Lossless protecting and repairing method for wooden roof
Through infrared and ultrasonic detection combined with carbon fiber cloth and epoxy resin repair methods, the problem of low efficiency in detection and repair of wooden roofs is solved, efficient and accurate repair is achieved, and the original style and structural stability of the building are retained.
Patent Information
- Application Number
- CN202411076490.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art is difficult to detect and repair damage to wooden roofs quickly and accurately, especially wooden structures with different degrees of damage, resulting in poor restoration efficiency and effect.
The combination of infrared and ultrasonic non-destructive testing technology is used to determine the damage information, and targeted repairs are combined with carbon fiber cloth, carbon fiber tendons and epoxy resin, including local wood grain cracking repair, insect-boring decaying beam repair, wooden beam head corrosion repair and Beam breaks and cracks are repaired.
Through non-destructive testing technology, the accuracy and efficiency of restoration are improved, the original style and structural stability of the building are retained, and targeted restoration is achieved for different levels of damage.
Smart Images

Figure CN119021500A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a roof repair technology, and in particular to a non-destructive protection and repair method for a wooden roof. Background Art
[0002] Traditional dwellings and historical buildings in Lingnan are mostly wooden-framed gable roofs. Due to weathering and long-term loads, the wood properties of these wooden structures have deteriorated, resulting in various forms of damage such as cracking, decay, and deformation. How to quickly detect and improve the accuracy and scientificity of the detection results during disease investigation, and how to use modern technology combined with traditional craftsmanship to carry out targeted repair technology for different degrees of damage to restore their original functions and appearance are technical challenges that need to be overcome today. Summary of the invention
[0003] The purpose of the present invention is to overcome the deficiencies of the above-mentioned prior art and provide a non-destructive protection and repair method for wooden roofs, so as to selectively repair the roofs according to different degrees of damage.
[0004] To achieve the above object, the technical solution of the present invention is:
[0005] A non-destructive protection and repair method for a wooden roof, comprising:
[0006] Use non-destructive testing to determine roof damage information;
[0007] repairing the damaged roof based on the determined roof damage information;
[0008] The repair is one or more of the following: repair of local cracks along the wood grain of beams / columns, repair of insect-damaged and decayed beams, repair of corrosion of wooden beam heads, repair of broken and cracked beams, and repair of columns.
[0009] Furthermore, the non-destructive testing method is infrared and / or ultrasonic.
[0010] Furthermore, the repair of local cracks along the wood grain of the beam / column includes:
[0011] When the cracks are within 5mm, use epoxy resin putty to seal them tightly, including:
[0012] Mix the epoxy resin and curing agent in the set ratio. After mixing all the ingredients, stir them thoroughly to ensure that the ingredients are evenly distributed to avoid stratification or precipitation.
[0013] Use a scraper or trowel to fill the prepared epoxy resin putty into the gaps in the wooden frame that need to be repaired, and make sure the putty is filled evenly without any voids;
[0014] According to the curing time of epoxy resin putty, wait for it to fully cure. According to the curing time of epoxy resin putty, wait for it to fully cure.
[0015] After curing, use sandpaper or grinding wheel to polish the surface, remove excess putty, make the surface smoother, and clean the polished surface to ensure there is no dust and impurities;
[0016] Finally, check the caulking and surface smoothing to ensure there are no defects or uneven areas.
[0017] Furthermore, the repair of local cracks along the wood grain of the beam / column includes:
[0018] When the crack width is 5 to 10 mm, epoxy resin is used for reinforcement, including:
[0019] Mix epoxy resin and hardener in the following weight ratio: E—epoxy resin: diethylenetriamine: dimethylamine = 100:10:10; then use a stirrer to stir thoroughly to ensure that the mixture is even and there are no bubbles.
[0020] When pouring epoxy resin, do not fill aggregates, and complete the pouring in layers. Each layer should be properly vibrated to make the epoxy resin liquid fill the gaps and bond firmly with the wood components.
[0021] The injected epoxy resin is below the surface of the wood component for an antique treatment.
[0022] Furthermore, the repair of local cracks along the wood grain of the beam / column includes:
[0023] When the crack width is 10-30mm, epoxy resin is used for reinforcement or combined with wood strips for repair, including:
[0024] Mix epoxy resin and hardener in the following weight ratio: E—epoxy resin: diethylenetriamine: dimethylamine = 100:10:10; then use a stirrer to stir thoroughly to ensure that the mixture is even and there are no bubbles.
[0025] Before pouring epoxy resin, the filling wood is processed into wooden strips. The inlay wooden strips are made of old wood with the same material as the wooden component and the same length along the grain. The cross-sectional width of the wooden strips is 2 to 3 mm smaller than the split width of the component.
[0026] Before filling the gap with wooden strips, first pour an appropriate amount of epoxy resin into the gap to wet the connection surface, then place the filling wooden strips in sequence, pour an appropriate amount of epoxy resin again, and knock and vibrate the wooden components appropriately to ensure that the filling wooden strips are fully soaked and wrapped by the epoxy resin and firmly bonded to the wooden components;
[0027] Determine the number of pouring layers according to the splitting depth. The interval between two pouring layers should be appropriate to ensure that the epoxy resin liquid poured in layers can bond together. The construction method of the latter layer is the same as the previous layer. After the last layer is completed, it should be ensured that the epoxy resin covers the inlaid wooden strips and shall not be higher than the surface of the wooden component. After the epoxy resin solidifies, it should be lower than the surface of the wooden component.
