Electrochemical device

By using a ceramic layer composed of unsaturated silicone and multi-particle inorganic particles in lithium-ion batteries, the silicon-based negative electrode volume expansion problem is solved, the high-temperature cycling and safety performance of the battery is improved, and a more uniform SEI film is achieved. and diaphragm heat transfer properties.

CN119029486APending Publication Date: 2024-11-26ZHUHAI COSMX BATTERY CO LTD

Patent Information

Application Number
CN202411131092.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The volume expansion effect of silicon-based anode in lithium-ion batteries hinders its commercial application and affects the high-temperature cycling performance, high-temperature storage performance and furnace temperature performance of the battery.

Method used

The electrolyte containing unsaturated silicone compound and a ceramic layer are used. The ceramic layer is composed of inorganic particles with large and small particle sizes. By controlling the mass ratio of inorganic particles and the content of unsaturated silicone, the electrolyte is improved. The wetting effect forms a more uniform and stable SEI film, inhibits the expansion of the silicon-based negative electrode, and improves the heat transfer performance of the diaphragm.

Benefits of technology

Effectively suppresses the expansion of the silicon-based negative electrode, improves the circulation and safety performance of the battery, enhances the stability and safety at high temperatures, avoids the shrinkage or rupture of the diaphragm, and improves the liquid retention and heat transfer of the battery. performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004997823970000041
    Figure BDA0004997823970000041
  • Figure BDA0004997823970000061
    Figure BDA0004997823970000061
  • Figure BDA0004997823970000151
    Figure BDA0004997823970000151
Patent Text Reader

Abstract

The present invention relates to the field of batteries, and provides an electrochemical device, the electrochemical device comprises a positive plate, a negative plate, a diaphragm and an electrolyte, the negative plate comprises a silicon-based material, the diaphragm comprises a base film and a ceramic layer arranged on at least one functional surface of the base film, the ceramic layer comprises two inorganic particles with different particle sizes, and the inorganic particles are arranged on the surface of the base film. The electrolyte contains an unsaturated siloxane compound, and the electrochemical device satisfies the relational expression 0.05 < = 10 * A / (B + C) < = 47; wherein the mass content of the unsaturated siloxane compound in the electrolyte is A wt%, and A is more than or equal to 0.1 and less than or equal to 10; the mass ratio of the first inorganic particles to the second inorganic particles is B, and B is more than or equal to 0.05 and less than or equal to 10; and the mass content of the silicon-based material in the negative active material is C wt%, wherein C is greater than or equal to 1 and less than or equal to 20. The electrochemical device can improve the high-temperature cycle performance, the high-temperature storage performance and the furnace temperature performance of the existing silicon-based lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to an electrochemical device. Background Art

[0002] Silicon has a high lithium storage capacity, far exceeding that of traditional graphite materials. Therefore, introducing silicon into the negative electrode can increase the energy density of the battery, enabling it to store more electrical energy. At the same time, silicon is one of the most abundant materials on earth, so using silicon in battery manufacturing may reduce costs. However, the volume expansion effect of silicon-based negative electrodes hinders their commercial application. In order to solve this difficulty, it is necessary to develop an electrolyte suitable for silicon-based lithium-ion batteries, which plays an important role in inhibiting the volume expansion of silicon materials and improving the performance of silicon-based negative electrode materials. Summary of the invention

[0003] The purpose of the present invention is to overcome the above-mentioned problems existing in the prior art and to provide an electrochemical device which can alleviate the volume expansion problem of existing silicon-based lithium-ion batteries and improve their high-temperature cycle performance, high-temperature storage performance and furnace temperature performance.

