Ultrahigh-shock-strength steel bar with ultra-fine grain structure and preparation method of ultrahigh-shock-strength steel bar
By controlling chemical composition and process flow, high-strength steel bars with fine grain structure are formed, which solves the problem of difficult to achieve yield strength and strong yield ratio in the prior art, and achieves efficient seismic resistance and economic benefits.
Patent Information
- Application Number
- CN202411473333.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-22
- Publication Date
- 2024-11-26
AI Technical Summary
The existing high-strength straight bar steel bars are difficult to meet the requirements of yield strength ≥650MPa and strong yield ratio, and their ferrite grain structure is difficult to meet the requirements of fine grain structure above level 10.0, and cannot meet the requirements of building seismic performance.
By controlling the ratio of chemical components such as C, Si, Mn, V, Nb, combined with nitrogen argon blowing, refining, continuous casting, heating and rolling, a uniform ferrite + pearlite metallographic structure is formed to ensure the yield of the steel bars. The strength, tensile strength and grain size meet the target requirements.
The high yield strength, tensile strength and high yield ratio of steel bars are achieved, which meets the indicators of seismic performance of buildings, while reducing production costs and improving economic benefits.
Smart Images

Figure CN119020696A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of steel materials, and in particular to an ultra-high seismic strength steel bar with an extremely fine grain structure and a preparation method thereof. The steel bar produced by the method of the present invention has a ferrite grain size of ≥10.0 level, a yield strength of ≥650MPa, a tensile strength-yield ratio of ≥820MPa, a strength-yield ratio of ≥1.26, and a maximum force total elongation of ≥10.0%. Background Art
[0002] Ultra-high seismic strength steel bars are the main reinforcement materials for reinforced concrete building structures. They carry various loads such as tensile and compressive stresses and strains, steel bar reprocessing effects (welding, mechanical connection, bending or straightening) in the structure and are widely used. High-strength seismic steel bars with diameters of Φ12 to 32 mm and yield strength ≥650 MPa have begun to be used in coastal cities and are gradually being used in inland provinces and cities such as Shaanxi and Anhui.
[0003] Reducing steel consumption is one way to reduce carbon emissions. As the strength of steel bars increases, the number and weight of steel bars used per unit area in building design will be reduced accordingly, which is conducive to the lightweight and diversified design of building structures; at the same time, in order to meet the requirements of building seismic performance, while the yield strength is increased, the tensile strength must also be increased to meet the seismic performance index of strength-to-yield ratio ≥ 1.25. As we all know, with the increase in the yield strength of steel bars, the increase in tensile strength is not linearly proportional to the increase in yield strength, which makes it difficult to achieve the strength-to-yield ratio requirements of high-strength steel bars. At present, vanadium is widely used in the market to ensure that the performance of steel bars meets the requirements, but the ferrite grain structure of straight steel bars is difficult to meet the fine grain structure requirements of grade 10.0 or above.
[0004] Therefore, how to solve the strength-to-yield ratio of ultra-high strength straight steel bars and the uniform and fine grain structure is a technical problem that needs to be solved urgently in this field. Summary of the invention
[0005] The purpose of the present invention is to provide an ultra-high seismic strength steel bar with an extremely fine grain structure and a preparation method thereof, in order to address the problem that the yield strength of the currently available high-strength seismic resistant steel bars is difficult to reach 650MPa, and it is difficult to meet the strength-to-yield ratio requirements. In addition, the ferrite grain structure of the straight steel bars is difficult to reach level 10.0 or above, and the fine grain requirements cannot be met.
[0006] The invention discloses an ultra-high seismic strength steel bar with an extremely fine grain structure, comprising the following chemical components in percentage by mass: C: 0.26-0.28%, Si: 0.50-0.70%, Mn: 1.50-1.60%, S≤0.030%, P≤0.030%, V+Nb: 0.150-0.180%, and the remainder being Fe and unavoidable impurities. In addition, the above components also satisfy the following relationship: (1) 5.0≤V / N≤7.0, (2) 0.55%≤Ceq≤0.58%.