[0028] Furthermore, the repair of local cracks along the wood grain of the beam / column includes:
[0029] When the width of the crack is more than 30mm and the depth does not exceed 1 / 4 of the diameter, the crack width is 10 to 30mm, and the full-length wood strips are inserted along the grain to repair it. The beams are also reinforced as follows:
[0030] At the cracked end of the beam, use a scraper or sandpaper to remove the loose wood chips around the crack, then use sandpaper to polish the surface of the beam to remove old paint and surface defects, use a bristle brush to clean the dust on the pasting surface and wipe it with a semi-wet towel to ensure that the crack and pasting surface are clean;
[0031] Use epoxy putty to repair the loose surface after cleaning, grind the repair surface and clean the surface dust;
[0032] Cut appropriate carbon fiber cloth according to the size of the cleaned part. The overlap length of the carbon fiber cloth end should be no less than 30mm and cover it on the cleaned beam surface;
[0033] Apply base resin on the surface of the beam reinforcement part and the carbon fiber cloth pasting surface, and paste the carbon fiber cloth from the bottom of the beam section to the top of the beam surface, leaving the interface at the upper end of the beam section. The carbon fiber cloth should be closely attached to the wood surface, and squeezed tightly with a roller to drive out bubbles;
[0034] After the epoxy resin or other adhesive is fully cured, use sandpaper to polish the surface of the carbon fiber cloth again to make it flush with the wood surface;
[0035] Finally, choose a wood grain paint that matches the color of the wood, and paint and distress it according to the paint's construction requirements.
[0036] Furthermore, the repair of the worm-eaten and decayed beams includes:
[0037] After pest control and disinfection, the corrosion of the beams is evaluated to determine the scope and extent of reinforcement required;
[0038] Before repairing the inside, use a scraper to apply the prepared epoxy resin putty to repair surface cracks and wormholes. For wider cracks, use wooden strips or wood chips to embed them to increase the firmness of the repair. When filling, ensure that the putty is full and even to avoid gaps.
[0039] Locate the rebar placement at a certain length from the edge of the four sides of the beam end section, and use laser equipment to drill holes in the beam along the direction of the beam;
[0040] Carbon fiber reinforcements were implanted at the locations of the laser-punched holes, and steel plates were used at the beginning and end of the beams and the carbon fiber reinforcements were temporarily fastened inside the beams;
[0041] Drill injection holes at locations where injection reinforcement is required;
[0042] Inject the prepared epoxy resin into the wood component from the injection hole to fill it. When liquid overflows, stop the action and wait for solidification. When pouring, fill the carbon fiber reinforcement holes to ensure that the carbon fiber reinforcement is closely connected to the beam structure.
[0043] After the epoxy resin is fully cured in the beam, use sandpaper or other grinding tools to polish the surface of the beam to remove excess resin and uneven parts;
[0044] Carbon fiber cloth is used to wrap both ends of the wooden components for reinforcement;
[0045] Finally, tighten the nuts at both ends of the carbon fiber to ensure that the carbon fiber ribs are effectively stressed.
[0046] Furthermore, the wooden beam head corrosion repair includes:
[0047] Use cutting tools to remove the stress-bearing parts affected by local corrosion;
[0048] Disinfect the cut wood surface and intact parts;
[0049] Take new wood of the same material as the old wood and make the interface of the old wood into a wedge-shaped interface that fits each other, and fit together to form a new beam structure. The interface wedge should be set vertically from top to bottom on the ground;
[0050] Drill holes along the longitudinal direction of the beam at a certain length above and below the edge of the new wood end section along the longitudinal vertical line for embedding carbon fiber reinforcements;
[0051] At several length positions of the end of the old wood inlaid with the new wood, holes are punched up and down along the longitudinal vertical line for embedding the tie rods of the carbon fiber reinforcement. Before drilling, a layer of carbon fiber cloth should be wrapped and reinforced on the surface of the old wood drilling position.
[0052] Continue drilling at the end section of the old wood that is to be inlaid with the new wood, aligning it with the opening of the new wood, until it penetrates to the tie rod hole;
[0053] Before installing the carbon fiber reinforcement, first insert the reinforcement sleeve from the cross-sectional hole at the end of the old wood, and then insert the tie rod into the tie rod hole from top to bottom, so that the tie rod forms a tie with sleeve 1 and sleeve 2 respectively, and the lower end of the tie rod is inserted into the nut for fastening;
[0054] Apply epoxy resin to the joints of new and old wood, and slowly insert the wedge-shaped joint of the new wood into the joint of the old wood from top to bottom, so that the four sides and the internal carbon fiber rib holes are aligned respectively; before the new and old wood are formally connected, a trial installation must be carried out first. During the formal connection, the end of the new wood should be lower than the end of the old wood to avoid epoxy resin from penetrating into the sleeve hole and causing contamination;
[0055] Insert the carbon fiber ribs through the end holes of the new wood and connect them to the sleeves to tighten them;
[0056] The carbon fiber reinforcement implantation hole is filled with epoxy resin, and a steel plate is used at the end, and screws are inserted into the carbon fiber reinforcement head to tighten the carbon fiber reinforcement.