[0004] In order to achieve the above-mentioned object, the present invention provides an electrochemical device, the electrochemical device comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, the negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer located on at least one side of the surface of the negative electrode current collector, the negative electrode active material layer comprises a negative electrode active material, the negative electrode active material comprises a silicon-based material, the separator comprises a base film and a ceramic layer arranged on at least one functional surface of the base film, the ceramic layer comprises a first inorganic particle and a second inorganic particle, the particle size of the first inorganic particle is larger than the particle size of the second inorganic particle, the electrolyte comprises a functional additive, the functional additive comprises an unsaturated siloxane compound, and the electrochemical device satisfies the relationship 0.05≤10*A / (B+C)≤47;

[0005] Wherein, the mass content of the unsaturated siloxane compound in the electrolyte is A wt%, 0.1≤A≤10;

[0006] The mass ratio of the first inorganic particles to the second inorganic particles is B, 0.05≤B≤10;

[0007] The mass content of the silicon-based material in the negative electrode active material is C wt%, 1≤C≤20.

[0008] The present invention adopts the above technical solution to achieve the following beneficial effects:

[0009] The ceramic layer of the diaphragm in the electrochemical device of the present invention includes inorganic particles of large and small particle sizes, and the gap of the ceramic layer is regulated by controlling the mass ratio of the two inorganic particles, and a certain amount of unsaturated siloxane is used in conjunction with the electrolyte to better infiltrate the diaphragm, which is beneficial to improving the battery's liquid retention capacity. On the basis of ensuring the liquid retention coefficient, the unsaturated siloxane is polymerized into a SEI film at the negative electrode, and the obtained SEI film is more uniform and stable, which can inhibit the expansion of the silicon-based negative electrode within a range matching the silicon content, so that the negative electrode has a better interface, reduces the damage of the SEI film and the diaphragm, and improves the battery's cycle performance and safety performance. At the same time, because the electrolyte can better infiltrate the diaphragm, the battery's liquid retention capacity is improved, and the diaphragm can also be heated more evenly, avoiding the occurrence of diaphragm shrinkage or film breakage, thereby improving the stability and safety of the battery at high temperatures.

[0010] In addition, by controlling the mass ratio of the two inorganic particles, the ceramic layer can also have a higher packing density. Therefore, compared with conventional ceramic layers, the safety performance of the ceramic layer in the electrochemical device of the present invention is more excellent.

[0011] The endpoints and any values ​​of the range disclosed in this article are not limited to the precise range or value, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Herein, in the absence of special instructions, data ranges include endpoints. DETAILED DESCRIPTION

[0012] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0013] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.

[0014] Traditional diaphragms have poor thermal conductivity. When used with silicon-based negative electrodes, under high temperature conditions, the heat convection inside the battery cell is easily insulated by the diaphragm and becomes uneven, forming a temperature difference. Some areas with poor heat transfer, such as the long heat transfer distance from the center of the battery cell to the surface of the battery cell, release heat rapidly during the test, which will cause the temperature to rise sharply, the diaphragm to shrink or break due to heat, and the positive and negative electrodes to short-circuit, causing failure. Studies have found that adding unsaturated siloxane to the electrolyte and setting a ceramic layer with a certain proportion of inorganic particles of different particle sizes on the diaphragm can improve the wetting effect of the electrolyte, make the diaphragm heat more evenly, avoid the occurrence of diaphragm shrinkage or rupture, and thus improve the high temperature performance of the battery.

[0015] The present invention provides an electrochemical device, the electrochemical device comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, the negative electrode sheet comprising a negative electrode current collector and a negative electrode active material layer located on at least one side of the surface of the negative electrode current collector, the negative electrode active material layer comprising a negative electrode active material, the negative electrode active material comprising a silicon-based material, the separator comprising a base film and a ceramic layer arranged on at least one functional surface of the base film, the ceramic layer comprising a first inorganic particle and a second inorganic particle, the particle size of the first inorganic particle is larger than the particle size of the second inorganic particle, the electrolyte comprising a functional additive, the functional additive comprising an unsaturated siloxane compound, the electrochemical device satisfies the relationship 0.05≤10*A / (B+C)≤47 (for example, 0.05, 0.1, 0.5, 1, 5, 10, 15, 20, 25, 30, 35, 40, 45, 47);

[0016] Wherein, the mass content of the unsaturated siloxane compound in the electrolyte is A wt%, 0.1≤A≤10 (for example, 0.1, 0.5, 1, 2, 4, 6, 8, 10);

