Powder flocculant for treating oily sewage on emergency accident site and preparation method of powder flocculant

By modifying powder flocculants of starch, bentonite and chitosan, the complexity and cost of treating oily wastewater in the prior art are solved, and rapid and efficient flocculation and emergency response are achieved at the accident site, avoiding Secondary pollution ensures the normal supply of fire water.

CN119018995AInactive Publication Date: 2024-11-26CHINA PETROLEUM & CHEMICAL CORP +1

Patent Information

Application Number
CN202310602753.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art processes are complex, costly and cannot meet the rapid and efficient needs of the emergency site when dealing with oily sewage. Liquid agents need to be used on site, which is difficult to meet the emergency needs of the accident site, and there is secondary pollution and insufficient fire water resources. question.

Method used

The powder flocculant is prepared by using modified starch, bentonite and chitosan. It is prepared into powder form through a simple process, which can quickly flocculate in oily wastewater, with a flocculation time of less than 60 seconds to avoid secondary pollution. And can be stored for a long time.

Benefits of technology

It realizes efficient emergency response at the accident site, ensures the normal supply of fire water, avoids secondary pollution, and simplifies the use of flocculant, reducing the complexity of on-site operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018995A_ABST
    Figure CN119018995A_ABST
Patent Text Reader

Abstract

The invention discloses a powder flocculant for treating oily sewage on an emergency accident site and a preparation method thereof, and the preparation method comprises the following steps: (1) adding starch into water, ethanol or isopropanol, adding an alkaline solution, stirring and activating, then adding a quaternary ammonium salt etherifying agent, and reacting at 40-70 DEG C for 3-4 hours to prepare modified starch; (2) preparing modified bentonite by adopting an acidification modifier and a sodium modification modifier; (3) compounding tannin and chitosan according to a ratio to prepare modified chitosan; and (4) uniformly mixing the modified starch, the modified bentonite and the modified chitosan prepared in the steps (1), (2) and (3) with sodium trichloroisocyanurate and aluminum hydroxide to prepare the flocculant. According to the present invention, the preparation process is simple, the prepared flocculant can rapidly flocculate solid substances and the like in the oily sewage, the flocculation time is less than 60 s, the solid substances in the oily sewage are substantially completely flocculated and settled 2-3 min after the material feeding, and the efficient emergency treatment of the oily sewage can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flocculants for treating oily sewage, and in particular to a powder flocculant for treating oily sewage at an emergency accident site and a preparation method thereof. Background Art

[0002] At present, the leakage and fire accidents in tank areas are mostly handled by foam fire extinguishing equipment in combination with tank cooling protection and other means. On the one hand, a large amount of cooling wastewater and firefighting sewage will be generated in a short period of time. If it is not handled properly, secondary accidents such as environmental pollution are very likely to occur. In addition, the oil, particulate matter and foam liquid surfactant components in the firefighting sewage not only affect the foaming multiple, fire control time, liquid separation time and anti-burning time of the reuse process, but also affect the service life of the internal pipelines and pumps of the fire truck. If there is a large amount of floating oil in the firefighting sewage, there will be safety hazards in the reuse process. On the other hand, long-term fire rescue is bound to face the problem of insufficient firefighting water resources.

[0003] For the above-mentioned oily wastewater treatment, flocculation technology is currently usually used for treatment, that is, flocculants are added to the oily wastewater, and the added flocculants can aggregate the suspended solids in the wastewater and float or sink by gravity, thereby separating the impurities. However, the flocculant preparation process in the prior art is complicated and costly, and the actual processing and production are slow to take effect and cannot meet the rapid and efficient requirements of the emergency site. In addition, the agent is generally in liquid form and needs to be prepared on site, which does not meet the emergency needs of the accident site.

[0004] Therefore, it is urgent to study an efficient powder flocculant that can be used for oily wastewater at accident sites, which is of great significance for reducing accident risks and ensuring the normal supply of fire-fighting water. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a powder flocculant for treating oily wastewater at emergency accident sites and a preparation method thereof. The process is simple, and the flocculant can quickly flocculate solid matter in the oily wastewater. The flocculation time is less than 60s, and after 2 to 3 minutes of feeding, the solid matter in the oily wastewater is basically completely flocculated and settled, which can achieve efficient emergency treatment of oily wastewater and avoid secondary pollution caused by improper treatment of oily wastewater.

[0006] The technical solution adopted by the present invention is:

[0007] A method for preparing a powder flocculant for treating oily sewage at an emergency accident site comprises the following steps:

[0008] (1) Preparation of modified starch

[0009] (11) preparing a starch solution with at least one of water, ethanol or isopropanol;

[0010] (12) adding an alkaline solution to the starch solution prepared in step (11) while stirring, adjusting the pH value to 9 to 10, and fully stirring and activating for 25 to 30 minutes to obtain an activated starch solution;

[0011] (13) adding a quaternary ammonium salt etherifying agent to the activated starch solution obtained in step (12), reacting at 40 to 70° C. for 3 to 4 hours, then filtering to obtain modified starch solid particles, and drying and grinding the modified starch solid particles for later use;

[0012] (2) Preparation of modified bentonite

[0013] (21) adding bentonite to water to prepare bentonite slurry;

[0014] (22) adding an acidifying modifier to the bentonite slurry prepared in step (21), and reacting at 60-70° C. for 4-6 hours, and then adding a sodium modifier, and reacting at 55-95° C. for 2-3 hours, and then filtering to obtain modified bentonite solid particles, and drying and grinding the modified bentonite solid particles for later use;

[0015] (3) Preparation of modified chitosan

[0016] (31) adding an acid solution to chitosan, and adding an alkaline solution to adjust the pH to 4-6, then dropping a protective agent, and reacting at 50-70° C. for 2-3 h to prepare a chitosan Schiff base;

[0017] (32) mixing the chitosan Schiff base obtained in step (31) with tannin, adding water to prepare a mixed solution, adding an alkaline solution to adjust the pH to 4-6, adding a cross-linking agent, reacting at 60-80° C. for 2-3 hours, and then filtering to obtain modified chitosan solid particles, and drying and grinding the modified chitosan solid particles for later use;

[0018] (4) Preparation of flocculants by compounding modified starch, modified bentonite and modified chitosan

[0019] The modified starch, modified bentonite, modified chitosan prepared in steps (1), (2) and (3) are uniformly mixed with sodium trichloroisocyanurate and aluminum hydroxide to obtain a flocculant.