[0057] Furthermore, the beam fracture and crack repair comprises:
[0058] Remove loose wood chips and dust from around the crack to ensure it is clean;
[0059] Reset and straighten the broken and bent beam;
[0060] Carbon fiber cloth is laid along the longitudinal bottom of the beam for reinforcement;
[0061] Carbon fiber cloth is laid in sections along the longitudinal side of the beam for reinforcement;
[0062] Carbon fiber reinforcement is implanted inside;
[0063] Apply distressed treatment to the surface of reinforced wood.
[0064] Furthermore, the reinforcement of laying carbon fiber cloth along the longitudinal bottom of the beam includes: firstly brushing base resin on the cross section of the end of the beam and the longitudinal bottom of the beam, and then pasting the carbon fiber cloth from the cross section of one end of the beam along the longitudinal bottom of the beam to the cross section of the other end of the beam, the carbon fiber cloth should be closely attached to the surface of the wood, and squeezed tightly with a roller to drive out bubbles;
[0065] The reinforcement of laying carbon fiber cloth in sections along the longitudinal side of the beam includes: firstly, segmenting along the longitudinal side of the beam, then brushing base resin according to the segment positioning, and then pasting the carbon fiber cloth from the bottom of the beam section upward along the beam surface, leaving the interface at the upper end of the beam section, the carbon fiber cloth and the wood surface should be closely attached, and squeezed densely with a roller to drive out bubbles; the overlap length of the end of the carbon fiber cloth should be not less than 30mm;
[0066] The internal implantation of carbon fiber reinforcement includes: locating the implantation position at a certain length position of the lower margin edge of the beam end section, using laser equipment to drill holes in the beam along the direction of the beam; implanting the carbon fiber reinforcement at the position drilled by the laser, injecting the prepared epoxy resin into the carbon fiber reinforcement hole to fill it, stopping the action after liquid overflows, and using steel plates at the head and tail ends of the beam to fasten the carbon fiber reinforcement in the beam.
[0067] Furthermore, before repairing the damaged roof, the damaged roof must be cleaned, including:
[0068] First, remove the wood tendons and stubble at the split, and then clean the dust in the split gap;
[0069] First cleaning: Use a bristle brush to clean the dust first. If there are wood tendons or stubble in the gap, use a scraper to remove them and then use a bristle brush to clean them. Finally, use an air pump and a spray gun to blow away the dust in the split gap.
[0070] Second cleaning: before pouring epoxy resin, use a spray gun to spray the cracks in the wood frame again to ensure that the cracks are clean and the epoxy resin is firmly bonded to the wood base.
[0071] Compared with the prior art, the present invention has the following beneficial effects:
[0072] (1) By using the combined nondestructive testing technology of infrared + ultrasonic, the location, path and degree of damage can be quickly and accurately determined, which greatly improves the efficiency and accuracy of repair and provides a scientific basis for in-situ nondestructive repair.
[0073] (2) Carbon fiber cloth + carbon fiber reinforcement + epoxy resin are used to carry out in-situ non-destructive / minimally damaged repairs on wooden components with various defects such as cracks, breaks, and decay, which greatly preserves the original appearance and structural stability of the building. BRIEF DESCRIPTION OF THE DRAWINGS
[0074] Figure 1 A flowchart of a method for non-destructive protection and repair of a roof provided by an embodiment of the present invention;
[0075] Figure 2 Schematic diagram of repair and reinforcement of local cracks along the wood grain of beams / columns;
[0076] Figure 3 for Figure 2 Cross-section at AA;
[0077] Figure 4 This is a schematic diagram of the repair and reinforcement of insect-eaten and decayed beams;
[0078] Figure 5 for Figure 4 Cross-section at BB;
[0079] Figure 6 Schematic diagram of the repair and reinforcement of the corrosion of wooden beam heads;
[0080] Figure 7 for Figure 6 Cross-section at CC;
[0081] Figure 8 for Figure 6 Cross-section at DD;
[0082] Fig. 9 This is a schematic diagram of the repair and reinforcement of broken and cracked beams;
[0083] Fig.10 for Fig. 9 Cross-section at EE;
[0084] Fig.11 Schematic diagram of repair and reinforcement of cracks in the beams at both ends of the column;
[0085] Fig.12 for Fig.11 Cross-sectional view at FF. DETAILED DESCRIPTION
[0086] Example:
[0087] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0088] See also Figure 1 As shown, the non-destructive protection and repair method for a wooden roof provided in this embodiment mainly includes:
[0089] 101. Use non-destructive testing methods to determine roof damage information.
[0090] Specifically, in this step, the combined non-destructive testing method of infrared + ultrasonic waves is used to quickly and accurately determine the location, path and degree of damage of the disease, greatly improving the efficiency and accuracy of the repair, and providing a scientific basis for in-situ non-destructive repair.
[0091] 102. Repair the damaged roof based on the determined roof damage information; the repair is one or more of the following: repair of local cracks along the wood grain of beams / columns, repair of worm-eaten and decayed beams, repair of corrosion on wooden beam heads, repair of broken and cracked beams, and repair of columns, so as to achieve in-situ non-destructive / minimally damaged repair, thereby greatly preserving the original appearance and structural stability of the building.
[0092] In a specific embodiment, the above-mentioned repair method further includes a cleaning step, and before repairing the damaged roof, the damaged roof is cleaned, including:
[0093] First, remove the wood tendons and stubble at the split, and then clean the dust in the split gap.
