2000-2500GS to obtain a stage of strong magnetic separation concentrate and a stage of strong magnetic separation tailings (a stage of strong magnetic separation tailings directly enters the tailings pond);
[0010] C. The concentrated ore obtained in step B is put into the cyclone for classification, and the diameter of the feed port is controlled to be 240-250mm, the working pressure is 0.06-0.15Mpa, the overflow pipe diameter is 300-310mm, the sand settling port diameter is 90-100mm, the slurry concentration is 40-45wt%, and the overflow and sand settling are obtained;
[0011] D. The sand settling obtained in step C is subjected to ball milling and re-grinding, the working speed is controlled to be 20-25r / min, the diameter of the ball milling steel ball is 40+60mm, the grinding concentration is 65-75%, and the ball mill discharge is returned to the cyclone for re-classification, forming a closed-circuit grinding and classification operation;
[0012] E. The overflow obtained in step C enters the high-frequency vibrating screen for inspection and screening. The sieve hole diameter of the high-frequency vibrating screen is 0.15-0.18 mm, the screen surface inclination is 23-25°, and the frequency is 55-65 Hz. The oversize and undersize are obtained. The oversize is returned to the cyclone with the ball mill discharge for re-classification;
[0013] F. The undersize obtained in step E is subjected to an iron removal magnetic separation operation (CTB1230 permanent magnetic drum magnetic separator can be used for the iron removal magnetic separation operation) to obtain an iron removal concentrate (the iron removal concentrate enters the concentrate bin) and an iron removal tailings;
[0014] G. The iron removal tailings obtained in step F are subjected to a second-stage strong magnetic separation operation (the second-stage strong magnetic separation can adopt LHGC2.5Ft.00WX vertical ring pulsating high gradient strong magnetic machine), the stroke is controlled to be 10-14mm, the pulse is 200-250min, the background field strength is 0.65-0.90T, the exciting power is 80-100kw, and the exciting voltage is 65-70V, to obtain the second-stage strong magnetic separation concentrate and the second-stage strong magnetic separation tailings (the second-stage strong magnetic separation tailings are returned to the cyclone with the ball mill discharge for re-classification);
[0015] H. The second-stage strong magnetic separation concentrate obtained in step G is subjected to fine-grained flotation operation (XCF flotation machine can be used for fine-grained flotation operation), and after flotation, fine-grained titanium concentrate is obtained.
[0016] Among them, in the above method for increasing the output of fine-grained titanium concentrate, in step A, the TFe grade of the titanium ore is 11.35-12.56wt%, and the TiO2 grade is 6.87-7.40wt%.
[0017] Among them, in the above method for increasing the output of fine-grained titanium concentrate, in step D, the mass ratio of 40 mm and 60 mm ball milling steel balls is 1:1.
[0018] Wherein, in the above method for increasing the yield of fine-grained titanium concentrate, in step F, the magnetic field intensity of the iron-removal magnetic separation operation is 2000-2500 GS.
[0019] Among them, in the above-mentioned method for increasing the output of fine-grained titanium concentrate, in step H, in the fine-grained flotation operation, the flotation agent used is a conventional flotation agent in the field, generally MOH-3 with a concentration of 5-10%, xanthate with a concentration of 5-10%, sulfuric acid with a concentration of 25-30%, diesel 200g / t and 2# oil 40g / t, and the pulp concentration is 50-65%.
[0020] In the present invention, the titanium ore is the tailings obtained by subjecting vanadium-titanium magnetite to the conventional iron separation process in the titanium selection process of the titanium plant, and then subjected to the conventional slag separation and classification.
[0021] Since the resource endowment in Panxi region is not much different, the process of the present invention can be extended to other ore dressing plants in Panxi region, which can greatly improve the utilization rate of vanadium and titanium resources in Panxi region. However, the present invention is not limited to Panxi region, and is applicable to vanadium and titanium magnetite in other regions.