[0020] Furthermore, the starch in step (11) is at least one of corn starch, wheat starch or sweet potato starch.

[0021] Furthermore, the concentration of the starch solution in step (11) is 20-40%wt.

[0022] Furthermore, the concentration of the alkaline solution in step (12) is 10-20%wt.

[0023] Furthermore, in the step (13), the amount of the quaternary ammonium salt etherifying agent added is 40 to 60% of the mass of the starch dry powder.

[0024] Furthermore, in step (13), the quaternary ammonium salt etherifying agent is 3-chloro-2-hydroxypropyltriethylammonium chloride.

[0025] Furthermore, the concentration of the bentonite slurry in step (21) is 40-50%wt.

[0026] Furthermore, in the step (22), the acidifying modifier is citric acid.

[0027] Furthermore, in the step (22), the sodium modifier is at least one of NaCl, CH3COONa, Na2CO3, and NaHCO3.

[0028] Furthermore, in the step (31), the amount of the acid solution added is 1-3% of the mass of the chitosan, and the concentration of the acid solution is 0.05-0.5 mol / L.

[0029] Furthermore, the protective agent in step (31) is glyoxal or formaldehyde, and the cross-linking agent in step (32) is glyoxal.

[0030] Furthermore, in the step (32), the mass ratio of chitosan Schiff base to tannin is 1:5-10, and the mass concentration of chitosan Schiff base in the mixed solution of chitosan Schiff base and tannin in the step (32) is 5-10%.

[0031] Furthermore, in the step (4), the mass ratio of the modified starch, the modified bentonite and the modified chitosan is 1:0.5 to 1:0.2 to 0.7, the amount of sodium trichloroisocyanurate added is 2 to 6% of the total mass of the modified starch, the modified bentonite and the modified chitosan, and the amount of aluminum hydroxide added is 5 to 10% of the total mass of the modified starch, the modified bentonite and the modified chitosan.

[0032] Furthermore, in the step (4), the mass ratio of the modified starch, the modified bentonite and the modified chitosan is 1:0.6-0.8:0.3-0.5.

[0033] The present invention also provides a powdered flocculant for treating oily sewage at an emergency accident site, which is prepared by the above-mentioned preparation method.

[0034] The beneficial effects of the present invention are:

[0035] (1) The powder flocculant provided by the present invention for treating oily wastewater at an emergency accident site is obtained by compounding starch, bentonite and chitosan after modification. The flocculant preparation process is simple, it can highly match the impurity components of oily wastewater, has excellent flocculation effect, and can be stored for a long time;

[0036] (2) The powder flocculant provided by the present invention for treating oily wastewater at an emergency accident site uses starch, bentonite and chitosan as raw materials. The raw materials are widely available and the flocculant itself is guaranteed not to cause secondary pollution.

[0037] (3) The powder flocculant provided by the present invention is used for treating oily wastewater at emergency accident sites. It does not need to be compounded on site, which saves emergency time. It can quickly flocculate solid matter in oily wastewater. The flocculation time is less than 60s. After 2 to 3 minutes of feeding, the solid matter in the oily wastewater is basically completely flocculated and settled, which can achieve efficient emergency treatment of oily wastewater and avoid secondary pollution caused by improper treatment of oily wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0039] Figure 1 A relationship diagram between different stirring rates and flocculation time after the flocculant prepared in Example 1 of the present invention is added to oily wastewater;

[0040] Figure 2 This is a graph showing the relationship between the solid content in the oily wastewater and the feeding time after the flocculant prepared in Example 1 of the present invention is added to the oily wastewater. DETAILED DESCRIPTION

[0041] The present invention provides a powder flocculant for treating oily sewage at an emergency accident site and a preparation method thereof. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0042] The present invention is described in detail below with reference to the accompanying drawings.

[0043] Example 1

[0044] This embodiment provides a method for preparing a powder flocculant for treating oily wastewater at an emergency accident site, comprising the following steps:

[0045] (1) Preparation of modified starch

[0046] (11) taking a certain amount of starch and adding water to prepare a starch solution;

[0047] In step (11), the starch is corn starch;

[0048] The concentration of the corn starch solution in step (11) is 20%wt;

[0049] (12) adding NaOH solution to the corn starch solution prepared in step (11) while stirring, adjusting the pH value to 9, and stirring and activating for 25 minutes to obtain an activated corn starch solution;

[0050] The concentration of the NaOH solution added in step (12) is 10%wt;

[0051] (13) adding a quaternary ammonium salt etherifying agent to the activated corn starch solution obtained in step (12), and reacting at 40° C. for 3 h to fully gelatinize the starch particles and increase the substitution effect of the etherification reaction. At the same time, mechanical stirring can be used to improve the gelatinization efficiency. Then, suction filtration is performed to obtain modified corn starch solid particles, and the modified corn starch solid particles are dried and ground for later use;

[0052] The quaternary ammonium salt etherifying agent added in step (13) is 3-chloro-2-hydroxypropyltriethylammonium chloride;

[0053] The amount of the quaternary ammonium salt etherifying agent added in step (13) is 40% of the mass of the corn starch dry powder in step (11);

[0054] (2) Preparation of modified bentonite

[0055] (21) adding bentonite to water to prepare bentonite slurry;

[0056] The concentration of the bentonite slurry in step (21) is 40%wt;

[0057] (22) adding an acidifying modifier, citric acid, to the bentonite slurry prepared in step (21), and reacting at 60° C. for 4 h, then adding a sodium modifier, NaCl, and reacting at 90° C. for 2 h, and then filtering to obtain modified bentonite solid particles, and drying and grinding the modified bentonite solid particles for later use;

[0058] (3) Preparation of modified chitosan

[0059] (31) adding an acid solution to chitosan, and adding a NaOH solution to adjust the pH to 5, then dropping a protective agent, and reacting at 50 °C for 2 h to prepare a chitosan Schiff base;

[0060] In step (31), the acid solution is acetic acid, the amount of which is 1% of the mass of chitosan, and the concentration of the acetic acid solution is 0.1 mol / L;

[0061] In the step (31), the protective agent is glyoxal;

[0062] (32) mixing the chitosan Schiff base obtained in step (31) with tannin, adding water to prepare a mixed solution, adding NaOH solution to adjust the pH to 4, adding a cross-linking agent, reacting at 60° C. for 2 h, and then filtering to obtain modified chitosan solid particles, and drying and grinding the modified chitosan solid particles for later use;

[0063] In step (32), the cross-linking agent is glyoxal;

[0064] In the step (32), the mass ratio of chitosan Schiff base to tannin is 1:5.