[0017] The mass ratio of the first inorganic particles to the second inorganic particles is B, 0.05≤B≤10 (for example, 0.05, 0.1, 0.5, 1, 2, 4, 6, 8, 10);

[0018] The mass content of silicon-based materials in the negative electrode active material is C wt%, 1≤C≤20 (C can be, for example, 1, 5, 10, 15, 20). The ceramic layer of the diaphragm in the electrochemical device of the present invention includes two inorganic particles of different particle sizes, and the gap between the ceramic layers is regulated by controlling the mass ratio of the two inorganic particles, and a certain amount of unsaturated siloxane is used to cooperate with the electrolyte to better infiltrate the diaphragm, which is beneficial to improving the battery's liquid retention capacity, and the unsaturated siloxane is polymerized at the negative electrode to obtain a more uniform and stable SEI film, which can inhibit the expansion of the silicon-based negative electrode within a range that matches the silicon content, so that the negative electrode has a better interface, reduces the damage to the SEI film, and improves the heat transfer performance of the diaphragm at high temperatures, thereby improving the stability and safety of the battery at high temperatures.

[0019] In some embodiments, the unsaturated siloxane compound comprises a compound represented by Formula I;

[0020]

[0021] R1, R2, R3 are the same or different and are independently selected from halogen, cyano, substituted or unsubstituted C 1-12 Alkyl, substituted or unsubstituted C 1-12 Alkoxy, substituted or unsubstituted C 3-12 Cycloalkyl, substituted or unsubstituted C 2-12 Alkenyl, substituted or unsubstituted C 3-12 Cycloalkenyl, substituted or unsubstituted C 6-12 Aryl; if substituted, the substituent is halogen, cyano, C 1-3 Alkyl, C 3-12 Cycloalkyl, C 2-12 Alkenyl, C 3-12 Cycloalkenyl, C 2-12 Alkynyl or C 6-12 Aryl; n is an integer of 0-5 (for example, 0, 1, 2, 3, 4, 5). Unsaturated siloxane compounds have unsaturated double bonds, which can polymerize into films at negative electrodes, improve the stability of SEI films, inhibit the expansion of silicon-based negative electrodes, and improve the cycle performance and safety performance of electrochemical devices at high temperatures.

[0022] In some embodiments, R1, R2, and R3 are the same or different and are independently selected from halogen, cyano, substituted or unsubstituted C 1-6 Alkyl, substituted or unsubstituted C 1-6 Alkoxy, substituted or unsubstituted C 3-6 Cycloalkyl, substituted or unsubstituted C 2-6 Alkenyl, substituted or unsubstituted C 3-6 Cycloalkenyl, substituted or unsubstituted C 6-10 Aryl; if substituted, the substituent is halogen, cyano, C 1-3 Alkyl, C 3-6 Cycloalkyl, C 2-6 Alkenyl, C 3-6 Cycloalkenyl, C 2-6 Alkynyl or C 6-10 Aryl.

[0023] In some embodiments, R1, R2, and R3 are the same or different and are independently selected from halogen, cyano, substituted or unsubstituted C 1-3 Alkyl (C 1-3 Alkyl such as methyl, ethyl, propyl, etc.), substituted or unsubstituted C 1-3 Alkoxy (C 1-3Alkoxy such as methoxy, ethoxy, propoxy, etc.), substituted or unsubstituted C 3-5 Cycloalkyl (C 3-5 Cycloalkyl (e.g., cyclopropyl, cyclobutyl, cyclopentyl), substituted or unsubstituted C 2-3 Alkenyl (C 2-3 Alkenyl such as vinyl, propenyl), substituted or unsubstituted C 3-5 Cycloalkenyl (C 3-5 Cycloalkenyl, such as C3 cycloalkenyl, C4 cycloalkenyl, C5 cycloalkenyl), substituted or unsubstituted C 6-8 Aryl (C 6-8 Aryl is, for example, phenyl, tolyl, ethylphenyl, xylyl); if substituted, the substituent is halogen, cyano, C 1-3 Alkyl, C 3-5 Cycloalkyl, C 2-3 Alkenyl, C 3-5 Cycloalkenyl, C 2-3 Alkynyl or C 6-8 Aryl.