[0007] Preferably, in the present invention, Si: 0.60-0.70%, V+Nb: 0.150-0.170%, (2) 0.56%≤Ceq≤0.58%.
[0008] The finished product diameter of the ultra-high seismic strength steel bar produced by the present invention is 12mm-40mm, and the delivery form is straight steel bar, with yield strength ≥650MPa, tensile strength-yield ratio ≥820MPa, strength-yield ratio ≥1.26, elongation after fracture ≥20%, and total elongation at maximum force ≥10.0%.
[0009] The metallographic structure of the ultra-high earthquake-resistant strength steel bar produced by the invention is uniform ferrite+pearlite, and the ferrite grain size is ≥10.0 grade.
[0010] The method for preparing a super-high seismic strength steel bar with an extremely fine grain structure of the present invention comprises the following steps: smelting in a converter → blowing argon in an argon station → refining → continuous casting → heating of the ingot → rolling → cooling, wherein: (1) Converter smelting: molten iron composition requirements: S < 0.030%, molten iron plus scrap steel weight 150-160 tons, tapping time ≥ 3 minutes, end point C: 0.06% ~ 0.16%, P ≤ 0.028%, alloy is added from 1 / 4 of the tapping, and the alloy is added before 3 / 4 of the tapping; (2) Refining: Blow nitrogen in the refining furnace for 12 to 15 minutes, add active lime and calcium carbide to fine-tune the composition and temperature, strictly control the C, Si, Mn, P, S, Nb, V, and N components during smelting and ensure that Ceq is within the control range. At the same time, strictly control the outlet temperature of molten steel at 1540-1560℃; (3) Continuous casting: The refined molten steel is continuously cast into continuous casting billets through a seven-machine, seven-strand continuous casting machine, and the casting speed is maintained at 3.0 to 3.8 m / s; (4) Billet heating: The preheating temperature of the heating furnace is 900-1080°C, the temperature of the heating section is 1200-1230°C, the temperature of the soaking section is 1200-1230°C, and the total heating time is 90-100 minutes; (5) Rolling: The rolling of the ingot includes rough rolling, intermediate rolling and finish rolling. The billet is rough rolled by 6 rolling mills to obtain rough rolled red steel. The rough rolled red steel is rolled by 4 to 6 rolling mills to obtain intermediate rolled red steel. The intermediate rolled red steel is rolled by 6 rolling mills to obtain finish rolled red steel. The final rolling speed is 6 to 15 m / s. At this time, the size of the finish rolled red steel is the size of the finished steel bar. (6) Cooling: The fine-rolled red steel is passed through a water cooling device, and the temperature of the cooling bed of the fine-rolled red steel that has been sheared to multiple lengths is controlled at 1000-1080°C, and the cooling rate is 2-4°C / S.
[0011] In the above step (1), the alloy comprises vanadium, niobium and a nitriding agent, wherein the vanadium is one or both of vanadium-nitrogen alloy and ferrovanadium, the niobium is one or both of ferroniobium and ferrophosphorus niobium, and the nitriding agent is one or both of ferrosilicon nitride, silicon manganese nitride and ferromanganese nitride.
[0012] Preferably, the pulling speed in the above step (3) is 3.2-3.6 m / s.
[0013] Preferably, the ingot heating step will place the qualified ingot into a regenerative walking beam heating furnace for preheating, heating and equalizing through an intelligent combustion system to ensure uniform temperature along the length of the ingot, and control the temperature difference between the temperature measuring points in the heating section and the equalizing section within 40°C.