[0065] In the step (32), the mass concentration of chitosan Schiff base in the mixed solution of chitosan Schiff base and tannin is 5%;

[0066] (4) Preparation of flocculants by compounding modified starch, modified bentonite and modified chitosan

[0067] The modified starch, modified bentonite and modified chitosan prepared in steps (1), (2) and (3) are uniformly mixed in a mass ratio of 1:0.6:0.5, and sodium trichloroisocyanurate and aluminum hydroxide are added and mixed uniformly, wherein the amount of sodium trichloroisocyanurate added is 2% of the total mass of the modified starch, modified bentonite and modified chitosan, and the amount of aluminum hydroxide added is 10% of the total mass of the modified starch, modified bentonite and modified chitosan. The above components are stirred and mixed uniformly at room temperature to obtain a flocculant.

[0068] Example 2

[0069] This embodiment provides a method for preparing a powder flocculant for treating oily wastewater at an emergency accident site, comprising the following steps:

[0070] (1) Preparation of modified starch

[0071] (11) taking a certain amount of starch and adding ethanol to prepare a starch solution;

[0072] In step (11), the starch is a mixture of corn starch and wheat starch;

[0073] The concentration of the starch solution in step (11) is 40%wt;

[0074] (12) adding NaOH solution to the starch solution prepared in step (11) while stirring, adjusting the pH value to 10, and stirring and activating for 30 minutes to obtain an activated starch solution;

[0075] The concentration of the NaOH solution added in step (12) is 20%wt;

[0076] (13) adding a quaternary ammonium salt etherifying agent to the activated starch solution obtained in step (12), reacting the mixture at 60° C. for 4 h, and then filtering the mixture to obtain modified starch solid particles, drying and grinding the modified starch solid particles for later use;

[0077] The quaternary ammonium salt etherifying agent added in step (13) is 3-chloro-2-hydroxypropyltriethylammonium chloride;

[0078] In step (13), the amount of the quaternary ammonium salt etherifying agent added is 60% of the sum of the mass of the corn starch and wheat starch dry powders;

[0079] (2) Preparation of modified bentonite

[0080] (21) adding bentonite to water to prepare bentonite slurry;

[0081] The concentration of the bentonite slurry in step (21) is 50%wt;

[0082] (22) adding an acidifying modifier, citric acid, to the bentonite slurry prepared in step (21), and reacting at 60° C. for 6 h, then adding a sodium modifier, CH3COONa, and reacting at a sodium temperature of 95° C. for 3 h, and then filtering to obtain modified bentonite solid particles, and drying and grinding the modified bentonite solid particles for later use;

[0083] (3) Preparation of modified chitosan

[0084] (31) adding an acid solution to chitosan, and adding a NaOH solution to adjust the pH to 6, then dropping a protective agent, and reacting at 65 °C for 3 h to prepare a chitosan Schiff base;

[0085] In step (31), the acid solution is acetic acid, the amount of which is 1% of the mass of chitosan, and the concentration of the acetic acid solution is 0.3 mol / L;

[0086] In the step (31), the protective agent is formaldehyde;

[0087] (32) mixing the chitosan Schiff base obtained in step (31) with tannin, adding water to prepare a mixed solution, adding NaOH solution to adjust the pH to 6, adding a cross-linking agent, reacting at 80° C. for 3 h, and then filtering to obtain modified chitosan solid particles, and drying and grinding the modified chitosan solid particles for later use;

[0088] In step (32), the cross-linking agent is glyoxal;

[0089] In step (32), the mass ratio of chitosan Schiff base to tannin is 1:10;

[0090] In the step (32), the mass concentration of chitosan Schiff base in the mixed solution of chitosan Schiff base and tannin is 10%;

[0091] (4) Preparation of flocculants by compounding modified starch, modified bentonite and modified chitosan

[0092] The modified starch, modified bentonite and modified chitosan prepared in steps (1), (2) and (3) are uniformly mixed in a mass ratio of 1:0.8:0.3, and sodium trichloroisocyanurate and aluminum hydroxide are added and mixed uniformly, wherein the amount of sodium trichloroisocyanurate added is 6% of the total mass of the modified starch, modified bentonite and modified chitosan, and the amount of aluminum hydroxide added is 5% of the total mass of the modified starch, modified bentonite and modified chitosan. The above components are stirred and mixed uniformly at room temperature to obtain a flocculant.

[0093] Example 3

[0094] This embodiment provides a method for preparing a powder flocculant for treating oily wastewater at an emergency accident site, comprising the following steps:

[0095] (1) Preparation of modified starch

[0096] (11) taking a certain amount of starch, adding isopropanol to prepare a starch solution;

[0097] In step (11), the starch is sweet potato starch;

[0098] The concentration of the starch solution in step (11) is 30%wt.

[0099] (12) adding NaOH solution to the starch solution prepared in step (11) while stirring, adjusting the pH value to 9.5, and stirring and activating for 30 minutes to obtain an activated starch solution;

[0100] The concentration of the NaOH solution in step (12) is 15%wt;

[0101] (13) adding a quaternary ammonium salt etherifying agent to the activated starch solution obtained in step (12), reacting the mixture at 70° C. for 3 h, and then filtering the mixture to obtain modified starch solid particles, drying and grinding the modified starch solid particles for later use;

[0102] The quaternary ammonium salt etherifying agent added in step (13) is 3-chloro-2-hydroxypropyltriethylammonium chloride;

[0103] In step (13), the amount of the quaternary ammonium salt etherifying agent added is 50% of the mass of the starch dry powder;

[0104] (2) Preparation of modified bentonite

[0105] (21) adding bentonite to water to prepare bentonite slurry;

[0106] The concentration of the bentonite slurry in step (21) is 45%wt;

[0107] (22) adding an acidifying modifier, citric acid, to the bentonite slurry prepared in step (21), and reacting at 65° C. for 6 h, then adding a sodium modifying agent, Na2CO3, and reacting at a sodium modifying temperature of 80° C. for 3 h, and then filtering to obtain modified bentonite solid particles, and drying and grinding the modified bentonite solid particles for later use;

