Method for preparing battery-grade iron phosphate from copper smelting slag
By optimizing the alkaline dissolution, acid leaching and dehydration processes of copper smelting slag, the problems of high cost of disposal of copper smelting slag and high operation difficulty were solved, and high active anhydrous iron phosphate was prepared for the positive electrode material of lithium-ion batteries, which improved the battery Performance and resource utilization.
Patent Information
- Application Number
- CN202411160872.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-26
AI Technical Summary
In the prior art, the disposal method of copper smelting slag is costly and difficult to operate, and it is difficult to effectively utilize its resources, affecting the environment and economic benefits.
By mixing the copper smelting slag with sodium hydroxide and stirring, then performing acid leach and diammonium hydrogen phosphate solution treatment, adjusting the pH value, and finally heating and dehydrating in the air, optimizing the process flow to prepare amorphous anhydrous iron phosphate.
It reduces production costs and operation difficulty, improves the activity and purity of iron phosphate, and is suitable for the preparation of high-performance lithium iron phosphate battery positive electrode materials, and improves the charging and discharging performance and cycle stability of lithium-ion batteries.
Smart Images

Figure CN119018866A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of new energy materials, and in particular to a method for preparing battery-grade iron phosphate by utilizing copper smelting slag. Background Art
[0002] Copper smelting slag is a by-product of the refined copper production process. Due to the characteristics of the copper smelting process, copper smelting slag usually contains a high content of iron. At the same time, the smelting slag is also listed as hazardous waste due to its high heavy metal content. If it is not properly disposed, it will cause harm to the environment. At present, the main methods for disposing copper smelting slag are on-site storage and as raw materials for cement production, but these methods are difficult to solve the environmental problems and resource utilization problems in the process.
[0003] The rapid development of electric vehicles and grid energy storage has continuously increased the requirements for lithium-ion battery cathode materials. Lithium iron phosphate cathode materials are widely used in the field of energy storage due to their superior structural stability and low cost. As a precursor of lithium iron phosphate cathode materials, iron phosphate has good thermal stability and durability, and its preparation technology has also made great progress in the past period of time. However, the activity, structure and composition of iron phosphate have a significant impact on the performance of lithium iron phosphate cathode materials. Therefore, the preparation of iron phosphate with excellent performance is very critical for subsequent battery manufacturing.
[0004] Chinese invention patent CN202410131858.5 discloses "a method for preparing battery-grade iron phosphate using laterite nickel ore". The method obtains battery-grade anhydrous iron phosphate and nickel-containing filtrate through four steps: pre-treatment, acid leaching, iron leaching, and post-treatment. The iron phosphate obtained by this method has uniform particle size and good performance, but the reduction roasting involved in its pre-treatment process increases costs and emissions.
[0005] Chinese invention patent CN202410284637.1 discloses "a method for producing nano-battery-grade iron phosphate from titanium dioxide green vanadium". This method removes impurities from the byproduct of titanium dioxide production in an aqueous solution in multiple steps, and then oxidizes, ion-exchanges, separates solids from liquids, washes and dries the obtained ferrous sulfate to obtain nano-battery-grade iron phosphate. The iron phosphate obtained by this method has small particle size and high purity, which meets the synthesis standards of lithium iron phosphate positive electrode materials. However, the multi-step impurity removal in the solution will inevitably increase reagent consumption and operation difficulty, which is not conducive to cost and process control.
[0006] Chinese invention patent 202311274371.4 discloses "a method for preparing battery-grade iron phosphate dihydrate using flotation copper tailings". This method mixes the heat-treated flotation copper tailings with an acid solution, heats and stirs to evaporate to dryness, then adds distilled water to dissolve, to obtain a ferrous solution; then the resulting solution is oxidized and a phosphorus source is added to age the iron, and crude iron phosphate dihydrate is obtained after solid-liquid separation; the crude iron phosphate dihydrate is recrystallized to obtain refined iron phosphate dihydrate. This method achieves the separation and comprehensive recycling of iron, zinc and silicon in copper tailings, but the concentrated acid evaporation method increases the operational difficulty and risk factor of the process.
[0007] In order to overcome the problems of high cost and difficult operation of the above-mentioned prior art, the present invention provides a new method for preparing battery-grade iron phosphate using copper smelting slag. The complicated process of iron extraction is rationally optimized, and good results are achieved. The iron phosphate product obtained after aging has uniform and small particle size and low impurity content. Summary of the invention
[0008] The object of the present invention is to provide a method for preparing battery-grade iron phosphate using copper smelting slag. The amorphous anhydrous iron phosphate obtained under optimized conditions in the method has higher activity than α-spinel iron phosphate, which is beneficial to the preparation of positive electrode materials and the improvement of their electrochemical performance.