[0094] The first cleaning: Because the splitting has a certain depth and the irregular shape of the gap, the dust in the gap is extremely difficult to clean. Use a bristle brush to clean the dust first. If there are wood tendons, stubble, etc. in the gap, use a scraper to remove them and then clean them with a bristle brush. Finally, use an air pump with a high-pressure spray gun to blow away the dust in the splitting gap. Use the pressure airflow to remove all the dust in the gap that is not easy to clean.
[0095] Second cleaning: Before pouring epoxy resin, use a high-pressure spray gun to spray the cracks of the wooden frame again to ensure that the cracks are clean and the epoxy resin is firmly bonded to the wood base. After the cracks of the wooden components are cleaned and blown clean, the epoxy resin should be sealed as soon as possible to prevent secondary contamination.
[0096] In this way, the two-pass cleaning ensures that the damaged roof is cleaned while also ensuring that the epoxy resin is firmly bonded to the wood base to prevent secondary contamination.
[0097] In a specific embodiment, the repair of local cracks along the wood grain of the beam / column includes:
[0098] 1) For small and slight cracks (with a crack width of less than 5mm), use epoxy resin putty to seal them tightly, as follows:
[0099] ① The cleaning and dust removal methods for wooden components are the same as the above cleaning steps;
[0100] ② According to the product instructions, mix the epoxy resin and curing agent in a certain proportion. This proportion can be adjusted according to the specific construction requirements and the purpose of the putty. The specific proportion needs to be determined according to the actual situation. After mixing all the ingredients, they need to be fully stirred to ensure that the ingredients are evenly distributed to avoid stratification or precipitation, so as to ensure the quality and performance of the putty;
[0101] ③ Use a scraper or trowel to fill the prepared epoxy resin putty into the gaps of the wooden frame that need to be repaired, and ensure that the putty is filled evenly without any voids;
[0102] ④ Use a trowel to smooth the surface of the putty, making sure it is even with the surrounding substrate surface. Press gently to ensure that the putty is in full contact with the substrate;
[0103] ⑤ According to the curing time of epoxy resin putty, wait for it to completely cure, which usually takes several hours to 24 hours. Avoid contact with moisture and other pollutants during the curing process;
[0104] ⑥After curing, use sandpaper or grinding wheel to polish the surface, remove excess putty, make the surface smoother, clean the polished surface, and ensure there is no dust and impurities;
[0105] ⑦ Finally, check the effects of caulking and surface smoothing to ensure there are no defects or uneven areas.
[0106] 2) If the crack width is 5 to 10 mm, it can be reinforced by injecting epoxy resin as follows:
[0107] ① Cleaning and dust removal methods for wooden components: the cleaning steps mentioned above;
[0108] ② According to the product instructions, mix the epoxy resin and hardener in proportion, usually the ratio of E-epoxy resin: diethylenetriamine: dimethylamine = 100:10:10 (weight ratio), use a stirrer to stir thoroughly to ensure uniform mixing without bubbles;
[0109] ③ When pouring epoxy resin, no wooden strips are needed (no aggregate filling), but if the split is deep, the pouring should be completed in layers (times), and the interval time should be controlled;
[0110] ④ Each layer (time) of pouring should be properly knocked and vibrated to make the epoxy resin liquid fill the gaps densely and firmly bonded with the wood components;
[0111] ⑤ After injection, the epoxy resin is 2 to 3 mm below the surface of the wooden component for aging treatment.
[0112] 3) If the crack width is 10-30mm, it can be reinforced by injecting epoxy resin or combined with wood strip gluing and repair. The operation method of wood strip gluing and repair is similar to the digging and patching method. The new and old wood should also be treated with antiseptic treatment. The details are as follows:
[0113] ① Cleaning and dust removal methods for wooden components: the cleaning steps mentioned above;
[0114] ② According to the product instructions, mix the epoxy resin and hardener in proportion, usually the ratio of E-epoxy resin: diethylenetriamine: dimethylamine = 100:10:10 (weight ratio), and ensure that the mixture is even and free of bubbles;
[0115] ③ Before pouring epoxy resin, the filling wood should be processed into wooden strips. The inlay wooden strips should be made of old wood with the same material and the same length along the grain as the wooden components. The cross-sectional width of the wooden strips should be 2 to 3 mm smaller than the split width of the components.
[0116] ④ Before filling the gap with wooden strips, first pour an appropriate amount of epoxy resin into the gap to wet the connection surface, then place the filling wooden strips in sequence, pour an appropriate amount of epoxy resin again, and knock and vibrate the wooden components appropriately to ensure that the filling wooden strips are fully soaked and wrapped by the epoxy resin and firmly bonded to the wooden components;
[0117] ⑤ If the splitting depth is large, the filling and filling of wood strips should be carried out in layers. The number of layers should be determined according to the splitting depth during construction, and the layer thickness should be controlled at about 25mm;
[0118] ⑥ The interval time between the two layers of pouring should be appropriate to ensure that the epoxy resin liquid poured in layers can be bonded together. The interval time between the layered pouring should be comprehensively controlled based on factors such as temperature, wind speed, and mix test records.
[0119] ⑦ The construction method of the last layer is the same as the previous layer. After the last layer is completed, the epoxy resin should cover the inlaid wood strips and should not be higher than the surface of the wood components. After the epoxy resin solidifies, it should be 3 to 4 mm lower than the surface of the wood components to facilitate the aging treatment;
[0120] ⑧During the interval between each layer of pouring, it is necessary to prevent dust and rain. It can be covered, but ventilation must be ensured to facilitate the curing and strength increase of the epoxy resin.