[0108] (3) Preparation of modified chitosan

[0109] (31) adding an acid solution to chitosan, and adding a NaOH solution to adjust the pH to 5, then dropping a protective agent, and reacting at 60 °C for 3 h to prepare a chitosan Schiff base;

[0110] In step (31), the acid solution is acetic acid, the amount of which is 2% of the mass of chitosan, and the concentration of the acetic acid solution is 0.1 mol / L;

[0111] In the step (31), the protective agent is glyoxal;

[0112] (32) mixing the chitosan Schiff base obtained in step (31) with tannin, adding water to prepare a mixed solution, adding NaOH solution to adjust the pH to 5, adding a cross-linking agent, reacting at 60° C. for 3 h, and then filtering to obtain modified chitosan solid particles, and drying and grinding the modified chitosan solid particles for later use;

[0113] In step (32), the cross-linking agent is glyoxal;

[0114] In the step (32), the mass ratio of chitosan Schiff base to tannin is 1:5.

[0115] In the step (32), the mass concentration of chitosan Schiff base in the mixed solution of chitosan Schiff base and tannin is 5%.

[0116] (4) Preparation of flocculants by compounding modified starch, modified bentonite and modified chitosan

[0117] The modified starch, modified bentonite and modified chitosan prepared in steps (1), (2) and (3) are uniformly mixed in a mass ratio of 1:0.7:0.4, and sodium trichloroisocyanurate and aluminum hydroxide are added and mixed uniformly, wherein the amount of sodium trichloroisocyanurate added is 4% of the total mass of the modified starch, modified bentonite and modified chitosan, and the amount of aluminum hydroxide added is 7% of the total mass of the modified starch, modified bentonite and modified chitosan. The above components are stirred and mixed uniformly at room temperature to obtain a flocculant.

[0118] Example 4

[0119] This embodiment provides a method for preparing a powder flocculant for treating oily wastewater at an emergency accident site, comprising the following steps:

[0120] (1) Preparation of modified starch

[0121] (11) taking a certain amount of starch, adding isopropanol to prepare a starch solution;

[0122] In step (11), the starch is sweet potato starch;

[0123] The concentration of the starch solution in step (11) is 30%wt.

[0124] (12) adding NaOH solution to the starch solution prepared in step (11) while stirring, adjusting the pH value to 9.5, and stirring and activating for 30 minutes to obtain an activated starch solution;

[0125] The concentration of the NaOH solution in step (12) is 15%wt;

[0126] (13) adding a quaternary ammonium salt etherifying agent to the activated starch solution obtained in step (12), reacting the mixture at 70° C. for 3 h, and then filtering the mixture to obtain modified starch solid particles, drying and grinding the modified starch solid particles for later use;

[0127] The quaternary ammonium salt etherifying agent added in step (13) is 3-chloro-2-hydroxypropyltriethylammonium chloride;

[0128] In step (13), the amount of the quaternary ammonium salt etherifying agent added is 50% of the mass of the starch dry powder;

[0129] (2) Preparation of modified bentonite

[0130] (21) adding bentonite to water to prepare bentonite slurry;

[0131] The concentration of the bentonite slurry in step (21) is 45%wt;

[0132] (22) adding an acidifying modifier, citric acid, to the bentonite slurry prepared in step (21), and reacting at 65° C. for 6 h, then adding a sodium modifier, NaHCO3, and reacting at a sodium temperature of 60° C. for 3 h, and then filtering to obtain modified bentonite solid particles, and drying and grinding the modified bentonite solid particles for later use;

[0133] (3) Preparation of modified chitosan

[0134] (31) adding an acid solution to chitosan, and adding a NaOH solution to adjust the pH to 5, then dropping a protective agent, and reacting at 60 °C for 3 h to prepare a chitosan Schiff base;

[0135] In step (31), the acid solution is acetic acid, the amount of which is 2% of the mass of chitosan, and the concentration of the acetic acid solution is 0.1 mol / L;

[0136] In the step (31), the protective agent is glyoxal;

[0137] (32) mixing the chitosan Schiff base obtained in step (31) with tannin, adding water to prepare a mixed solution, adding NaOH solution to adjust the pH to 5, adding a cross-linking agent, reacting at 60° C. for 3 h, and then filtering to obtain modified chitosan solid particles, and drying and grinding the modified chitosan solid particles for later use;

[0138] In step (32), the cross-linking agent is glyoxal;

[0139] In the step (32), the mass ratio of chitosan Schiff base to tannin is 1:5.

[0140] In the step (32), the mass concentration of chitosan Schiff base in the mixed solution of chitosan Schiff base and tannin is 5%.

[0141] (4) Preparation of flocculants by compounding modified starch, modified bentonite and modified chitosan

[0142] The modified starch, modified bentonite and modified chitosan prepared in steps (1), (2) and (3) are uniformly mixed in a mass ratio of 1:0.7:0.4, and sodium trichloroisocyanurate and aluminum hydroxide are added and mixed uniformly, wherein the amount of sodium trichloroisocyanurate added is 4% of the total mass of the modified starch, modified bentonite and modified chitosan, and the amount of aluminum hydroxide added is 7% of the total mass of the modified starch, modified bentonite and modified chitosan. The above components are stirred and mixed uniformly at room temperature to obtain a flocculant.

[0143] Example 5

[0144] This embodiment provides a method for preparing a powder flocculant for treating oily wastewater at an emergency accident site, comprising the following steps:

[0145] (1) Preparation of modified starch

[0146] (11) taking a certain amount of starch, adding isopropanol to prepare a starch solution;

[0147] In step (11), the starch is sweet potato starch;

[0148] The concentration of the starch solution in step (11) is 30%wt.