[0014] The process principle of the present invention is: by strictly controlling the narrow range of each element of C, Si, Mn, V, Nb and N, the fine grain strengthening and precipitation strengthening effects of V, Nb and N are fully exerted; further, the present invention controls the heating temperature, heating time and upper cooling bed temperature of the steel bar to ensure that the V, Nb and N elements can be fully dissolved into austenite during heating, and then controls the transmission speed of the steel bar during the cooling process to ensure that in the γ / α phase transformation process, the V (N, C) and Nb (N, C) elements can be fully precipitated to exert the precipitation strengthening effect, so that the seismic straight steel bar prepared by the method of the present invention has higher yield strength and tensile strength, high strength-to-yield ratio and uniform and fine ferrite plus pearlite metallographic structure.
[0015] The beneficial effects of the present invention are as follows: The present invention utilizes the solid solution strengthening, fine grain strengthening, and precipitation strengthening effects of elements such as carbon, manganese, silicon, vanadium, niobium, and nitrogen, especially by precisely controlling the range of each element and the vanadium-nitrogen ratio, especially by precisely controlling the vanadium-nitrogen ratio, and then in combination with corresponding heating and temperature control technologies, to form a highly seismic-resistant steel bar production technology that can meet the various index requirements of the 650MPa level by adjusting the chemical composition and rolling process on the basis of ordinary steel bars through hot rolling without heat treatment. The method of the present invention has the technical effect of reducing production costs and greatly improving economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1is a tensile curve diagram of the steel bar prepared in Example 1 of the present invention; Figure 2 is a tensile curve diagram of the steel bar prepared in Example 2 of the present invention; Figure 3 is a tensile curve diagram of the steel bar prepared in Example 3 of the present invention; Figure 4 is a metallographic structure diagram of the steel bar prepared in Example 1 of the present invention; Figure 5 is a metallographic structure diagram of the steel bar prepared in Example 2 of the present invention; Figure 6 3 is the metallographic structure diagram of the steel bar prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0017] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0018] Therefore, the following detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0019] Example 1 The method for preparing a super-high seismic strength steel bar with an extremely fine grain structure in this embodiment comprises converter smelting → argon blowing at an argon station → refining → continuous casting → heating of the ingot → rolling → cooling, wherein: (1) Converter smelting: molten iron composition requirements: S < 0.030%, molten iron plus scrap steel weight 154 tons, tapping time ≥ 3 minutes, end point C: 0.09%, P: 0.025%, alloy is added from 1 / 4 of the tapping, and the alloy is added before 3 / 4 of the tapping; the alloys added in this step include vanadium nitrogen alloy, ferroniobium and silicon manganese nitride; (2) Refining: Blow nitrogen in the refining furnace for 12 minutes, add active lime and calcium carbide to fine-tune the composition and temperature, strictly control the content of each element within the target range during smelting, and control the outlet temperature of molten steel at 1548°C. After refining, the composition of molten steel is as follows: C: 0.26%, Si: 0.60%, Mn: 1.50%, P: 0.022%, S: 0.024%, Nb+V: 0.151%, V / N: 6.15, Ceq: 0.55%, and the balance is Fe and unavoidable impurities; (3) Continuous casting: The refined molten steel is continuously cast into continuous casting billets through a seven-machine, seven-strand continuous casting machine, and the casting speed is maintained at 3.4 m / s; (4) Heating of ingot: the preheating temperature of the heating furnace is not higher than 1080°C, the temperature of the heating section is 1220°C, the temperature of the soaking section is 1215°C, and the total heating time is 95 minutes; the heating furnace is a regenerative walking beam heating furnace; (5) Rolling: The rolling of the ingot includes rough rolling, intermediate rolling and finishing rolling. The billet is subjected to rough rolling by 6 alternating horizontal and vertical rough rolling mills to obtain rough rolled red steel with a diameter of φ70 mm. The rough rolled red steel is rolled by 5 rolling mills to obtain intermediate rolled red steel with a cross-sectional size of 60 mm × 23 mm. The intermediate rolled red steel is rolled by 6 rolling mills to obtain finishing rolled red steel with a diameter of φ12 mm. The final rolling speed is 14.5 m / s. At this time, the size of the finishing rolled red steel is the size of the finished steel bar. (6) Cooling: The fine-rolled red steel is passed through a water cooling device, and the temperature of the cooling bed of the fine-rolled red steel that has been sheared to multiple lengths is controlled at 1050°C, and the cooling rate is 2-4°C / S.