[0024] In some embodiments, the unsaturated siloxane compound comprises at least one of the compounds represented by Formula II to Formula VII;

[0025]

[0026] In the present invention, the mass content of the unsaturated siloxane compound in the electrolyte is A wt%, 0.1≤A≤10, that is, A can be 0.1, 0.2, 0.4, 0.6, 0.8, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10. In some embodiments, 0.1≤A≤5. When the above relationship 0.05≤10*A / (B+C)≤47 is satisfied, when the content of the unsaturated siloxane compound is within this range, the battery's liquid retention capacity can be further improved, and a more uniform and stable SEI film can be obtained by polymerization at the negative electrode, so that the negative electrode has a better interface, and the stability and safety of the battery at high temperature are improved. If A is too large or A is too small, the stability of the SEI film will be reduced, resulting in poor interface performance, which will adversely affect the cycle performance and safety performance of the electrochemical device at high temperature.

[0027] In some embodiments, 0.2≤A≤2.

[0028] In the present invention, the unsaturated siloxane compound can be purchased from commercial sources or prepared by methods known in the art.

[0029] In some embodiments, the functional additives further include other functional additives, and the other functional additives include at least one of 1,3-propane sultone (PS), 1,3-propylene sultone (PST), fluoroethylene carbonate (FEC), diethylene sulfate (DTD), maleic anhydride, citraconic anhydride, succinic anhydride, succinonitrile (SN), adiponitrile (ADN), ethylene glycol bis (propionitrile) ether (EGBE), and 1,3,6-hexanetrinitrile (HTCN).

[0030] In some embodiments, in the electrolyte, the mass content of other functional additives is 0.1-15wt%, for example, 0.1%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt% or 15wt%.

[0031] In some embodiments, the electrolyte further comprises an organic solvent and an electrolyte lithium salt.

[0032] In some embodiments, the organic solvent comprises carbonate and / or carboxylate.

[0033] In some embodiments, the organic solvent comprises at least one of ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), ethyl propionate (EP), propyl propionate (PP), ethyl acetate (EA), ethyl butyrate (EB) and γ-butyrolactone (GBL).

[0034] In some embodiments, the electrolyte lithium salt includes at least one of lithium hexafluorophosphate (LiPF6), lithium difluorophosphate (LiPF2O2), lithium difluorobisoxalate phosphate (LiPF2(C2O4)2), lithium tetrafluorooxalate phosphate (LiPF4C2O4), lithium oxalate phosphate (LiPO2C2O4), lithium bisoxalatoborate (LiBOB), lithium difluorooxalatoborate (LiODFB), lithium tetrafluoroborate (LiBF4), lithium bistrifluoromethylsulfonyl imide (LiTFSI) and lithium bisfluorosulfonyl imide (LiFSI).

[0035] In some embodiments, in the electrolyte, the mass content of the electrolyte lithium salt is 10-15wt%, for example, 10wt%, 11wt%, 12wt%, 13wt%, 14wt% or 15wt%.

[0036] In some embodiments, the particle size Dv50 of the first inorganic particle is 0.5 μm-1.5 μm, such as 0.5 μm, 0.6 μm, 0.8 μm, 1 μm, 1.2 μm, 1.4 μm, 1.5 μm. In some embodiments, the particle size Dv50 of the second inorganic particle is 0.05 μm-0.3 μm, such as 0.05 μm, 0.1 μm, 0.15 μm, 0.2 μm, 0.25 μm, 0.3 μm. The particle size of the inorganic particles can be measured by a particle size analyzer. When the above relationship 0.05≤10*A / (B+C)≤47 is satisfied, when the particle size of the first inorganic particle and the second inorganic particle is within this range, the gap between the ceramic layers can be further optimized, the electrolyte infiltration effect and the liquid retention capacity of the electrochemical device can be improved, and the ceramic layer has a higher packing density, giving the electrochemical device better cycle performance and safety performance at high temperatures.