[0149] (12) adding NaOH solution to the starch solution prepared in step (11) while stirring, adjusting the pH value to 9.5, and stirring and activating for 30 minutes to obtain an activated starch solution;

[0150] The concentration of the NaOH solution in step (12) is 15%wt;

[0151] (13) adding a quaternary ammonium salt etherifying agent to the activated starch solution obtained in step (12), reacting the mixture at 70° C. for 3 h, and then filtering the mixture to obtain modified starch solid particles, drying and grinding the modified starch solid particles for later use;

[0152] The quaternary ammonium salt etherifying agent added in step (13) is 3-chloro-2-hydroxypropyltriethylammonium chloride;

[0153] In step (13), the amount of the quaternary ammonium salt etherifying agent added is 50% of the mass of the starch dry powder;

[0154] (2) Preparation of modified bentonite

[0155] (21) adding bentonite to water to prepare bentonite slurry;

[0156] The concentration of the bentonite slurry in step (21) is 45%wt;

[0157] (22) adding an acidifying modifier, citric acid, to the bentonite slurry prepared in step (21), and reacting at 65° C. for 6 h, then adding a sodium modifying agent, Na2CO3, and reacting at a sodium modifying temperature of 80° C. for 3 h, and then filtering to obtain modified bentonite solid particles, and drying and grinding the modified bentonite solid particles for later use;

[0158] (3) Preparation of modified chitosan

[0159] (31) adding an acid solution to chitosan, and adding a NaOH solution to adjust the pH to 5, then dropping a protective agent, and reacting at 60 °C for 3 h to prepare a chitosan Schiff base;

[0160] In step (31), the acid solution is acetic acid, the amount of which is 2% of the mass of chitosan, and the concentration of the acetic acid solution is 0.1 mol / L;

[0161] In the step (31), the protective agent is glyoxal;

[0162] (32) mixing the chitosan Schiff base obtained in step (31) with tannin, adding water to prepare a mixed solution, adding NaOH solution to adjust the pH to 5, adding a cross-linking agent, reacting at 60° C. for 3 h, and then filtering to obtain modified chitosan solid particles, and drying and grinding the modified chitosan solid particles for later use;

[0163] In step (32), the cross-linking agent is glyoxal;

[0164] In the step (32), the mass ratio of chitosan Schiff base to tannin is 1:5.

[0165] In the step (32), the mass concentration of chitosan Schiff base in the mixed solution of chitosan Schiff base and tannin is 5%.

[0166] (4) Preparation of flocculants by compounding modified starch, modified bentonite and modified chitosan

[0167] The modified starch, modified bentonite and modified chitosan prepared in steps (1), (2) and (3) are uniformly mixed in a mass ratio of 1:0.7:0.4, and sodium trichloroisocyanurate and aluminum hydroxide are added and mixed uniformly, wherein the amount of sodium trichloroisocyanurate added is 5% of the total mass of the modified starch, modified bentonite and modified chitosan, and the amount of aluminum hydroxide added is 8% of the total mass of the modified starch, modified bentonite and modified chitosan. The above components are stirred and mixed uniformly at room temperature to obtain a flocculant.

[0168] Example 6

[0169] This embodiment provides a method for preparing a powder flocculant for treating oily wastewater at an emergency accident site, comprising the following steps:

[0170] (1) Preparation of modified starch

[0171] (11) taking a certain amount of starch, adding isopropanol to prepare a starch solution;

[0172] In step (11), the starch is corn starch;

[0173] The concentration of the corn starch solution in step (11) is 35%wt.

[0174] (12) adding NaOH solution to the starch solution prepared in step (11) while stirring, adjusting the pH value to 9, and stirring and activating for 30 minutes to obtain an activated starch solution;

[0175] The concentration of the NaOH solution in step (12) is 15%wt;

[0176] (13) adding a quaternary ammonium salt etherifying agent to the activated starch solution obtained in step (12), reacting the mixture at 70° C. for 3 h, and then filtering the mixture to obtain modified starch solid particles, drying and grinding the modified starch solid particles for later use;

[0177] The quaternary ammonium salt etherifying agent added in step (13) is 3-chloro-2-hydroxypropyltriethylammonium chloride;

[0178] In step (13), the amount of the quaternary ammonium salt etherifying agent added is 50% of the mass of the starch dry powder;

[0179] (2) Preparation of modified bentonite

[0180] (21) adding bentonite to water to prepare bentonite slurry;

[0181] The concentration of the bentonite slurry in step (21) is 45%wt;

[0182] (22) adding an acidifying modifier, citric acid, to the bentonite slurry prepared in step (21), and reacting at 65° C. for 6 h, then adding a sodium modifying agent, Na2CO3, and reacting at a sodium modifying temperature of 80° C. for 3 h, and then filtering to obtain modified bentonite solid particles, and drying and grinding the modified bentonite solid particles for later use;

[0183] (3) Preparation of modified chitosan

[0184] (31) adding an acid solution to chitosan, and adding a NaOH solution to adjust the pH to 5, then dropping a protective agent, and reacting at 60 °C for 3 h to prepare a chitosan Schiff base;

[0185] In step (31), the acid solution is acetic acid, the amount of which is 2% of the mass of chitosan, and the concentration of the acetic acid solution is 0.1 mol / L;

[0186] In the step (31), the protective agent is glyoxal;

[0187] (32) mixing the chitosan Schiff base obtained in step (31) with tannin, adding water to prepare a mixed solution, adding NaOH solution to adjust the pH to 5, adding a cross-linking agent, reacting at 60° C. for 3 h, and then filtering to obtain modified chitosan solid particles, and drying and grinding the modified chitosan solid particles for later use;

[0188] In step (32), the cross-linking agent is glyoxal;

[0189] In the step (32), the mass ratio of chitosan Schiff base to tannin is 1:6.

[0190] In the step (32), the mass concentration of chitosan Schiff base in the mixed solution of chitosan Schiff base and tannin is 6%.

[0191] (4) Preparation of flocculants by compounding modified starch, modified bentonite and modified chitosan

[0192] The modified starch, modified bentonite and modified chitosan prepared in steps (1), (2) and (3) are uniformly mixed in a mass ratio of 1:0.7:0.4, and sodium trichloroisocyanurate and aluminum hydroxide are added and mixed uniformly, wherein the amount of sodium trichloroisocyanurate added is 4% of the total mass of the modified starch, modified bentonite and modified chitosan, and the amount of aluminum hydroxide added is 7% of the total mass of the modified starch, modified bentonite and modified chitosan. The above components are stirred and mixed uniformly at room temperature to obtain a flocculant.

[0193] Example 7

[0194] This embodiment provides a method for preparing a powder flocculant for treating oily wastewater at an emergency accident site, comprising the following steps:

[0195] (1) Preparation of modified starch

[0196] (11) taking a certain amount of starch, adding isopropanol to prepare a starch solution;

[0197] In step (11), the starch is sweet potato starch;

[0198] The concentration of the starch solution in step (11) is 30%wt.