[0121] 4) If the crack width is more than 30mm and the depth does not exceed 1 / 4 of the diameter, after repairing the crack with a full-length wooden strip in the same direction as the crack width of 10 to 30mm, the beam should also be reinforced. Figure 2-3 As shown, the details are as follows:
[0122] ① At the cracked end of beam / column 1, use a scraper or sandpaper to remove the loose wood chips around the crack 3, then use sandpaper to polish the surface of the beam to remove old paint and surface defects, use a bristle brush to clean the dust on the pasting surface and wipe it with a semi-wet towel to ensure that the crack and pasting surface are clean;
[0123] ② Use epoxy putty to repair the loose surface after cleaning, polish the repair surface and clean the surface dust;
[0124] ③ Cut appropriate carbon fiber cloth (usually 5-10mm) according to the size of the cleaned part to prevent carbonization or corrosion of the wood pasting part after a long time, which will affect the reinforcement strength of carbon fiber cloth 2. The overlap length of the carbon fiber cloth end should be no less than 30mm, covering the cleaned beam surface. The carbon fiber cloth can provide additional tensile strength to help repair cracks;
[0125] ④ Apply base resin on the surface of the beam reinforcement part and the carbon fiber cloth pasting surface, and paste the carbon fiber cloth from the bottom of the beam section to the top of the beam surface, leaving the interface at the upper end of the beam section. The carbon fiber cloth should be closely attached to the wood surface, and squeezed tightly with a roller to drive out bubbles;
[0126] ⑤ After the epoxy resin or other adhesive is fully cured, use sandpaper to polish the surface of the carbon fiber cloth again to make it flush with the wood surface;
[0127] ⑥ In order to avoid the invasion of harmful substances and cause damage to wooden components and extend their service life, finally choose wood grain paint that matches the color of the wood, and paint and age it according to the construction requirements of the paint.
[0128] After being infested by insects, the outer skin is often intact, but the interior is hollow, or due to improper selection during the original construction, the heart rot wood is used, and after a long time, the internal decay of the column will occur. Such wooden components with basically intact outer skin can generally be reinforced by chemical methods. For this reason, in a specific embodiment, if Figure 4-5 As shown, the worm-eaten decayed beam repair includes:
[0129] ① After pest control and disinfection, first conduct a detailed assessment of the corrosion of the wooden beam 4 to determine the scope and degree of reinforcement required.
[0130] ② Before repairing the inside, use a scraper to apply the prepared epoxy resin 5 putty to repair surface cracks and worm holes. For wider cracks, you can use small wooden strips or wood chips to embed them to increase the firmness of the repair. When filling, make sure the putty is full and even to avoid gaps.
[0131] ③ Locate the positions of 4 embedded rebars at about 30mm from the edges of the four sides of the beam end section, and use laser equipment to drill holes in the direction of the beam.
[0132] ④ Implant the carbon fiber ribs 6 into the laser-punched positions, and use steel plates 8 at the head and tail ends of the beam to temporarily fasten the carbon fiber ribs 6 inside the beam.
[0133] ⑤ Use a small electric drill to drill holes at locations that require injection and reinforcement.
[0134] ⑥ Use low-pressure pouring to inject the prepared epoxy resin into the wood component from the pouring hole to fill it. When liquid overflows, stop the action and wait for solidification. When pouring, fill the carbon fiber reinforcement holes to ensure that the carbon fiber reinforcement is closely connected to the structure of the wood beam. The prepared epoxy resin should be used up within two hours.
[0135] ⑦ After 72 hours of pouring, when the epoxy resin is fully cured in the beam, use sandpaper or other grinding tools to polish the surface of the beam to remove excess resin and uneven parts.
[0136] ⑧ Carbon fiber cloth 2 is used to wrap the two ends of the wooden component for reinforcement.
[0137] ⑨Finally, tighten the nuts 7 at both ends of the carbon fiber ribs 6 to ensure that the carbon fiber ribs 6 are effectively stressed.
[0138] In this way, the insect-eaten and decayed beams can be repaired in situ without damage or with minimal damage through the method of carbon fiber cloth + carbon fiber reinforcement + epoxy resin, which greatly preserves the original appearance and structural stability of the building.
[0139] The beam head supports of the wooden roof frame are buried in the wall part, exposed to the outdoors, and usually not ventilated. They are not easy to dry due to moisture and are prone to decay due to moisture. In addition, some roofs have poor drainage, which causes leakage and increases the moisture of the wall, which aggravates the decay of the beam head. For the beam heads that are not deeply or internally decayed, first remove and plan the decayed part of the beam head, and disinfect it to prevent further growth of bacteria or fungi. Use wooden boards to wrap, glue, and nail according to the size of the beam head, and finally fill the beam head panel. During the whole process, the new and old wood should be treated with anti-corrosion as required. When local corrosion is serious and affects the force, the decayed beam head + carbon fiber rib internal tie reinforcement measures can be adopted. For this reason, in a specific embodiment, Figure 6-8 As shown, the wooden beam head corrosion repair specifically includes the following steps:
[0140] ① Use cutting tools to remove the parts that are severely corroded and affect the load-bearing parts.
[0141] ② Disinfect the cut wood surface and intact parts to prevent further growth of bacteria or fungi.
[0142] ③ Take new wood 10 of the same material as the old wood 9 and make wedge-shaped interfaces with the old wood to fit each other, and fit together to form a new beam structure. The interface wedge should be set vertically from top to bottom on the ground. In this way, the rotten beam head can be restored to look like new.