[0009] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:
[0010] A method for preparing battery-grade iron phosphate using copper smelting slag comprises the following steps:
[0011] S1: mixing copper smelting slag with sodium hydroxide and pure water, heating and stirring, filtering, washing and drying the mixed solution to obtain alkaline hydrolysis slag for use;
[0012] S2: adding a mixed solution of hydrogen peroxide and nitric acid to the obtained alkaline hydrolysis residue for acid leaching, and filtering to obtain an acid leaching solution and acid leaching residue;
[0013] S3: adding diammonium hydrogen phosphate solution to the acid leaching solution, adjusting the pH under heating conditions, reacting for 0.5-2.5 hours, filtering, washing, and drying to obtain ferric phosphate dihydrate;
[0014] S4: The obtained dihydrated iron phosphate is heated and dehydrated in air to obtain anhydrous iron phosphate.
[0015] Furthermore, in step S1, the alkaline reagent is sodium hydroxide, and the alkali-slag ratio is 1.5:1, the alkali is configured as a solution, and the liquid-solid ratio of the alkaline solution to the copper smelting slag is 5:1, the alkaline hydrolysis temperature is 80-90°C, the stirring rate is 100-120rpm, and the reaction time is 3-5h;
[0016] Furthermore, the process temperature in step S2 is 75-95°C, the stirring rate is 100-120rpm, the concentration of the nitric acid solution is 1.5M, the concentration of the hydrogen peroxide is 0.5M, the ratio of the nitric acid solution to the hydrogen peroxide solution in the acid leaching solution is 7:3, the reaction liquid-solid ratio is 8-16:1, and the reaction time is 0.25-1.5h;
[0017] Furthermore, in step S3, the pH value is adjusted to pH=1-2, the amount of phosphorus source input is calculated according to the phosphorus-iron ratio of 1.15-1.25, the reaction temperature is 55-75°C, the reaction time is 0.5-1.5h, and the pH regulator is concentrated ammonia water. The drying temperature is 100°C;
[0018] Furthermore, in step S3, the pH of the acid leaching solution is 0.5-0.8.
[0019] Furthermore, the heating time of step S4 is 4 hours, and the heating temperature is 500-700°C.
[0020] On the other hand, the present invention proposes the application of the above method in the preparation of lithium iron phosphate positive electrode material precursor.
[0021] Further, the preparation principle of the present invention is as follows:
[0022] During the alkaline hydrolysis process, the main elements and impurity elements in the copper smelting slag undergo the following chemical reactions:
[0023] Fe2SiO4+2NaOH→Na2FeSiO4+FeO+H2O
[0024] Na2FeSiO4+2NaOH→Na4SiO4+FeO+H2O
[0025] Al2O3+2NaOH=Na2Al2O4+H2O
[0026] The following chemical reactions occur during the pickling process:
[0027] 2FeO+H2O2+2HNO3→2FeNO3+2H2O
[0028] The main reactions during the Chen Tie process are as follows:
[0029] Fe 3+ +PO4 3- →FePO4
[0030] Beneficial effects of the present invention:
[0031] The present invention utilizes copper smelting slag to prepare battery-grade iron phosphate, which not only effectively solves the environmental problems caused by the storage of copper smelting slag, but also converts it into high value-added products, significantly improving resource utilization. A large amount of iron in copper smelting slag is often bound by silicates and difficult to extract. The alkaline hydrolysis process of the present invention destroys the fayalite structure in the copper smelting slag, dissociates the iron from the stable structure, and is beneficial to improving the leaching rate of iron. At the same time, NaOH, as a de-impurity agent, destroys the mineral structure while removing some impurities, especially Si, which has a greater impact on the process, and Al, which poses a potential risk to product quality. Therefore, compared with the existing process of separating iron from copper smelting slag, this method is beneficial to reducing costs and reagent consumption. During the alkaline hydrolysis process, the iron in the copper smelting slag is converted into soluble iron in situ, and the specific reaction is as follows:
[0032] Fe2SiO4+2NaOH→Na2FeSiO4+FeO+H2O
[0033] Through further acid leaching treatment, the iron element is highly selectively extracted in the form of iron salts, providing a high-purity source of iron ions for the subsequent preparation of iron phosphate. As a by-product of the leaching process, the acid leaching residue in the present invention has a certain content of magnetic iron oxide, which can be used as a raw material for recovering magnetite. This method not only solves the problem of treating smelting waste residue, but also realizes the effective utilization of metal resources, which is in line with the concept of circular economy and sustainable development.