[0199] (12) adding NaOH solution to the starch solution prepared in step (11) while stirring, adjusting the pH value to 10, and stirring and activating for 30 minutes to obtain an activated starch solution;

[0200] The concentration of the NaOH solution in step (12) is 18%wt;

[0201] (13) adding a quaternary ammonium salt etherifying agent to the activated starch solution obtained in step (12), reacting the mixture at 70° C. for 3 h, and then filtering the mixture to obtain modified starch solid particles, drying and grinding the modified starch solid particles for later use;

[0202] The quaternary ammonium salt etherifying agent added in step (13) is 3-chloro-2-hydroxypropyltriethylammonium chloride;

[0203] In step (13), the amount of the quaternary ammonium salt etherifying agent added is 50% of the mass of the starch dry powder;

[0204] (2) Preparation of modified bentonite

[0205] (21) adding bentonite to water to prepare bentonite slurry;

[0206] The concentration of the bentonite slurry in step (21) is 46%wt;

[0207] (22) adding an acidifying modifier, citric acid, to the bentonite slurry prepared in step (21), and reacting at 65° C. for 6 h, then adding a sodium modifying agent, Na2CO3, and reacting at a sodium modifying temperature of 85° C. for 3 h, and then filtering to obtain modified bentonite solid particles, and drying and grinding the modified bentonite solid particles for later use;

[0208] (3) Preparation of modified chitosan

[0209] (31) adding an acid solution to chitosan, and adding a NaOH solution to adjust the pH to 5, then dropping a protective agent, and reacting at 60 °C for 3 h to prepare a chitosan Schiff base;

[0210] In step (31), the acid solution is acetic acid, the amount of which is 3% of the mass of chitosan, and the concentration of the acetic acid solution is 0.1 mol / L;

[0211] In the step (31), the protective agent is glyoxal;

[0212] (32) mixing the chitosan Schiff base obtained in step (31) with tannin, adding water to prepare a mixed solution, adding NaOH solution to adjust the pH to 5, adding a cross-linking agent, reacting at 60° C. for 3 h, and then filtering to obtain modified chitosan solid particles, and drying and grinding the modified chitosan solid particles for later use;

[0213] In step (32), the cross-linking agent is glyoxal;

[0214] In the step (32), the mass ratio of chitosan Schiff base to tannin is 1:6.

[0215] In the step (32), the mass concentration of chitosan Schiff base in the mixed solution of chitosan Schiff base and tannin is 6%.

[0216] (4) Preparation of flocculants by compounding modified starch, modified bentonite and modified chitosan

[0217] The modified starch, modified bentonite and modified chitosan prepared in steps (1), (2) and (3) are uniformly mixed in a mass ratio of 1:0.7:0.5, and sodium trichloroisocyanurate and aluminum hydroxide are added and mixed uniformly, wherein the amount of sodium trichloroisocyanurate added is 5% of the total mass of the modified starch, modified bentonite and modified chitosan, and the amount of aluminum hydroxide added is 8% of the total mass of the modified starch, modified bentonite and modified chitosan. The above components are stirred and mixed uniformly at room temperature to obtain a flocculant.

[0218] Example 8

[0219] This embodiment provides a method for preparing a powder flocculant for treating oily wastewater at an emergency accident site, comprising the following steps:

[0220] (1) Preparation of modified starch

[0221] (11) taking a certain amount of starch and adding water to prepare a starch solution;

[0222] In step (11), the starch is corn starch;

[0223] The concentration of the corn starch solution in step (11) is 20%wt;

[0224] (12) adding a mixed solution of NaOH and aqueous ammonia to the corn starch solution prepared in step (11) while stirring, adjusting the pH value to 9, and stirring and activating for 25 minutes to obtain an activated corn starch solution;

[0225] The concentration of NaOH and ammonia solution added in step (12) is 10%wt, and the mass ratio of NaOH to ammonia solution is 1:0.1-1;

[0226] (13) adding a quaternary ammonium salt etherifying agent to the activated corn starch solution obtained in step (12), and reacting at 40° C. for 3 h to fully gelatinize the starch particles and increase the substitution effect of the etherification reaction. At the same time, mechanical stirring can be used to improve the gelatinization efficiency. Then, suction filtration is performed to obtain modified corn starch solid particles, and the modified corn starch solid particles are dried and ground for later use;

[0227] The quaternary ammonium salt etherifying agent added in step (13) is 3-chloro-2-hydroxypropyltriethylammonium chloride;

[0228] The amount of the quaternary ammonium salt etherifying agent added in step (13) is 40% of the mass of the corn starch dry powder in step (11);

[0229] (2) Preparation of modified bentonite

[0230] (21) adding bentonite to water to prepare bentonite slurry;

[0231] The concentration of the bentonite slurry in step (21) is 40%wt;

[0232] (22) adding an acidifying modifier, citric acid, to the bentonite slurry prepared in step (21), and reacting at 60° C. for 4 h, then adding a sodium modifier, NaCl, and reacting at 90° C. for 2 h, and then filtering to obtain modified bentonite solid particles, and drying and grinding the modified bentonite solid particles for later use;

[0233] (3) Preparation of modified chitosan

[0234] (31) adding an acid solution to chitosan, and adding a mixed solution of NaOH and ammonia water to adjust the pH to 5, then dropping a protective agent, and reacting at 50 °C for 2 h to prepare a chitosan Schiff base;

[0235] In step (31), the acid solution is acetic acid, the amount of which is 1% of the mass of chitosan, and the concentration of the acetic acid solution is 0.1 mol / L;

[0236] In the step (31), the protective agent is glyoxal;

[0237] (32) mixing the chitosan Schiff base obtained in step (31) with tannin, adding water to prepare a mixed solution, adding a mixed solution of NaOH and ammonia water to adjust the pH to 4, adding a cross-linking agent, reacting at 60° C. for 2 h, and then filtering to obtain modified chitosan solid particles, and drying and grinding the modified chitosan solid particles for later use;

[0238] In step (32), the cross-linking agent is glyoxal;

[0239] In the step (32), the mass ratio of chitosan Schiff base to tannin is 1:5.