[0037] In the present invention, 0.03≤B≤12, that is, B can be 0.03, 0.05, 0.1, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12.

[0038] In some embodiments, the first inorganic particles and the second inorganic particles independently contain at least one of silicon dioxide, boehmite, magnesium oxide, magnesium hydroxide, aluminum oxide, zinc oxide, zirconium dioxide, titanium oxide, boron nitride, and aluminum nitride. That is, the specific composition of the first inorganic particles and the second inorganic particles can be the same or different, and the particle size is different.

[0039] In some embodiments, the thickness of the ceramic layer is 0.5 μm-4 μm, for example, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, or 4 μm.

[0040] In some embodiments, in the ceramic layer, the total content of the first inorganic particles and the second inorganic particles is 50wt%-99wt%. Other components may include, for example, a binder, which may be a binder conventionally used in the art, such as but not limited to at least one of polyacrylate, sodium carboxymethyl cellulose, polyvinylidene fluoride, polyacrylonitrile, and polyvinyl alcohol. In some embodiments, in the ceramic layer, the content of the binder is 1wt%-50wt%, such as 1wt%, 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt%, and 50wt%.

[0041] The base film in the separator may be any conventional type in the art. In some embodiments, the base film is made of polyolefin, more preferably polypropylene and / or polyethylene.

[0042] In some embodiments, the base film has a thickness of 3 μm-9 μm, for example, 3 μm, 4 μm, 6 μm, 8 μm, or 9 μm.

[0043] In some embodiments, the silicon-based material comprises a silicon-carbon anode material and / or a silicon-oxygen anode material (SiO x , 0 <x<2)。

[0044] In some embodiments, the negative electrode active material further comprises a carbon-based material.

[0045] In some embodiments, the carbon material comprises at least one of natural graphite, artificial graphite, mesocarbon microbeads, soft carbon, hard carbon, and graphene.

[0046] In some embodiments, the negative electrode active material layer further includes a negative electrode conductor and a negative electrode binder.

[0047] In some embodiments, the negative electrode active material layer comprises 80-99.8 wt % of a negative electrode active material, 0.1-10 wt % of a negative electrode conductor, and 0.1-10 wt % of a negative electrode binder.

[0048] In some embodiments, the negative electrode active material layer comprises 90-99.6 wt % of a negative electrode active material, 0.2-5 wt % of a negative electrode conductor, and 0.2-5 wt % of a negative electrode binder.

[0049] In one embodiment, the negative electrode conductive agent includes at least one of conductive carbon black, acetylene black, Ketjen black, conductive graphite, conductive carbon fiber, carbon nanotubes, metal powder, and carbon fiber.

[0050] In one embodiment, the negative electrode binder includes at least one of sodium carboxymethyl cellulose, styrene-butadiene latex, polytetrafluoroethylene, and polyethylene oxide.

[0051] The negative electrode current collector may be a negative electrode current collector commonly used in the art, such as copper foil or a composite current collector.

[0052] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer coated on one side or both sides of the positive electrode current collector, and the positive electrode active material layer includes a positive electrode active material.

[0053] In some embodiments, the positive electrode active material includes LiNi x Co y Mn z M 1-x-y-zO2 or LiLPO4, wherein 0≤x≤1, 0≤y≤1, 0≤z≤1, 0≤x+y+z≤1, M includes at least one of Mn and Al, M includes at least one of Mg, Zn, Ga, Ba, Al, Fe, Cr, Sn, V, Sc, Ti, Nb, Mo, Zr, Ta, W, B, F, Si, and L includes at least one of Mn, Fe, and Co.

[0054] In some embodiments, the positive electrode active material layer further includes a positive electrode conductor and a positive electrode binder.

[0055] In some embodiments, the mass percentage of each component in the positive electrode active material layer is: 80-99.8wt% of positive electrode active material, 0.1-10wt% of positive electrode conductive agent, and 0.1-10wt% of positive electrode binder.