[0020] The mechanical properties of the steel bars prepared in this embodiment are shown in Table 1.
[0021] Example 2 The method for preparing a super-high seismic strength steel bar with an extremely fine grain structure in this embodiment comprises converter smelting → argon blowing at an argon station → refining → continuous casting → heating of the ingot → rolling → cooling, wherein: (1) Converter smelting: molten iron composition requirements: S < 0.030%, molten iron plus scrap steel weight 160 tons, tapping time ≥ 3 minutes, end point C: 0.12%, P: 0.024%, alloy is added from 1 / 4 of the tapping, and the alloy is added before 3 / 4 of the tapping; the alloys added in this step include ferrovanadium, ferroniobium and ferromanganese nitride; (2) Refining: Nitrogen was blown into the refining furnace for 13 minutes, and active lime and calcium carbide were added to fine-tune the composition and temperature. During smelting, the content of each element was strictly controlled within the target range, and the outlet temperature of the molten steel was controlled at 1550°C. At the end of refining, the composition of the molten steel was as follows: C: 0.278%, Si: 0.58%, Mn: 1.52%, P: 0.027%, S: 0.018%, Nb+V: 0.169%, V / N: 6.13, Ceq: 0.576%, and the remainder was Fe and unavoidable impurities; (3) Continuous casting: The refined molten steel is continuously cast into continuous casting billets through a seven-machine, seven-strand continuous casting machine, and the casting speed is maintained at 3.5 m / s; (4) Heating of ingot: the preheating temperature of the heating furnace is not higher than 1080°C, the temperature of the heating section is 1216°C, the temperature of the soaking section is 1206°C, and the total heating time is 93 minutes; the heating furnace is a regenerative walking beam heating furnace; (5) Rolling: The rolling of the ingot includes rough rolling, intermediate rolling and finishing rolling. The billet is subjected to rough rolling by 6 alternating horizontal and vertical rough rolling mills to obtain rough rolled red steel with a diameter of φ91 mm. The rough rolled red steel is rolled by 4 rolling mills to obtain intermediate rolled red steel with a diameter of φ59 mm. The intermediate rolled red steel is rolled by 6 rolling mills to obtain finishing rolled red steel with a diameter of φ25 mm. The final rolling speed is 8.5 m / s. At this time, the size of the finishing rolled red steel is the size of the finished steel bar. (6) Cooling: The fine-rolled red steel is passed through a water cooling device, and the temperature of the cooling bed of the fine-rolled red steel that has been sheared to multiple lengths is controlled at 1050°C, and the cooling rate is 2-4°C / S.
[0022] The mechanical properties of the steel bars prepared in this embodiment are shown in Table 1.