[0240] In the step (32), the mass concentration of chitosan Schiff base in the mixed solution of chitosan Schiff base and tannin is 5%;

[0241] (4) Preparation of flocculants by compounding modified starch, modified bentonite and modified chitosan

[0242] The modified starch, modified bentonite and modified chitosan prepared in steps (1), (2) and (3) are uniformly mixed in a mass ratio of 1:0.6:0.5, and sodium trichloroisocyanurate and aluminum hydroxide are added and mixed uniformly, wherein the amount of sodium trichloroisocyanurate added is 2% of the total mass of the modified starch, modified bentonite and modified chitosan, and the amount of aluminum hydroxide added is 10% of the total mass of the modified starch, modified bentonite and modified chitosan. The above components are stirred and mixed uniformly at room temperature to obtain a flocculant.

[0243] Example 9

[0244] This embodiment provides a method for preparing a powder flocculant for treating oily wastewater at an emergency accident site, comprising the following steps:

[0245] (1) Preparation of modified starch

[0246] (11) taking a certain amount of starch, adding isopropanol to prepare a starch solution;

[0247] In step (11), the starch is wheat starch;

[0248] The concentration of the starch solution in step (11) is 35%wt.

[0249] (12) adding NaOH solution to the starch solution prepared in step (11) while stirring, adjusting the pH value to 9.5, and stirring and activating for 30 minutes to obtain an activated starch solution;

[0250] The concentration of the NaOH solution in step (12) is 15%wt;

[0251] (13) adding a quaternary ammonium salt etherifying agent to the activated starch solution obtained in step (12), reacting the mixture at 50° C. for 3 h, and then filtering the mixture to obtain modified starch solid particles, drying and grinding the modified starch solid particles for later use;

[0252] The quaternary ammonium salt etherifying agent added in step (13) is 3-chloro-2-hydroxypropyltriethylammonium chloride;

[0253] In step (13), the amount of the quaternary ammonium salt etherifying agent added is 50% of the mass of the starch dry powder;

[0254] (2) Preparation of modified bentonite

[0255] (21) adding bentonite to water to prepare bentonite slurry;

[0256] The concentration of the bentonite slurry in step (21) is 50%wt;

[0257] (22) adding an acidifying modifier, citric acid, to the bentonite slurry prepared in step (21), and reacting at 65° C. for 6 h, then adding a sodium modifying agent, Na2CO3, and reacting at a sodium modifying temperature of 75° C. for 3 h, and then filtering to obtain modified bentonite solid particles, and drying and grinding the modified bentonite solid particles for later use;

[0258] (3) Preparation of modified chitosan

[0259] (31) adding an acid solution to chitosan, and adding a NaOH solution to adjust the pH to 5, then dropping a protective agent, and reacting at 60 °C for 3 h to prepare a chitosan Schiff base;

[0260] In step (31), the acid solution is acetic acid, the amount of which is 2% of the mass of chitosan, and the concentration of the acetic acid solution is 0.1 mol / L;

[0261] In the step (31), the protective agent is glyoxal;

[0262] (32) mixing the chitosan Schiff base obtained in step (31) with tannin, adding water to prepare a mixed solution, adding NaOH solution to adjust the pH to 5, adding a cross-linking agent, reacting at 60° C. for 3 h, and then filtering to obtain modified chitosan solid particles, and drying and grinding the modified chitosan solid particles for later use;

[0263] In step (32), the cross-linking agent is glyoxal;

[0264] In the step (32), the mass ratio of chitosan Schiff base to tannin is 1:7.

[0265] In the step (32), the mass concentration of chitosan Schiff base in the mixed solution of chitosan Schiff base and tannin is 8%.

[0266] (4) Preparation of flocculants by compounding modified starch, modified bentonite and modified chitosan

[0267] The modified starch, modified bentonite and modified chitosan prepared in steps (1), (2) and (3) are uniformly mixed in a mass ratio of 1:1:0.2, and sodium trichloroisocyanurate and aluminum hydroxide are added and mixed uniformly, wherein the amount of sodium trichloroisocyanurate added is 4% of the total mass of the modified starch, modified bentonite and modified chitosan, and the amount of aluminum hydroxide added is 9% of the total mass of the modified starch, modified bentonite and modified chitosan. The above components are stirred and mixed uniformly at room temperature to obtain a flocculant.

[0268] The flocculant prepared in the above Example 1 was used to treat oily wastewater (oil products in the process of oily wastewater reuse) to test its ability to treat oily wastewater.

[0269] Six portions of the flocculant prepared in Example 1 were added to 1000 ml of oily wastewater, the solid suspended matter concentration in the oily wastewater was 3000 mg / L, the amount of flocculant added was set to 1 g, and the mixture was stirred at stirring rates of 0, 200 r / min, 400 r / min, 600 r / min, 800 r / min, and 1200 r / min, respectively, to study the flocculation time of the flocculant at different stirring rates, as shown in Table 1 and Figure 1 shown.

[0270] Table 1

[0271]

[0272] From the above Table 1 and Figure 1 It can be seen that with the increase of stirring rate, the flocculation time of solid suspended particles in oily wastewater gradually shortens, and when the stirring rate reaches 200-600r / min, the flocculation time is maintained at about 40-60s, and when the stirring rate reaches 800-1200r / min, the flocculation time is maintained at about 25-30s, which can achieve rapid flocculation, thereby realizing efficient emergency disposal of oily wastewater and avoiding secondary pollution.

[0273] In addition, through the study of the flocculation time of the flocculant at different stirring rates, when the flocculant of the present invention is used to treat oily wastewater, a mechanical stirring device can be used to accelerate flocculation, and the stirring rate is preferably 800-1200 r / min.

[0274] In addition, the flocculant prepared in Example 1 was added to the oily wastewater, the initial concentration of suspended solids in the oily wastewater was 3000 mg / L, the stirring rate was set to 800-1200 r / min, and the variation of the suspended solids content in the oily wastewater with the feeding time was studied, as shown in Table 2 and Figure 2 shown.

[0275] Table 2

[0276]

[0277] From the above Table 2 and Figure 2 It can be seen that the content of suspended solids in the oily wastewater decreases gradually with the extension of the feeding time. When it reaches 100s, the content of suspended solids in the oily wastewater is significantly reduced; when it reaches 110-120s, the content of suspended solids in the oily wastewater is basically 0. This shows that the use of the flocculant of the present invention to treat oily wastewater can basically remove the suspended solids in the oily wastewater within 2 minutes, and the flocculation reaction time is short, thereby realizing efficient emergency treatment of oily wastewater.