[0022] Beneficial effects of the present invention:
[0023] The present invention deeply studies the mineral particle size composition, which is the main factor affecting grinding and classification, and studies the changes in mineral content between each particle size of titanium ore and screened qualified products, optimizes and adjusts the process, and accurately controls parameters such as increasing cyclone concentration and grinding concentration to improve classification efficiency, change the distribution of chemical analysis and particle size during the mineral processing process, make the TiO2 in the qualified products more enriched, and significantly improve the output and quality of fine-grained titanium concentrate when the flotation grade is low, greatly release the production capacity of fine-grained titanium concentrate, thereby promoting the improvement of titanium concentrate operation rate and achieving more full utilization of iron ore tailings resources.
[0024] In addition, the method of the present invention improves the grinding and classification efficiency in the titanium selection process, releases the hourly processing capacity of the ball mill and classification equipment, reduces the grinding and classification cycle load, reduces the power consumption of the grinding equipment and classification equipment, improves the equipment utilization coefficient, greatly improves the grinding output and grinding efficiency, increases the qualified output of titanium concentrate, improves the economic benefits of the enterprise, and is of great significance in energy conservation, emission reduction, cost reduction and efficiency improvement. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a schematic diagram of the process flow of the present invention. DETAILED DESCRIPTION
[0026] The present invention is further described in detail below by way of examples, but the protection scope of the present invention is not limited to the scope of the examples.
[0027] Test Example 1
[0028] The test object selected this time is the titanium ore in the titanium selection process of a titanium plant in Panxi area (the titanium ore is the tailings obtained after the vanadium-titanium magnetite is processed through the iron selection process, and then the material is separated and classified). Since the particle size entering the flotation is required to be below 0.1mm, the evaluation standard for the test results is -0.1mm. According to the requirements of the test plan, the composition of the test raw materials was analyzed, and the relevant analysis results are shown in Table 1.
[0029] Table 1 Chemical analysis results of main elements of titanium ore / wt%
[0030] P TFe <![CDATA[TiO2]]> S CaO <![CDATA[K2O]]> 0.016 12.00 7.05 0.355 12 0.084 MgO <![CDATA[Na2O]]> <![CDATA[SiO2]]> <![CDATA[Al2O3]]> — — 10.04 1.28 38.14 10.96 — —
[0031] As can be seen from Table 1, the TFe grade in the titanium ore is 12.00%, and the TiO2 grade is 7.05%. The Ca, Mg, and Al contents (in terms of oxide content) are 12.00%, 10.04%, and 10.96%, respectively. The contents are relatively high, which has a great impact on the subsequent utilization of titanium concentrate.
[0032] In order to better formulate the test plan, a screening test was carried out on the main influencing factor of grinding and classification - mineral particle size composition. The test equipment mainly used the multi-layer hydraulic screen of the beneficiation and smelting joint laboratory combined with manual inspection and screening. The screening results are shown in Table 2.
[0033] Table 2 Titanium ore screening test / wt%
[0034] +65 mesh 65-100 mesh 100-150 mesh 150-200 mesh 200-400 mesh -400 mesh 22.03 18.38 8.12 11.37 4.87 35.23
[0035] Among them, "+65 mesh" means the material on the 65 mesh standard sieve; "65-100 mesh" means the material under the 65 mesh standard sieve and the material on the 100 mesh standard sieve; "100-150 mesh" means the material under the 100 mesh standard sieve and the material on the 150 mesh standard sieve; "150-200 mesh" means the material under the 150 mesh standard sieve and the material on the 200 mesh standard sieve; "200-400 mesh" means the material under the 200 mesh standard sieve and the material on the 400 mesh standard sieve; "-400 mesh" means the material under the 400 mesh standard sieve.
[0036] As can be seen from Table 2, the main particle size of the titanium ore shows an extreme phenomenon of "big at both ends and small in the middle", indicating that the particle size fluctuations in the upstream iron selection operation are large, and pre-screening before entering the mill is very necessary. In addition, the particle size above 0.1mm (150 mesh) accounts for about 50%, while the particle size requirement for entering the mill is generally less than 0.1mm, so there is a large grinding space for the titanium ore.
[0037] In order to better understand the changes in mineral content between different particle sizes of titanium ore and qualified screened products, chemical analysis was carried out on the sieved samples of each particle size. The results are shown in Tables 3 and 4.