[0143] ④ Use a laser drill to drill holes along the longitudinal direction of the beam at 30 to 50 mm above and below the edge of the new wood end section along the longitudinal vertical line for embedding carbon fiber reinforcement 6.
[0144] ⑤ Use a laser drill to drill holes up and down along the longitudinal vertical line at 300-500mm from the end of the old wood inlaid with the new wood for embedding the tie rod of the carbon fiber rib 6. Before drilling, a layer of carbon fiber cloth 2 should be wrapped and reinforced on the surface of the old wood drilling position.
[0145] ⑥ Use a laser drill to align the end section of the old wood that is inlaid with the new wood with the opening position of the new wood and continue drilling until it penetrates the tie rod hole.
[0146] ⑦ Before installing the carbon fiber reinforcement 6, first insert the reinforcement sleeve from the cross-sectional hole at the end of the old wood, and then insert the pull rod 12 into the pull rod hole from top to bottom, so that the pull rod forms a tie with the two metal sleeves 11 in turn, and the nut is inserted into the lower end of the pull rod to tighten it.
[0147] ⑧Apply epoxy resin to the joints of new and old wood, and slowly place the wedge-shaped joint of the new wood into the joint of the old wood from top to bottom, so that the four sides and the internal carbon fiber rib holes are aligned respectively; a trial installation must be carried out before the new and old wood are formally connected. During the formal connection, the new wood end should be lower than the old wood end to avoid epoxy resin infiltration into the sleeve hole and cause contamination.
[0148] ⑨ Insert the carbon fiber rib 6 through the end hole of the new wood and connect and fasten it with the metal sleeve 11.
[0149] ⑩ Use low-pressure perfusion to fill the carbon fiber reinforcement implantation hole with epoxy resin 5, and use a steel plate 8 at the end, and insert a nut 7 into the head of the carbon fiber reinforcement 6 to tighten the carbon fiber reinforcement 6.
[0150] In this way, by repairing the old wood and forming a new beam structure + carbon fiber cloth + carbon fiber reinforcement + epoxy resin + metal sleeve, the corrosion of the wooden beam head can be repaired in situ without damage / minimal damage, which greatly preserves the original appearance and structural stability of the building.
[0151] In a specific embodiment, if Figure 9-10 The beam fracture repair includes the following steps:
[0152] ① Use a scraper or sandpaper to remove loose wood chips and dust around the crack 3 to ensure that the crack is clean.
[0153] ② Reset and straighten the broken and bent beam.
[0154] ③ Lay carbon fiber cloth 2 along the longitudinal bottom of the beam for reinforcement: First, apply base resin on the cross section of the beam end and the longitudinal bottom of the beam, and then paste the carbon fiber cloth 2 from the cross section of one end of the beam along the longitudinal bottom of the beam to the cross section of the other end of the beam. The carbon fiber cloth 2 should fit tightly with the surface of the wood, and squeeze it tightly with a roller to drive out bubbles.
[0155] ④Lay carbon fiber cloth along the longitudinal side of the beam in sections, each section is about 300-500mm: First, divide the beam into sections, then apply base resin according to the section positioning, and then paste carbon fiber cloth 2 from the bottom of the beam section along the beam surface, leaving the interface at the upper end of the beam section. The carbon fiber cloth should be closely attached to the wood surface, and squeezed with a roller to drive out bubbles. To prevent carbonization or corrosion of the wood pasting area after a long time, affecting the reinforcement strength of the carbon fiber cloth, the overlap length of the carbon fiber cloth end should be no less than 30mm.
[0156] ⑤ Internal implantation of carbon fiber ribs 6 for reinforcement: Locate 2 implantation positions at about 30mm from the edge of the lower margin of the beam end section, and use laser equipment to drill holes in the beam along the direction of the beam. Secondly, implant the carbon fiber ribs into the laser-drilled positions, and use low-pressure perfusion to inject the prepared epoxy resin into the carbon fiber rib holes to fill them. Stop the action when liquid overflows, and use steel plates 8 and nuts 7 at the head and tail ends of the beam to fasten the carbon fiber ribs 6 in the beam.
[0157] ⑥ Give the reinforced wood surface an antique treatment.
[0158] In a specific embodiment, if Figure 11-12 As shown, the repair of cracks in the beams at both ends of the column (melon column) is similar to the repair of cracks in the beams mentioned above.
[0159] In summary, the present invention uses a combination of infrared + ultrasonic non-destructive testing technology to quickly and accurately determine the location, path and degree of damage, greatly improving the efficiency and accuracy of repair, and providing a scientific basis for in-situ non-destructive repair. Modern technologies such as carbon fiber cloth + carbon fiber tendons + epoxy resin + traditional processes are used to implement in-situ non-destructive / minor-damage repair of cracked, broken, decayed and other wood components with different diseases, which greatly preserves the original appearance and structural stability of the building. Through the analysis of the diseases of wooden components and combined with the "repair the old as it is old" restoration concept, special in-situ non-destructive / minor-damage repair plans are formulated for different diseased wooden components to achieve in-situ non-destructive repair of damaged components.
[0160] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable ordinary technicians in the field to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made based on the essence of the content of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for non-destructive protection and repair of a wooden roof, characterized in that: include: Use non-destructive testing to determine roof damage information; repairing the damaged roof based on the determined roof damage information; The repair is one or more of the following: repair of local cracks along the wood grain of beams / columns, repair of insect-damaged and decayed beams, repair of corrosion of wooden beam heads, repair of broken and cracked beams, and repair of columns.