[0023] Example 3 The method for preparing a super-high seismic strength steel bar with an extremely fine grain structure in this embodiment comprises converter smelting → argon blowing at an argon station → refining → continuous casting → heating of the ingot → rolling → cooling, wherein: (1) Converter smelting: molten iron composition requirements: S < 0.030%, molten iron plus scrap steel weight 158 tons, tapping time ≥ 3 minutes, end point C: 0.15%, P: 0.021%, alloy is added from 1 / 4 of the tapping, and the alloy is added before 3 / 4 of the tapping; the alloys added in this step include vanadium nitrogen alloy, phosphorus niobium iron and silicon nitride iron; (2) Refining: Blow nitrogen in the refining furnace for 15 minutes, add active lime and calcium carbide to fine-tune the composition and temperature, strictly control the content of each element within the target range during smelting, and control the outlet temperature of molten steel at 1542°C. After refining, the composition of molten steel is as follows: C: 0.28%, Si: 0.64%, Mn: 1.53%, P: 0.028%, S: 0.029%, Nb+V: 0.165%, V / N: 5.9, Ceq: 0.58%, and the balance is Fe and unavoidable impurities; (3) Continuous casting: The refined molten steel is continuously cast into continuous casting billets through a seven-machine, seven-strand continuous casting machine, and the casting speed is maintained at 3.6 m / s; (4) Heating of ingot: the preheating temperature of the heating furnace is not higher than 1080°C, the temperature of the heating section is 1205°C, the temperature of the soaking section is 1204°C, and the total heating time is 94 minutes; the heating furnace is a regenerative walking beam heating furnace; (5) Rolling: The rolling of the ingot includes rough rolling, intermediate rolling and finishing rolling. The billet is subjected to rough rolling by 6 alternating horizontal and vertical rough rolling mills to obtain rough rolled red steel with a diameter of φ88 mm. The rough rolled red steel is rolled by 2 rolling mills to obtain intermediate rolled red steel with a diameter of φ68 mm. The intermediate rolled red steel is rolled by 6 rolling mills to obtain finishing rolled red steel with a diameter of φ32 mm. The final rolling speed is 9 m / s. At this time, the size of the finishing rolled red steel is the size of the finished steel bar. (6) Cooling: The fine-rolled red steel is passed through a water cooling device, and the temperature of the cooling bed of the fine-rolled red steel that has been sheared to multiple lengths is controlled at 1050°C, and the cooling rate is 2-4°C / S.
[0024] The mechanical properties of the steel bars prepared in this embodiment are shown in Table 1.
[0025] Example 4 The method for preparing a super-high seismic strength steel bar with an extremely fine grain structure in this embodiment comprises converter smelting → argon blowing at an argon station → refining → continuous casting → heating of the ingot → rolling → cooling, wherein: (1) Converter smelting: molten iron composition requirements: S < 0.030%, molten iron plus scrap steel weight 153 tons, tapping time ≥ 3 minutes, end point C: 0.11%, P: 0.026%, alloy is added from 1 / 4 of the tapping, and the alloy is added before 3 / 4 of the tapping; the alloys added in this step include vanadium nitrogen alloy, phosphorus niobium iron and silicon nitride iron; (2) Refining: Blow nitrogen in the refining furnace for 15 minutes, add active lime and calcium carbide to fine-tune the composition and temperature, strictly control the content of each element within the target range during smelting, and control the outlet temperature of molten steel at 1542°C. After refining, the composition of molten steel is as follows: C: 0.28%, Si: 0.64%, Mn: 1.53%, P: 0.028%, S: 0.029%, Nb+V: 0.165%, V / N: 5.9, Ceq: 0.58%, and the balance is Fe and unavoidable impurities; (3) Continuous casting: The refined molten steel is continuously cast into continuous casting billets through a seven-machine, seven-strand continuous casting machine, and the casting speed is maintained at 3.6 m / s; (4) Heating of ingot: the preheating temperature of the heating furnace is not higher than 1080°C, the temperature of the heating section is 1205°C, the temperature of the soaking section is 1204°C, and the total heating time is 94 minutes; the heating furnace is a regenerative walking beam heating furnace; (5) Rolling: The rolling of the cast billet includes rough rolling, intermediate rolling and finishing rolling. The billet is subjected to rough rolling operation by 6 alternating horizontal and vertical rough rolling mills to obtain rough rolled red steel with a diameter of φ75 mm. The rough rolled red steel is rolled by 5 rolling mills to obtain intermediate rolled red steel with a diameter of φ68 mm. The intermediate rolled red steel is rolled by 6 rolling mills to obtain finishing rolled red steel with a diameter of φ18 mm. The final rolling speed is 12 m / s. At this time, the size of the finishing rolled red steel is the size of the finished steel bar. (6) Cooling: The fine-rolled red steel is passed through a water cooling device, and the temperature of the cooling bed of the fine-rolled red steel that has been sheared to multiple lengths is controlled at 1050°C, and the cooling rate is 2-4°C / S.