[0034] The preparation process of the present invention is simple in design and convenient for industrial large-scale production. Compared with the existing technologies such as strong acid evaporation treatment, the NaOH introduced in the present method is used as an alkaline hydrolysis agent and an impurity remover at the same time, avoiding complex pretreatment steps and multi-step impurity removal processes, reducing production difficulty and operation risks. Through the simplified process of alkaline hydrolysis and acid leaching, iron is efficiently extracted from copper smelting slag. According to the potential-pH of iron phosphate precipitation, this scheme selects a precipitation method with simple operation difficulty and low product impurities to prepare iron phosphate from copper smelting slag leachate. Theoretical analysis shows that 1-2 is the ideal pH for iron phosphate precipitation. Therefore, by adding diammonium hydrogen phosphate solution and controlling the temperature and pH of the system, dihydrate iron phosphate is finally obtained. Operating conditions such as alkaline hydrolysis temperature, acid leaching solution concentration and stirring rate are easy to achieve under conventional industrial equipment, and the reaction conditions are mild (such as alkaline hydrolysis temperature 80-90°C, acid leaching temperature 75-95°C), ensuring the stability and controllability of the process. Compared with complex reduction roasting and multi-step impurity removal technology, this method significantly reduces equipment investment and operating costs.
[0035] The present invention significantly reduces reagent consumption and production costs by optimizing reagent ratios and reaction conditions. In the acid leaching stage, a mixed solution of hydrogen peroxide and nitric acid is used to achieve an oxidative acid leaching effect and improve the leaching efficiency of iron ions. The reaction is as follows:
[0036] 2FeO+H2O2+2HNO3→2FeNO3+2H2O
[0037] As an efficient oxidant, hydrogen peroxide works synergistically with nitric acid to enhance the thermodynamics of ion leaching and improve leaching efficiency. At the same time, the reaction conditions are mild, avoiding the high dosage of strong acid and related treatment problems. By reasonably controlling the solution ratio, not only the reaction rate is increased, but also the pH range of the leaching solution can be controlled, which is conducive to reducing the amount of pH regulator used in the iron aging process, thereby reducing the amount of pH regulator used.
[0038] The anhydrous iron phosphate prepared by the present invention has high purity and high activity, and is suitable for the preparation of high-performance lithium iron phosphate battery positive electrode materials. By controlling the pH value (1-2) and reaction temperature (55-75°C) of the diammonium hydrogen phosphate solution, dihydrate iron phosphate with uniform particles is uniformly precipitated, and then dehydrated by air heating (500-700°C) to obtain anhydrous iron phosphate. Generally, when iron phosphate is heated at 550°C-590°C, a crystal transformation will occur, from an amorphous structure to an α-spinel structure. Compared with the latter, amorphous iron phosphate has a higher specific surface area and more active sites, which is beneficial to subsequent electrochemical reactions and improves the electrochemical performance of the positive electrode material. The specific reaction is as follows:
[0039] Fe 3+ +PO4 3- →FePO4
[0040] In addition, the lithium iron phosphate cathode material synthesized by amorphous anhydrous iron phosphate and a lithium source has higher reaction activity and ion migration rate than the lithium iron phosphate synthesized by α-spinel iron phosphate, thereby significantly improving the charge and discharge performance and cycle stability of lithium-ion batteries. In summary, the present invention not only optimizes the resource utilization process, simplifies the process flow, and reduces production costs, but also significantly improves the quality and performance of the product, and has broad application prospects and market value.