[0056] In some embodiments, the mass percentage of each component in the positive electrode active material layer is: 90-99.6wt% of positive electrode active material, 0.2-5wt% of positive electrode conductive agent, and 0.2-5wt% of positive electrode binder.

[0057] In some embodiments, the positive electrode conductive agent includes at least one of conductive carbon black, acetylene black, Ketjen black, conductive graphite, conductive carbon fiber, carbon nanotubes, and metal powder.

[0058] In some embodiments, the positive electrode binder includes at least one of sodium carboxymethyl cellulose, styrene-butadiene latex, polytetrafluoroethylene, and polyethylene oxide.

[0059] In some embodiments, the positive electrode current collector may be a positive electrode current collector conventionally used in the art, such as aluminum foil or a composite current collector.

[0060] In some embodiments, the electrochemical device is a lithium-ion battery.

[0061] If not otherwise specified, other options for the electrochemical device are conventional options in the art. The battery can be assembled in a conventional manner in the art.

[0062] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0063] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0064] The present invention is described in detail below in conjunction with specific embodiments, which are used to understand but not to limit the present invention.

[0065] Example 1

[0066] 1) Preparation of positive electrode

[0067] The positive electrode active materials lithium cobalt oxide (LiCoO2), polyvinylidene fluoride (PVDF), SP (super P) and carbon nanotubes (CNT) are mixed in a mass ratio of 96:2:1.5:0.5, N-methylpyrrolidone (NMP) is added, and the mixture is stirred under the action of a vacuum mixer until the mixed system becomes a positive electrode active slurry with uniform fluidity; the positive electrode active slurry is evenly coated on both surfaces of an aluminum foil; the coated aluminum foil is dried, and then rolled and cut to obtain the desired positive electrode sheet.

[0068] 2) Negative electrode preparation

[0069] The negative electrode active materials silicon carbon / artificial graphite (containing 5wt% silicon carbon and 95wt% artificial graphite), sodium carboxymethyl cellulose (CMC-Na), styrene-butadiene rubber, conductive carbon black (SP) and carbon nanotubes (CNT) are mixed in a mass ratio of 94.5:2.5:1.5:1:0.5, deionized water is added, and the negative electrode active slurry is obtained under the action of a vacuum mixer; the negative electrode active slurry is evenly coated on both surfaces of the copper foil; the coated copper foil is dried at room temperature, and then transferred to an oven at 80°C for drying for 10 hours, and then cold pressed and cut to obtain a negative electrode sheet.

[0070] 3) Preparation of electrolyte

[0071] In a glove box filled with argon (H2O<0.1ppm, O2<0.1ppm), EC / PC / DEC / PP were mixed evenly in a mass ratio of 10 / 20 / 40 / 30, and then fully dried lithium hexafluorophosphate (LiPF6) was quickly added thereto to a final concentration of 1 mol / L. After dissolution, 12 wt% of fluoroethylene carbonate based on the total mass of the electrolyte was added, 2 wt% of adiponitrile based on the total mass of the electrolyte was added, and unsaturated siloxane (specific amount and type are described in Table 1) was added, stirred evenly, and after passing the moisture and free acid tests, the desired electrolyte was obtained.

[0072] 4) Preparation of diaphragm

[0073] The diaphragm includes a stacked base film and a ceramic layer, wherein the total thickness of the diaphragm is 7 μm, the thickness of the base film is 5 μm, and the thickness of the ceramic layer is 2 μm. The base film is made of polyethylene, and the ceramic layer includes a first inorganic particle and a second inorganic particle with a total mass content of 90 wt% and a binder of 10 wt%, wherein the first inorganic particle and the second inorganic particle are both aluminum oxide particles, and the particle sizes Dv50 are 1 μm and 0.1 μm, respectively, the mass ratio B of the first inorganic particle and the second inorganic particle is 5, and the binder is polyacrylate.