[0026] The mechanical properties of the steel bars prepared in this embodiment are shown in Table 1.
[0027] Example 5 The method for preparing a super-high seismic strength steel bar with an extremely fine grain structure in this embodiment comprises converter smelting → argon blowing at an argon station → refining → continuous casting → heating of the ingot → rolling → cooling, wherein: (1) Converter smelting: molten iron composition requirements: S < 0.030%, molten iron plus scrap steel weight 158 tons, tapping time ≥ 3 minutes, end point C: 0.08%, P: 0.020%, alloy is added from 1 / 4 of the tapping, and the alloy is added before 3 / 4 of the tapping; the alloys added in this step include vanadium nitrogen alloy, phosphorus niobium iron and silicon nitride iron; (2) Refining: Blow nitrogen in the refining furnace for 15 minutes, add active lime and calcium carbide to fine-tune the composition and temperature, strictly control the content of each element within the target range during smelting, and control the outlet temperature of molten steel at 1542°C. After refining, the composition of molten steel is as follows: C: 0.28%, Si: 0.64%, Mn: 1.53%, P: 0.028%, S: 0.029%, Nb+V: 0.165%, V / N: 5.9, Ceq: 0.58%, and the balance is Fe and unavoidable impurities; (3) Continuous casting: The refined molten steel is continuously cast into continuous casting billets through a seven-machine, seven-strand continuous casting machine, and the casting speed is maintained at 3.6 m / s; (4) Heating of ingot: the preheating temperature of the heating furnace is not higher than 1080°C, the temperature of the heating section is 1205°C, the temperature of the soaking section is 1204°C, and the total heating time is 94 minutes; the heating furnace is a regenerative walking beam heating furnace; (5) Rolling: The rolling of the cast billet includes rough rolling, intermediate rolling and finishing rolling. The billet is subjected to rough rolling operation by 6 alternating horizontal and vertical rough rolling mills to obtain rough rolled red steel with a diameter of φ88 mm. The rough rolled red steel is rolled by 2 rolling mills to obtain intermediate rolled red steel with a diameter of φ68 mm. The intermediate rolled red steel is rolled by 4 rolling mills to obtain finishing rolled red steel with a diameter of φ40 mm. The final rolling speed is 6 m / s. At this time, the size of the finishing rolled red steel is the size of the finished steel bar. (6) Cooling: The fine-rolled red steel is passed through a water cooling device, and the temperature of the cooling bed of the fine-rolled red steel that has been sheared to multiple lengths is controlled at 1050°C, and the cooling rate is 2-4°C / S.
[0028] The mechanical properties of the steel bars prepared in this embodiment are shown in Table 1.
[0029] The mechanical properties of the steel bars prepared in Examples 1 to 5 are tested, and the results are shown in Table 1 below.
[0030] Table 1 List of mechanical properties test results of the steel bars prepared in Examples 1 to 5 of the present invention
[0031] For 650MPa grade high strength earthquake resistant steel bars, the yield strength must be ≥650MPa and the strength-to-yield ratio must be ≥1.25, that is, the ratio of tensile strength to yield strength must be ≥1.25, which requires that while the yield strength is increased by 10MPa, the tensile strength must be increased by at least 12.5MPa to meet the strength-to-yield ratio ≥1.25. At the same time, due to the particularity of the steel bars, the yield strength will tend to decrease with the extension of time, so the yield strength must be guaranteed to be at least 20MPa. It can be seen from Table 1 above that embodiments 1 to 5 of the present invention ensure a suitable V / N ratio, sufficient heating time, and a higher upper cooling bed temperature, and the steel bar yield strength ReL obtained is sufficient compared with the characteristic value of 650MPa, and the tensile strength Rm can also reach more than 840MPa, which can ensure a higher strength-to-yield ratio and better meet the earthquake resistance requirements. At the same time, the elongation after fracture A and the maximum force total elongation Agt are high, and the elongation performance is good.