[0278] It should be noted that some parts not described in the present invention can be implemented by adopting or drawing on existing technologies.

[0279] In addition, the optional embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the embodiments of the present invention are not limited to the specific details in the above embodiments. Within the technical concept of the embodiments of the present invention, the technical scheme of the embodiments of the present invention can be subjected to a variety of simple modifications, and these simple modifications all belong to the protection scope of the embodiments of the present invention. In addition, it should be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the embodiments of the present invention will not further describe various possible combinations.

Claims

1. A method for preparing a powder flocculant for treating oily wastewater at an emergency accident site, characterized in that: The steps include: (1) Preparation of modified starch (11) preparing a starch solution with at least one of water, ethanol or isopropanol; (12) adding an alkaline solution to the starch solution prepared in step (11) while stirring, adjusting the pH value to 9 to 10, and fully stirring and activating for 25 to 30 minutes to obtain an activated starch solution; (13) adding a quaternary ammonium salt etherifying agent to the activated starch solution obtained in step (12), reacting at 40 to 70° C. for 3 to 4 hours, then filtering to obtain modified starch solid particles, and drying and grinding the modified starch solid particles for later use; (2) Preparation of modified bentonite (21) adding bentonite to water to prepare bentonite slurry; (22) adding an acidifying modifier to the bentonite slurry prepared in step (21), and reacting at 60-70° C. for 4-6 hours, and then adding a sodium modifier, and reacting at 55-95° C. for 2-3 hours, and then filtering to obtain modified bentonite solid particles, and drying and grinding the modified bentonite solid particles for later use; (3) Preparation of modified chitosan (31) adding an acid solution to chitosan, and adding an alkaline solution to adjust the pH to 4-6, then dropping a protective agent, and reacting at 50-70° C. for 2-3 h to prepare a chitosan Schiff base; (32) mixing the chitosan Schiff base obtained in step (31) with tannin, adding water to prepare a mixed solution, adding an alkaline solution to adjust the pH to 4-6, adding a cross-linking agent, reacting at 60-80° C. for 2-3 hours, and then filtering to obtain modified chitosan solid particles, and drying and grinding the modified chitosan solid particles for later use; (4) Preparation of flocculants by compounding modified starch, modified bentonite and modified chitosan The modified starch, modified bentonite, modified chitosan prepared in steps (1), (2) and (3) are uniformly mixed with sodium trichloroisocyanurate and aluminum hydroxide to obtain a flocculant.

2. The method for preparing a powder flocculant for treating oily wastewater at an emergency accident site according to claim 1, characterized in that: In the step (11), the starch is at least one of corn starch, wheat starch or sweet potato starch.

3. The method for preparing a powder flocculant for treating oily wastewater at an emergency accident site according to claim 1, characterized in that: The concentration of the starch solution in step (11) is 20-40%wt.

4. The method for preparing a powder flocculant for treating oily wastewater at an emergency accident site according to claim 1, characterized in that: The concentration of the alkaline solution in step (12) is 10-20%wt.

5. The method for preparing a powder flocculant for treating oily wastewater at an emergency accident site according to claim 1, characterized in that: In the step (13), the amount of the quaternary ammonium salt etherifying agent added is 40-60% of the mass of the starch dry powder.

6. The method for preparing a powder flocculant for treating oily wastewater at an emergency accident site according to claim 1, characterized in that: In the step (13), the quaternary ammonium salt etherifying agent is 3-chloro-2-hydroxypropyltriethylammonium chloride.

7. The method for preparing a powder flocculant for treating oily wastewater at an emergency accident site according to claim 1, characterized in that: The concentration of the bentonite slurry in the step (21) is 40-50%wt.

8. The method for preparing a powder flocculant for treating oily wastewater at an emergency accident site according to claim 1, characterized in that: In the step (22), the acidifying modifier is citric acid.

9. The method for preparing a powder flocculant for treating oily wastewater at an emergency accident site according to claim 1, characterized in that: In the step (22), the sodium-modifying agent is at least one of NaCl, CH3COONa, Na2CO3, and NaHCO3.

10. The method for preparing a powder flocculant for treating oily wastewater at an emergency accident site according to claim 1, characterized in that: In the step (31), the amount of the acid solution added is 1-3% of the mass of the chitosan, and the concentration of the acid solution is 0.05-0.5 mol / L.

11. The method for preparing a powder flocculant for treating oily wastewater at an emergency accident site according to claim 1, characterized in that: The protective agent in step (31) is glyoxal or formaldehyde, and the cross-linking agent in step (32) is glyoxal.

12. The method for preparing a powder flocculant for treating oily wastewater at an emergency accident site according to claim 1, characterized in that: The mass ratio of chitosan Schiff base to tannin in the step (32) is 1:5-10, and the mass concentration of chitosan Schiff base in the mixed solution of chitosan Schiff base and tannin in the step (32) is 5-10%.

13. The method for preparing a powder flocculant for treating oily wastewater at an emergency accident site according to claim 1, characterized in that: In the step (4), the mass ratio of the modified starch, the modified bentonite and the modified chitosan is 1:0.5 to 1:0.2 to 0.7, the amount of sodium trichloroisocyanurate added is 2 to 6% of the total mass of the modified starch, the modified bentonite and the modified chitosan, and the amount of aluminum hydroxide added is 5 to 10% of the total mass of the modified starch, the modified bentonite and the modified chitosan.

14. The method for preparing a powder flocculant for treating oily wastewater at an emergency accident site according to claim 1, characterized in that: In the step (4), the mass ratio of modified starch, modified bentonite and modified chitosan is 1:0.6-0.8:0.3-0.

5.

15. A powder flocculant for treating oily wastewater at an emergency accident site, which is prepared by the preparation method according to any one of claims 1 to 14.

Citation Information

Patent Citations

  • Method for preparing reagent for removing printing and dyeing waste water COD (Chemical Oxygen Demand) and chroma

    CN102309953A

  • Material for adsorbing tannin coupled on surface of non-woven fabric and preparation method of material

    CN103233362A

  • Cationic starch flocculating agent and preparation method thereof

    CN104193837A

  • Xanthated chitosan and preparation method thereof

    CN106824119A

  • Sewage treatment agent and preparation method and applications thereof

    CN110563162A

Cited By

  • Polymeric coagulant as well as preparation method and application thereof

    CN119461609A