[0041] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0043] Figure 1 This is the XRD pattern of the original copper smelting slag;
[0044] Figure 2 Process flow chart of the present invention;
[0045] Figure 3 This is the XRD diagram of the alkaline hydrolysis residue obtained by alkaline hydrolysis in Example 1 of the present invention;
[0046] Figure 4 This is the XRD diagram of the acid leaching residue obtained by acid leaching in Example 1 of the present invention;
[0047] Figure 5 The XRD pattern of iron phosphate dihydrate obtained from Example 1 of the present invention;
[0048] Figure 6 This is a SEM image of ferric phosphate dihydrate obtained from iron in Example 1 of the present invention;
[0049] Figure 7 The XRD pattern of iron phosphate prepared in Example 1 of the present invention;
[0050] Figure 8 This is a SEM image of iron phosphate prepared in Example 1 of the present invention;
[0051] Fig. 9 The XRD pattern of iron phosphate prepared in Example 2 of the present invention;
[0052] Fig.10 This is a SEM image of iron phosphate prepared in Example 2 of the present invention;
[0053] Fig.11 The XRD pattern of iron phosphate prepared in Example 3 of the present invention;
[0054] Fig.12 This is a SEM image of iron phosphate prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0055] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0056] The copper smelting slag used in the examples was provided by a company in Sichuan. Figure 1As shown in Table 1, the total iron content in the copper smelting slag is 309.212 g / Kg, and the main elements and their contents are shown in Table 1. In addition to iron, the Al content is relatively high among the main metal elements in the copper smelting slag, and it mainly exists in the form of silicates. Since the formation conditions of its phosphate compound are similar to those of FePO4, it is easy to generate AlPO4 and exist in FePO4 as an impurity, affecting the purity and performance of the product. Therefore, efficient separation of Fe and Al is one of the technical challenges of synthesizing FePO4 from copper smelting slag. In response to this problem, the alkaline hydrolysis process of this scheme converts Al into Na2Al2O4 and enters the alkaline hydrolysis solution to achieve Al separation. At the same time, Si, as the main component, is not only a factor that restricts iron acid leaching, but also one of the sources of impurities in the product. In response to this problem, this scheme converts the insoluble silicate into Na4SiO4 through the alkaline hydrolysis process, which improves the degree of solution ionization while also reducing the Si content.
[0057] Table 1
[0058]
[0059] Example 1
[0060] like Figure 2 As shown, a method for preparing battery-grade iron phosphate using copper smelting slag described in this embodiment includes the following steps:
[0061] S1: Dissolve 45g of sodium hydroxide in 150ml of pure water, and then add 30g of copper smelting slag to the solution. Heat the solution in a water bath at 85°C and stir at 110rpm for 4h. After the reaction is completed, filter, wash and dry the cooled solution to obtain the main phase of the alkaline hydrolysis slag. Figure 3 Compared with the raw material, the diffraction peak intensity of the phase in the copper smelting slag after alkaline hydrolysis is reduced, which means that the degree of crystallization of the material in the copper smelting slag is reduced, which is beneficial to the subsequent acid leaching process.
[0062] S2: Take the copper smelting slag from step S1, add a nitric acid-hydrogen peroxide mixed solution at a liquid-solid ratio of 12:1, wherein the concentration of the nitric acid solution is 1.5M, the concentration of the hydrogen peroxide solution is 0.5M, and the ratio of the two in the mixed solution is 7:3; heat and stir, the leaching temperature is 85°C, the stirring rate is 110rpm, the reaction time is 0.5h, and after solid-liquid separation, an iron-rich solution and acid leaching residue are obtained. The main elements and concentrations of the solution are shown in Table 2, and the main phases of the acid leaching residue are as follows Figure 4 As shown. The main impurity elements in the acid leaching solution are Zn and Mg, but the precipitation conditions of the phosphates and hydroxides of these two elements are far from the formation range of iron phosphate, that is, these two high-content impurities can be removed by controlling the reaction conditions. At the same time, the content of Al in the acid leaching solution has been greatly reduced, confirming the beneficial effect of the alkaline hydrolysis process on impurity removal. Figure 4 Phase analysis showed a large amount of dissolution of ferrosilicate after acid leaching, which is consistent with the high iron content in the solution. In addition, the intensity of the magnetite peak in the acid leached residue increased, indicating an increase in its relative content, making the copper smelting slag after acid leaching a potential product for magnetic separation of magnetite.
[0063] Table 2
[0064] element Fe Al Zn Pb Mg Concentration g / L 12.01 0.06 0.6 0.09 0.4
[0065] S3: Under heating conditions of 65°C, add 0.1M diammonium hydrogen phosphate solution to the acid leaching solution (pH = 0.7) in a phosphorus-iron ratio of 1.2:1, and adjust the pH to 1.5. The reaction time is 1h. Immediately after the reaction, filter the solution and wash it with hot water 3 times. Place the filter residue in a 100°C forced air drying oven to dry it to obtain dihydrated iron phosphate. Its XRD and SEM images are shown in the figure. Figure 5 , 6 XRD shows that the iron phosphate dihydrate obtained by the method is amorphous; SEM images and EDS energy spectrum preliminarily prove that the obtained material is a blocky iron phosphide compound, and its particle size is between several microns and more than ten microns.