2. The method for non-destructive protection and repair of wooden roofs according to claim 1, characterized in that: The non-destructive testing method is infrared and / or ultrasonic.
3. The method for non-destructive protection and repair of wooden roofs according to claim 1, characterized in that: The repair of local cracks along the wood grain of beams / columns includes: When the cracks are within 5mm, use epoxy resin putty to seal them tightly, including: Mix the epoxy resin and curing agent in the set ratio. After mixing all the ingredients, stir them thoroughly to ensure that the ingredients are evenly distributed to avoid stratification or precipitation. Fill the prepared epoxy resin putty into the gaps in the wooden frame that need to be repaired, and make sure the putty is filled evenly without any voids; According to the curing time of epoxy resin putty, wait for it to fully cure. According to the curing time of epoxy resin putty, wait for it to fully cure. After curing, sand the filled surface to remove excess putty to make the surface smoother, and clean the sanded surface to ensure there is no dust and impurities; Finally, check the caulking and surface smoothing to ensure there are no defects or uneven areas.
4. The method for non-destructive protection and repair of wooden roofs according to claim 1, characterized in that: The repair of local cracks along the wood grain of beams / columns includes: When the crack width is 5 to 10 mm, epoxy resin is used for reinforcement, including: Mix epoxy resin and hardener in the following weight ratio: E—epoxy resin: diethylenetriamine: dimethylamine = 100:10:10; then use a stirrer to stir thoroughly to ensure that the mixture is even and free of bubbles; When pouring epoxy resin, do not fill aggregates, and complete the pouring in layers. Each layer should be properly vibrated to make the epoxy resin liquid fill the gaps and bond firmly with the wood components. The injected epoxy resin is below the surface of the wood component for an antique treatment.
5. The method for non-destructive protection and repair of wooden roofs according to claim 1, characterized in that: The repair of local cracks along the wood grain of beams / columns includes: When the crack width is 10-30mm, epoxy resin is used for reinforcement or combined with wood strips for repair, including: Mix epoxy resin and hardener in the following weight ratio: E—epoxy resin: diethylenetriamine: dimethylamine = 100:10:10; then use a stirrer to stir thoroughly to ensure that the mixture is even and free of bubbles; Before pouring epoxy resin, the filling wood is processed into wooden strips. The inlay wooden strips are made of old wood with the same material as the wooden component and the same length along the grain. The cross-sectional width of the wooden strips is 2 to 3 mm smaller than the split width of the component. Before filling the gap with wooden strips, first pour an appropriate amount of epoxy resin into the gap to wet the connection surface, then place the filling wooden strips in sequence, pour an appropriate amount of epoxy resin again, and knock and vibrate the wooden components appropriately to ensure that the filling wooden strips are fully soaked and wrapped by the epoxy resin and firmly bonded to the wooden components; Determine the number of pouring layers according to the splitting depth. The interval between two pouring layers should be appropriate to ensure that the epoxy resin liquid poured in layers can bond together. The construction method of the latter layer is the same as the previous layer. After the last layer is completed, it should be ensured that the epoxy resin covers the inlaid wooden strips and shall not be higher than the surface of the wooden component. After the epoxy resin solidifies, it should be lower than the surface of the wooden component.
6. The method for non-destructive protection and repair of wooden roofs according to claim 1, characterized in that: The repair of local cracks along the wood grain of beams / columns includes: When the width of the crack is more than 30mm and the depth does not exceed 1 / 4 of the diameter, the crack width is 10 to 30mm, and the full-length wood strips are inserted along the grain to repair it. The beams are also reinforced as follows: At the cracked end of the beam, remove the loose sawdust around the crack, then sand the surface of the beam, remove old paint and surface defects, clean the dust on the pasting surface and wipe it with a semi-wet towel to ensure that the crack and pasting surface are clean; Use epoxy putty to repair the loose surface after cleaning, grind the repair surface and clean the surface dust; Cut appropriate carbon fiber cloth according to the size of the cleaned part. The overlap length of the carbon fiber cloth end should be no less than 30mm and cover it on the cleaned beam surface; Apply base resin on the surface of the beam reinforcement part and the carbon fiber cloth pasting surface, and paste the carbon fiber cloth from the bottom of the beam section to the top of the beam surface, leaving the interface at the upper end of the beam section. The carbon fiber cloth should be closely attached to the wood surface, and squeezed tightly with a roller to drive out bubbles; After the epoxy resin or other adhesive is fully cured, polish the surface of the carbon fiber cloth again to make it flush with the wood surface; Finally, choose wood grain paint that matches the color of the wood, and paint and distress it according to the construction requirements of the paint; The repair of insect-eaten and decayed beams includes: After pest control and disinfection, the corrosion of the beams is evaluated to determine the scope and extent of reinforcement required; Before repairing the interior, use the epoxy resin putty prepared to repair surface cracks and wormholes. For cracks that exceed the filling size range, use wooden strips or wood chips to embed them to increase the firmness of the repair. When filling, ensure that the putty is full and even to avoid gaps. Locate the rebar placement at a certain length from the edge of the four sides of the beam end section, and use laser equipment to drill holes in the beam along the direction of the beam; Carbon fiber reinforcements were implanted at the locations of the laser-punched holes, and steel plates were used at the beginning and end of the beams and the carbon fiber reinforcements were temporarily fastened inside the beams; Drill injection holes at locations where injection reinforcement is required; Inject the prepared epoxy resin into the wood component from the injection hole to fill it. When liquid overflows, stop the action and wait for solidification. When pouring, fill the carbon fiber reinforcement holes to ensure that the carbon fiber reinforcement is closely connected to the beam structure. After the epoxy resin is fully cured in the beam, use sandpaper or other grinding tools to polish the surface of the beam to remove excess resin and uneven parts; Carbon fiber cloth is used to wrap both ends of the wooden components for reinforcement; Finally, tighten the nuts at both ends of the carbon fiber to ensure that the carbon fiber ribs are effectively stressed.