[0032] The steel bars obtained in the above examples 1 to 3 were tested for mechanical properties, and the tensile curves were as follows: Figure 1-3 shown.
[0033] from Figures 1 to 3 It can be seen that the steel bars produced in Examples 1 to 3 have normal room temperature tensile curves, and the yield platform can be well maintained above a value of 650 and is far away from 650, indicating that the steel bars produced in Examples 1 to 3 have stable mechanical properties such as yield strength, tensile strength, and total elongation at maximum force.
[0034] The tensile curve and performance results show that by blowing nitrogen into the refining furnace, the N (nitrogen) element in the steel bar can be appropriately increased while the C, Si, Mn, V, and Nb elements remain unchanged, thereby obtaining a suitable V / N ratio. A better V / N ratio can promote the V (vanadium) alloy element to combine with nitrogen to form nitrides during the later steel rolling process and exert a precipitation strengthening effect, thereby improving the yield strength; at the same time, when the C, Si, Mn, V, and Nb elements remain unchanged, the appropriate heating time is determined to ensure the complete and uniform solid solution of alloy elements such as Mn, V, and Nb, providing conditions for the subsequent uniform precipitation; according to the action mechanism of C, Si, Mn, V, and Nb elements and the characteristics of the process equipment of the Echeng Iron and Steel Bar Production Line, the appropriate upper cooling bed temperature can ensure the full precipitation of the uniformly dissolved N compounds of micro-alloying elements such as V and Nb, ensuring that the yield strength of the steel bar is ≥650MPa.
[0035] The metallographic structure of the steel bars prepared in Examples 1 to 5 was tested, and the results are shown in Table 2.
[0036] Table 2 List of metallographic structure test results of Examples 1 to 5 of the present invention
[0037] It can be seen from Table 2 above that the steel bars prepared in Examples 1 to 5 of the present invention have a grain size grade of ≥10.0, indicating that the steel bars prepared by the method of the present invention have an extremely fine grain structure.
[0038] Figures 4 to 6 It is the metallographic structure picture of the steel bar obtained by Example 1-3 of the present invention, from Figures 4 to 6 It can be seen that the steel bars prepared in Examples 1 to 3 of the present invention have sufficient VN and NbN precipitation due to the microalloying elements such as V and Nb under the action of N, and the microstructure is uniform ferrite plus pearlite, and the ferrite and pearlite are evenly distributed, and the ferrite grain size is very fine, which fully meets the requirement of ferrite grain size ≥ 9.0 for fine-grained steel bars.
[0039] The above embodiments are only specific examples for explaining the present invention and do not limit the present invention in any form. Any non-substantial changes made by anyone based on the above contents and forms without departing from the protection scope of the claims of the present invention shall be deemed to fall within the protection scope of the claims of the present invention. The present invention is not limited to the above specific implementation examples.
Claims
1. An ultra-high seismic strength steel bar with an extremely fine grain structure, characterized in that The invention comprises the following chemical compositions in percentage by weight: C: 0.26-0.28%, Si: 0.50-0.70%, Mn: 1.50-1.60%, S≤0.030%, P≤0.030%, V+Nb: 0.150-0.180%, and the remainder is Fe and unavoidable impurities. In addition, the above compositions also satisfy the following relationship: (1) 5.0≤V / N≤7.0, (2) 0.55%≤Ceq≤0.58%.
2. The ultra-high seismic strength steel bar with an extremely fine grain structure according to claim 1, characterized in that: The Si is 0.60-0.70%, the V+Nb is 0.150-0.170%, (2) 0.56%≤Ceq≤0.58%.