[0038] Table 3 Chemical analysis results of titanium ore / wt%
[0039] Mesh TFe <![CDATA[TiO2]]> +65 15.12 11.76 65-100 21.00 22.74 100-150 19.50 18.32 150-200 19.38 16.58 200-400 20.25 16.50 -400 24.13 19.88
[0040] Table 4 Chemical analysis results of qualified products (i.e., raw materials for floating) / wt%
[0041] Mesh TFe <![CDATA[TiO2]]> +65 12.50 6.41 65-100 15.60 11.14 100-150 16.50 12.29 150-200 17.50 14.15 200-400 19.40 16.62 -400 22.90 19.56
[0042] From the analysis of Table 3, it can be seen that the TFe content and TiO2 content in the titanium ore show a fluctuation change of first increasing, then decreasing, and then increasing as the particle size decreases, and at 65-100 mesh, the TFe and TiO2 contents basically reach the peak value, indicating that the available ilmenite resources in the 0.15mm milled product are relatively large, and effective grinding operations can increase the output of titanium concentrate. From the analysis of Table 4, it can be seen that as the particle size of the screened qualified product decreases, the TFe content and TiO2 content become larger and larger. The basic rule is that the finer the particle size, the higher the TFe content and TiO2 content. Among them, when the particle size composition is -400 mesh, the TFe and TiO2 contents are 22.90% and 19.56%, respectively, reaching the peak value. And it meets the particle size requirements of the subsequent coarse particle flotation operation of the titanium plant, indicating that the grinding classification test should mainly consider the proportion of 150-200 mesh, which can improve the titanium selection operation rate and increase the output of titanium concentrate.
[0043] Based on the above findings, the present invention optimizes and adjusts the process to make the TiO2 in the qualified product more enriched, thereby improving the flotation grade and ultimately increasing the output and grade of fine-grained titanium concentrate.
[0044] Example 1
[0045] A. The titanium ore in Experimental Example 1 is subjected to a weak magnetic separation to remove iron, and the magnetic field strength is 2000GS. The tailings obtained by the weak magnetic separation are subjected to a strong magnetic separation operation, and the secondary iron concentrate is incorporated into the upstream iron concentrate;
[0046] B. The magnetic field strength of the first stage of strong magnetic separation is 2000GS. The concentrate obtained by the first stage of strong magnetic separation is classified by cyclone, and the tailings are directly sent to the tailings pond;
[0047] C. During the hydrocyclone classification, the feed port diameter is controlled to be 250mm, the working pressure is 0.12Mpa, the overflow pipe diameter is 300mm, the sand settling port diameter is 100mm, and the pulp concentration is 45wt%. The overflow obtained from the hydrocyclone classification enters the high-frequency vibrating screen for inspection and screening, and the sand is sent to the ball mill for regrinding;
[0048] D. During ball milling and regrinding, control the working speed to 20r / min-1 The diameter of the ball mill is 40+60mm (mass ratio 1:1), the grinding concentration is 68wt%, and the ball mill discharge is returned to the cyclone for re-classification, forming a closed-loop grinding and classification operation;
[0049] E. The diameter of the high-frequency vibration screen is 0.15 mm, and the screen surface inclination is 25 ° The frequency is 60Hz. The material on the screen is returned to the cyclone for re-classification along with the ball mill discharge, and the material under the screen enters the next stage of magnetic separation for iron removal.
[0050] F. The iron removal operation uses a CTB1230 permanent magnetic drum magnetic separator with a magnetic field strength of 2000GS. The iron-free concentrate obtained by magnetic separation enters the concentrate bin, and the tailings (TiO2 grade 18.56%) undergo a second-stage strong magnetic separation operation;
[0051] G. The second stage of high-intensity magnetic separation uses LHGC2.5Ft.00WX vertical ring pulsating high-gradient high-intensity magnetic machine, 14mm stroke, 220min pulse, background field strength of 0.8T, exciting power of 80kw, exciting voltage of 66.8V, and the magnetic concentrate (TiO2 grade 16.98%) obtained from the second stage of high-intensity magnetic separation is subjected to fine-grained flotation operation, and the tailings are returned to the cyclone with the ball mill discharge for re-classification;
[0052] H. The magnetic concentrate obtained from the second stage of strong magnetic separation is fed into the XCF flotation machine for fine-grained flotation. The flotation reagents are MOH-3 (5%), xanthate (5%), sulfuric acid (25%), diesel 200g / t and 2# oil 40g / t. The pulp concentration is 50%. After flotation, fine-grained titanium concentrate is obtained. The Ti recovery rate is 85.17%, the TiO2 grade is 47.5%, and 0.11 tons of fine-grained titanium concentrate can be obtained per ton of raw ore; the TiO2 grade of the tailings is 4.35%, and the yield is 94.46%. According to 82.55t·h -1 Calculations show that tailings will be reduced by about 30,000 tons per year.