7. The method for non-destructive protection and repair of a wooden roof according to claim 1, characterized in that: The wooden beam head corrosion repair includes: Use cutting tools to remove the stress-bearing parts affected by local corrosion; Disinfect and preserve the cut wood surface and intact parts; Take new wood of the same material as the old wood and make the interface of the old wood into a wedge-shaped interface that fits each other, and fit together to form a new beam structure. The interface wedge should be set vertically from top to bottom on the ground; Drill holes along the longitudinal direction of the beam at a certain length above and below the edge of the new wood end section along the longitudinal vertical line for embedding carbon fiber reinforcements; At several length positions of the end of the old wood inlaid with the new wood, holes are punched up and down along the longitudinal vertical line to embed the carbon fiber reinforcement rod; before drilling, a layer of carbon fiber cloth should be wrapped and reinforced on the surface of the old wood. Continue drilling at the end section of the old wood that is to be inlaid with the new wood, aligning it with the opening of the new wood, until it penetrates to the tie rod hole; Before installing the carbon fiber reinforcement, first insert the reinforcement sleeve from the cross-sectional hole at the end of the old wood, and then insert the tie rod into the tie rod hole from top to bottom, so that the tie rod forms a tie with the metal sleeve 1 and the metal sleeve 2 in sequence, and the nut is inserted into the lower end of the tie rod to tighten it; Apply epoxy resin to the joints of new and old wood, and slowly insert the wedge-shaped joint of the new wood into the joint of the old wood from top to bottom, so that the four sides and the internal carbon fiber rib holes are aligned respectively; before the new and old wood are formally connected, a trial installation must be carried out first. During the formal connection, the end of the new wood should be lower than the end of the old wood to avoid epoxy resin from penetrating into the sleeve hole and causing contamination; Insert the carbon fiber ribs through the end holes of the new wood and connect them to the sleeves to tighten them; The carbon fiber reinforcement implantation hole is filled with epoxy resin, and a steel plate is used at the end, and screws are inserted into the carbon fiber reinforcement head to tighten the carbon fiber reinforcement.
8. The method for non-destructive protection and repair of a wooden roof according to claim 1, characterized in that: The beam fracture repair comprises: Remove loose wood chips and dust from around the crack to ensure it is clean; Reset and straighten the broken and bent beam; Carbon fiber cloth is laid along the longitudinal bottom of the beam for reinforcement; Carbon fiber cloth is laid in sections along the longitudinal side of the beam for reinforcement; Carbon fiber reinforcement is implanted inside; Apply distressed treatment to the surface of reinforced wood.
9. The method for non-destructive protection and repair of a wooden roof according to claim 8, characterized in that: The method of laying carbon fiber cloth for reinforcement along the longitudinal bottom of the beam includes: firstly, applying base resin to the cross section of the end of the beam and the longitudinal bottom of the beam, and then pasting the carbon fiber cloth from the cross section of one end of the beam along the longitudinal bottom of the beam to the cross section of the other end of the beam, the carbon fiber cloth should be closely attached to the surface of the wood, and squeezed tightly with a roller to drive out bubbles; The reinforcement of laying carbon fiber cloth in sections along the longitudinal side of the beam includes: firstly, segmenting along the longitudinal side of the beam, then brushing base resin according to the segment positioning, and then pasting the carbon fiber cloth from the bottom of the beam section upward along the beam surface, leaving the interface at the upper end of the beam section, the carbon fiber cloth and the wood surface should be closely attached, and squeezed densely with a roller to drive out bubbles; the overlap length of the end of the carbon fiber cloth should be not less than 30mm; The internal implantation of carbon fiber reinforcement includes: locating the implantation position at a certain length position of the lower margin edge of the beam end section, using laser equipment to drill holes in the beam along the direction of the beam; implanting the carbon fiber reinforcement at the position drilled by the laser, injecting the prepared epoxy resin into the carbon fiber reinforcement hole to fill it, stopping the action after liquid overflows, and using steel plates at the head and tail ends of the beam to fasten the carbon fiber reinforcement in the beam.
10. The method for non-destructive protection and repair of a wooden roof according to claim 1, characterized in that: Before repairing the damaged roof, it also includes cleaning the damaged roof, including: First, remove the wood tendons and stubble at the split, and then clean the dust in the split gap; First cleaning: Use a bristle brush to clean the dust first. If there are wood tendons or stubble in the gap, use a scraper to remove them and then use a bristle brush to clean them. Finally, use an air pump and a spray gun to blow away the dust in the split gap. Second cleaning: This is done before pouring epoxy resin. Use a spray gun to spray the cracks in the wooden frame again to ensure that the cracks are clean and the epoxy resin is firmly bonded to the wood base.
Citation Information
Cited By
Old wood recycling and splicing method
CN120396065A