[0066] S4: Sinter the dihydrated iron phosphate obtained in step S3 at 500 degrees Celsius in an air atmosphere for 4 hours, and grind to obtain anhydrous iron phosphate. Figure 7 , 8 Its main components, content, particle size and comparison with battery-grade iron phosphate are shown in Table 3. XRD shows that the iron phosphate obtained under this condition is amorphous; SEM images and EDS spectra also prove that the obtained substance is a phosphorus iron compound, and its morphology is flocculent, and the three elements of P, Fe and O are evenly distributed in the product. The elements and particle size in Table 3 and their comparison with the standard of battery-grade iron phosphate show that the iron phosphate obtained under this condition has a small particle size and the content of each element meets the requirements of battery-grade iron phosphate.
[0067] Table 3
[0068]
[0069]
[0070] Example 2
[0071] A method for preparing battery-grade iron phosphate using copper smelting slag as described in this embodiment includes the following steps:
[0072] S1: Dissolve 45g of sodium hydroxide in 150ml of pure water, and then add 30g of copper smelting slag to the solution. Heat the solution in a water bath at 80°C and stir at 100rpm for 4h. After the reaction is completed, filter the cooled solution to obtain alkaline hydrolysis slag.
[0073] S2: Take the copper smelting slag from step S1, add a nitric acid-hydrogen peroxide mixed solution at a liquid-solid ratio of 8:1, wherein the concentration of the nitric acid solution is 1.5M, the concentration of the hydrogen peroxide solution is 0.5M, and the ratio of the two in the mixed solution is 7:3; heat and stir, the leaching temperature is 75°C, the stirring rate is 100rpm, the reaction time is 0.25h, and after solid-liquid separation, an iron-rich solution is obtained for standby use;
[0074] S3: Under heating conditions of 55°C, add 0.1M diammonium hydrogen phosphate solution to the acid leaching solution (pH = 0.8) in a phosphorus to iron ratio of 1.15:1, and adjust the pH to 1.0. The reaction time is 0.5h. Immediately after the reaction, filter the solution and wash it with hot water three times. Place the filter residue in a 100°C forced air drying oven to dry it to obtain dihydrated iron phosphate.
[0075] S4: Sinter the dihydrated iron phosphate obtained in step S3 at 600 degrees Celsius in an air atmosphere for 4 hours, and grind to obtain anhydrous iron phosphate. Fig. 9 , 10 Its main components, content and particle size are shown in Table 3. XRD shows that the iron phosphate obtained under this condition is crystalline, that is, olivine-type iron phosphate; SEM images and EDS energy spectra also prove that the obtained substance is a blocky iron phosphate compound, P and O are missing in some areas of the EDS spectrum, and the element distribution is uneven. The elements and particle size in Table 3 and their comparison with the standard of battery-grade iron phosphate show that the iron phosphate obtained under this condition has a slightly larger particle size, and the content of each element meets the requirements of battery-grade iron phosphate.
[0076] Example 3
[0077] A method for preparing battery-grade iron phosphate using copper smelting slag as described in this embodiment includes the following steps:
[0078] S1: Dissolve 45g of sodium hydroxide in 150ml of pure water, and then add 30g of copper smelting slag to the solution. Heat the solution in a water bath at 90°C and stir at 120rpm for 4h. After the reaction is completed, filter the cooled solution to obtain alkaline hydrolysis slag.
[0079] S2: taking the copper smelting slag from step S1, adding a nitric acid-hydrogen peroxide mixed solution at a liquid-solid ratio of 16:1, wherein the concentration of the nitric acid solution is 1.5M, the concentration of the hydrogen peroxide solution is 0.5M, and the ratio of the two in the mixed solution is 7:3; heating and stirring, the leaching temperature is 95°C, the stirring rate is 120rpm, the reaction time is 1.5h, and after solid-liquid separation, an iron-rich solution is obtained for standby use;
[0080] S3: Under heating conditions of 75°C, add 0.1M diammonium hydrogen phosphate solution to the acid leaching solution (pH=0.5) in a phosphorus-iron ratio of 1.25:1, and adjust the pH to 2.0. The reaction time is 1.5 hours. Immediately after the reaction, filter the solution and wash it with hot water three times. Place the filter residue in a 100°C forced air drying oven to dry it to obtain dihydrated iron phosphate.