[0053] Table 5 Statistics of particle size distribution of fine-grained titanium concentrate / wt%
[0054]
[0055] The sieve analysis test results of this embodiment are shown in Table 6, and the classification efficiency is shown in Table 7.
[0056] Table 6 Example 1 Sieve Analysis Test Results / wt%
[0057]
[0058] The classification efficiency is divided into two evaluation indicators: classification quality efficiency and quantity efficiency. In actual production, the classification efficiency is mostly calculated by quality efficiency. The calculation formula is as follows:
[0059]
[0060] Among them, β represents the content of -0.074mm particle size in the classification overflow; α represents the content of -0.074mm particle size in the classification feed; θ represents the content of -0.074mm particle size in the classification return sand.
[0061] Table 7 Statistics of classification efficiency of Example 1 and Comparative Example 1
[0062]
[0063] Comparative Example 1
[0064] Traditional crafts:
[0065] A. The titanium ore in Experimental Example 1 is subjected to weak magnetic separation to remove iron, and the magnetic field strength is 3000GS. The tailings obtained by weak magnetic separation are subjected to a strong magnetic separation operation, and the secondary iron concentrate is incorporated into the upstream iron concentrate;
[0066] B. The magnetic field strength of the first stage of strong magnetic separation is 5500GS. The concentrate obtained by the first stage of strong magnetic separation is classified by cyclone, and the tailings are directly sent to the tailings pond;
[0067] C. During the hydrocyclone classification, the feed port diameter is controlled to be 250mm, the working pressure is 0.06-0.15Mpa, the overflow pipe diameter is 300mm, the sand settling port diameter is 110mm, and the pulp concentration is 34.08wt%. The overflow obtained from the hydrocyclone classification enters the high-frequency vibrating screen for inspection and screening, and the sand is sent to the ball mill for regrinding;
[0068] D. During ball milling and regrinding, the working speed is controlled at 19.4r·min -1 The diameter of the ball mill is 40 mm, the grinding concentration is 52.76 wt%, and the ball mill discharge is returned to the cyclone for reclassification, forming a closed-loop grinding and classification operation;
[0069] E. The mesh size of the high-frequency vibrating screen is 0.15 mm, the screen surface inclination is 20°, and the frequency is 50 Hz. The material on the screen is returned to the cyclone for re-classification along with the ball mill discharge, and the material under the screen enters the next stage of magnetic separation for iron removal.
[0070] F. For iron removal, a Slon-4000 vertical ring pulsating high gradient medium magnetic machine is used, with a magnetic field strength of 5500GS. The iron-removing concentrate obtained by magnetic separation enters the concentrate bin, and the tailings (TiO2 grade 17.12%) undergo a second stage of strong magnetic separation.
[0071] G. The second stage of high-intensity magnetic separation uses a Slon-2500TP (0.8) vertical ring pulsating high-gradient high-intensity magnetic machine with a magnetic field strength of 5500GS, a 25mm stroke, a 300min pulse, a background field strength of 1.0T, an exciting power of 77.28kw, and an exciting voltage of 220V. The magnetic concentrate (TiO2 grade 16.03%) obtained from the second stage of high-intensity magnetic separation is subjected to fine-grained flotation, and the tailings enter the tailings pond along with the concentrated tailings;
[0072] H. The magnetic concentrate obtained by the second-stage strong magnetic separation is fed into the XCF flotation machine for fine-grained flotation. The flotation reagents are MOH-3 (5%), xanthate (5%), sulfuric acid (25%), diesel 200g / t and 2# oil 40g / t. The pulp concentration is 50%. After flotation, fine-grained titanium concentrate is obtained. The Ti recovery rate is 83.78%, the TiO2 grade is 47.37%, and 0.08 tons of fine-grained titanium concentrate can be obtained per ton of raw ore; the TiO2 grade of the tailings is 4.6%, and the yield is 97.34%.