3. The ultra-high seismic strength steel bar with an extremely fine grain structure according to claim 1 or 2, characterized in that: The finished product diameter of the ultra-high seismic strength steel bar is 12mm~40mm, and the delivery form is straight steel bar, with yield strength ≥650MPa, tensile strength-yield ratio ≥820MPa, strength-yield ratio ≥1.26, elongation after fracture ≥20%, and total elongation at maximum force ≥10.0%.
4. The ultra-high seismic strength steel bar with an extremely fine grain structure according to claim 1 or 2, characterized in that: The metallographic structure of the ultra-high seismic strength steel bar is uniform ferrite+pearlite, and the ferrite grain size is ≥10.0 grade.
5. The method for preparing a steel bar with ultra-high seismic strength having an extremely fine grain structure according to claim 1 or 2, characterized in that The method comprises converter smelting → argon blowing at an argon station → refining → continuous casting → heating of the ingot → rolling → cooling, wherein: (1) Converter smelting: molten iron composition requirements: S < 0.030%, molten iron plus scrap steel weight 150-160 tons, tapping time ≥ 3 minutes, end point C: 0.06% ~ 0.16%, P ≤ 0.028%, alloy is added from 1 / 4 of the tapping, and the alloy is added before 3 / 4 of the tapping; (2) Refining: Blow nitrogen in the refining furnace for 12 to 15 minutes, add active lime and calcium carbide to fine-tune the composition and temperature, strictly control the C, Si, Mn, P, S, Nb, V, and N components during smelting and ensure that Ceq is within the control range. At the same time, strictly control the outlet temperature of molten steel at 1540-1560℃; (3) Continuous casting: The refined molten steel is continuously cast into continuous casting billets through a seven-machine, seven-stream continuous casting machine, and the casting speed is maintained at 3.0 to 3.8 m / s; (4) Billet heating: The preheating temperature of the heating furnace is 900-1080°C, the temperature of the heating section is 1200-1230°C, the temperature of the soaking section is 1200-1230°C, and the total heating time is 90-100 minutes; (5) Rolling: The rolling of the ingot includes rough rolling, intermediate rolling and finish rolling. The billet is rough rolled by 6 rolling mills to obtain rough rolled red steel. The rough rolled red steel is rolled by 4 to 6 rolling mills to obtain intermediate rolled red steel. The intermediate rolled red steel is rolled by 6 rolling mills to obtain finish rolled red steel. The final rolling speed is 6 to 15 m / s. At this time, the size of the finish rolled red steel is the size of the finished steel bar. (6) Cooling: The fine-rolled red steel is passed through a water cooling device, and the temperature of the cooling bed of the fine-rolled red steel that has been sheared to multiple lengths is controlled at 1000-1080°C, and the cooling rate is 2-4°C / S.
6. The method for preparing a steel bar with ultra-high seismic strength and ultra-fine grain structure according to claim 5, characterized in that: In step (1), the alloy includes vanadium, niobium and a nitriding agent, wherein the vanadium is one or both of vanadium-nitrogen alloy and ferrovanadium, the niobium is one or both of ferroniobium and ferrophosphorus niobium, and the nitriding agent is one or both of ferrosilicon nitride, silicon manganese nitride and ferromanganese nitride.
7. The method for preparing a steel bar with ultra-high seismic strength and ultra-fine grain structure according to claim 5, characterized in that: The pulling speed in step (3) is 3.2-3.6 m / s.
8. The method for preparing a steel bar with ultra-high seismic strength and ultra-fine grain structure according to claim 5, characterized in that: The ingot heating step allows the ingot to enter a regenerative walking beam heating furnace after acceptance, and is preheated, heated and evenly heated through an intelligent combustion system to ensure uniform temperature along the length of the ingot, and the temperature difference between the temperature measuring points in the heating section and the evenly heating section in the furnace is controlled within 40°C.
Citation Information
Cited By
Novel high-strength steel bar process control method
CN121250216A
645MPa aseismic steel bar with specification of phi 10-40mm and production method of 645MPa aseismic steel bar
CN121380758A