[0081] S4: The dihydrated iron phosphate obtained in step S3 is sintered at 700 degrees Celsius in an air atmosphere for 4 hours, and then ground to obtain anhydrous iron phosphate. Fig.11 , 12 Its main components, contents and particle sizes are shown in Table 3. XRD shows that the iron phosphate obtained under this condition is crystalline, i.e., olivine-type iron phosphate; SEM images and EDS energy spectra also prove that the obtained substance is a blocky flocculent iron phosphate compound, and P, O, and Fe are relatively evenly distributed in the EDS spectrum. The elements and particle sizes in Table 3 and their comparison with the standard of battery-grade iron phosphate show that the particle size of the iron phosphate obtained under this condition is relatively large, and the content of each element basically meets the requirements of battery-grade iron phosphate.
[0082] In summary, the present invention proposes a method for preparing battery-grade iron phosphate using copper smelting slag. The oxidative acid leaching method of the present invention realizes oxidation while leaching iron, and the introduction of an oxidant enhances the leaching process, thereby obtaining a relatively ideal leachate, which is beneficial to the pH adjustment and precipitation of iron phosphate in the subsequent aging process. Oxidation and acid leaching promote each other and simplify the operation process.
[0083] The present invention is conducive to the preparation of lithium iron phosphate positive electrode materials with high discharge capacity, stable cycle performance and excellent rate performance, and provides a new idea for the preparation of lithium iron phosphate positive electrode material precursors.
[0084] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for preparing battery-grade iron phosphate using copper smelting slag, characterized in that: The following steps are involved: S1: mixing copper smelting slag with sodium hydroxide and pure water, heating and stirring, filtering, washing and drying the mixed solution to obtain alkaline hydrolysis slag for use; S2: adding a mixed solution of hydrogen peroxide and nitric acid to the obtained alkaline hydrolysis residue for acid leaching, and filtering to obtain an acid leaching solution and acid leaching residue; S3: adding diammonium hydrogen phosphate solution to the acid leaching solution, adjusting the pH under heating conditions, reacting for 0.5-2.5 hours, filtering, washing, and drying to obtain ferric phosphate dihydrate; S4: The obtained dihydrated iron phosphate is heated and dehydrated in air to obtain anhydrous iron phosphate.
2. The method for preparing battery-grade iron phosphate using copper smelting slag according to claim 1, characterized in that: In step S1, the alkali reagent is sodium hydroxide, and the alkali-slag ratio is 1.5:1, the alkali is configured as a solution, and the liquid-solid ratio of the alkali solution to the copper smelting slag is 5:1, the alkaline hydrolysis temperature is 80-90°C, the stirring rate is 100-120rpm, and the reaction time is 3-5h.
3. The method for preparing battery-grade iron phosphate using copper smelting slag according to claim 1, characterized in that: The process temperature in step S2 is 75-95° C., the stirring rate is 100-120 rpm, the concentration of the nitric acid solution is 1.5 M, the concentration of the hydrogen peroxide is 0.5 M, the ratio of the nitric acid solution to the hydrogen peroxide solution in the acid leaching solution is 7:3, the reaction liquid-to-solid ratio is 8-16:1, and the reaction time is 0.25-1.5 h.
4. The method for preparing battery-grade iron phosphate using copper smelting slag according to claim 1, characterized in that: In step S3, the pH is adjusted to 1-2, the amount of phosphorus source input is calculated according to the phosphorus-iron ratio of 1.15-1.25, the reaction temperature is 55-75°C, the reaction time is 0.5-1.5h, the pH regulator is concentrated ammonia water; and the drying temperature is 100°C.
5. The method for preparing battery-grade iron phosphate using copper smelting slag according to claim 1, characterized in that: The pH of the acid leaching solution in step S3 is 0.5-0.
8.
6. The method for preparing battery-grade iron phosphate using copper smelting slag according to claim 1, characterized in that: The heating time of step S4 is 4 hours, and the heating temperature is 500-700°C.
7. Use of the method according to any one of claims 1 to 6 in the preparation of lithium iron phosphate positive electrode material precursor.
Citation Information
Cited By
High-compaction-density ferric sodium pyrophosphate positive electrode material and preparation method thereof
CN119929768A
Highly compacted density pyrophosphate sodium ferric phosphate cathode material and preparation method thereof
CN119929768B