[0073] Table 8 Statistics of particle size distribution of fine-grained titanium concentrate / wt%
[0074]
[0075] The sieve analysis test results of this comparative example are shown in Table 9.
[0076] Table 9 Comparative Example 1 Sieve Analysis Test Effect / wt%
[0077]
[0078]
[0079] From the analysis of Tables 5 to 9, it can be seen that after the process flow is optimized by the present invention, the classification efficiency of the cyclone and the vibrating screen is significantly improved, and the coarse particles above 150 mesh in the overflow of the cyclone are reduced, the qualified products on the screen in the vibrating screen are reduced (more qualified products enter under the screen), the qualified products under the screen in the vibrating screen are increased, and the output of fine-grained titanium concentrate is significantly improved, indicating that the process optimization is successful.
Claims
1. A method for increasing the yield of fine-grained titanium concentrate, characterized in that: The following steps are involved: A. Perform a weak magnetic separation to remove iron from the titanium ore, with a magnetic field strength of 1800-2000GS, to obtain weak magnetic separation tailings and sub-iron concentrate; B. The weak magnetic separation tailings obtained in step A are subjected to a stage of strong magnetic separation operation, and the magnetic field strength is 2000-2500GS to obtain a stage of strong magnetic separation concentrate and a stage of strong magnetic separation tailings; C. The concentrated ore obtained in step B is put into the cyclone for classification, and the diameter of the feed port is controlled to be 240-250mm, the working pressure is 0.06-0.15Mpa, the overflow pipe diameter is 300-310mm, the sand settling port diameter is 90-100mm, the slurry concentration is 40-45wt%, and the overflow and sand settling are obtained; D. The sand settling obtained in step C is subjected to ball milling and re-grinding, the working speed is controlled to be 20-25r / min, the diameter of the ball milling steel ball is 40+60mm, the grinding concentration is 65-75%, and the ball mill discharge is returned to the cyclone for re-classification, forming a closed-circuit grinding and classification operation; E. The overflow obtained in step C enters the high-frequency vibrating screen for inspection and screening. The sieve hole diameter of the high-frequency vibrating screen is 0.15-0.18 mm, the screen surface inclination is 23-25°, and the frequency is 55-65 Hz. The oversize and undersize are obtained. The oversize is returned to the cyclone with the ball mill discharge for re-classification; F. The undersize obtained in step E is subjected to magnetic separation for iron removal to obtain iron-removing concentrate and iron-removing tailings; G. The iron removal tailings obtained in step F are subjected to a two-stage strong magnetic separation operation, with a controlled stroke of 10 to 14 mm, a pulse of 200 to 250 min, a background field strength of 0.65 to 0.90 T, an exciting power of 80 to 100 kW, and an exciting voltage of 65 to 70 V to obtain a two-stage strong magnetic separation concentrate and a two-stage strong magnetic separation tailings; H. The second-stage strong magnetic separation concentrate obtained in step G is subjected to fine-grained flotation operation. After flotation, fine-grained titanium concentrate is obtained.
2. The method for increasing the yield of fine-grained titanium concentrate according to claim 1, characterized in that: In step A, the TFe grade of the titanium ore is 11.35-12.56wt%, and the TiO2 grade is 6.87-7.40wt%.
3. The method for increasing the yield of fine-grained titanium concentrate according to claim 1, characterized in that: In step D, the mass ratio of 40 mm and 60 mm milling steel balls is 1:
1.
4. The method for increasing the yield of fine-grained titanium concentrate according to claim 1, characterized in that: In step F, the magnetic field strength of the iron removal magnetic separation operation is 2000-2500 GS.
5. The method for increasing the yield of fine-grained titanium concentrate according to any one of claims 1 to 4, characterized in that: In step H, in the fine particle flotation operation, the flotation reagents are MOH-3, xanthate, sulfuric acid, diesel and 2# oil, and the pulp concentration is 50-65%.