[0074] 5) Preparation of batteries

[0075] The positive electrode sheet of step 1), the negative electrode sheet of step 2) and the separator are stacked in the order of positive electrode sheet, separator and negative electrode sheet, and then wound to obtain a battery cell; the battery cell is placed in an outer packaging aluminum foil, and the electrolyte of step 3) is injected into the outer packaging, and the battery is obtained through vacuum packaging, standing, forming, shaping, sorting and other processes. The battery of the present invention has a charge and discharge range of 3.0-4.5V.

[0076] Comparative Example 1

[0077] The operation was carried out in accordance with the method described in Example 1, except that no unsaturated siloxane was added to the electrolyte.

[0078] Example 2 and Comparative Example 2

[0079] The operation was carried out according to the method described in Example 1, except that the amount A of unsaturated siloxane added to the electrolyte was different, as shown in Table 1.

[0080] Example 3 and Comparative Example 3

[0081] The operation was carried out according to the method described in Example 1, except that the content C of the silicon-carbon material in the negative electrode active material was different, as shown in Table 1.

[0082] Example 4 and Comparative Example 4

[0083] The operation was performed according to the method described in Example 1, except that the mass ratio B of the first inorganic particles and the second inorganic particles in the separator was different, as shown in Table 1.

[0084] Example 5 and Comparative Example 5

[0085] The operation was carried out according to the method described in Example 1, except that A, B and C were different, as shown in Table 1.

[0086] Example 6 Group

[0087] The operation was carried out according to the method described in Example 1, except that the types of unsaturated siloxane added to the electrolyte were different, as shown in Table 1.

[0088] Comparative Example 6

[0089] The operation was performed according to the method described in Example 1, except that the particle sizes of the first inorganic particles and the second inorganic particles in the ceramic layer were the same, both being 0.5 μm.

[0090] Table 1

[0091] Group Unsaturated siloxane types A B C 10*A / (B+C) Comparative Example 1 / 0 10 5 0 Example 1 Compound of formula II 0.5 5 5 0.5 Example 2-1 * 1 * * 1 Example 2-2 * 2 * * 2 Example 2-3 * 4 * * 4 Embodiment 2-4 * 6 * * 6 Comparative Example 2-1 * 0.05 * * 0.05 Comparative Example 2-2 * 12 * * 12 Example 3-1 * * * 7 0.42 Example 3-2 * * * 10 0.33 Example 3-3 * * * 15 0.25 Embodiment 3-4 * * * 20 0.2 Comparative Example 3 * * * 25 0.17 Example 4-1 * * 0.5 * 0.91 Example 4-2 * * 1 * 0.83 Example 4-3 * * 10 * 0.33 Comparative Example 4-1 * * 0.01 * 1.00 Comparative Example 4-2 * * 15 * 0.25 Example 5-1 * 5 0.1 2 23.81 Example 5-2 * 8 0.2 2 36.36 Comparative Example 5-1 * 5 0.05 1 47.62 Comparative Example 5-2 * 0.1 10 20 0.03 Example 6-1 Compound of formula III * * * * Example 6-2 Compounds of formula IV * * * * Example 6-3 Compounds of formula V * * * * Example 6-4 Compound of formula VI * * * *

[0092] Note: * indicates the same as Example 1.

[0093] Test Case

[0094] The obtained batteries were subjected to 45°C cycle performance test, 60°C high temperature storage performance test and furnace temperature performance test, and the results are shown in Table 2.

[0095] 1) 45℃ cycle performance test

[0096] The batteries prepared in the embodiments and comparative examples were charged and discharged at 45°C at a rate of 1C within the charge and discharge cut-off voltage range. The discharge capacity of the first week of the test was calculated as x1 mAh, and the discharge capacity of the Nth cycle was calculated as y1 mAh. The capacity of the Nth week was divided by the capacity of the first week to obtain the cycle capacity retention rate R1=y1 / x1 of the Nth week, and the cycle number of the battery when the cycle capacity retention rate R1 was 80% was recorded.

[0097] 2) 60℃ high temperature storage performance test

[0098] The batteries prepared in the examples and comparative examples were charged at 25°C at a rate of 1C to a cut-off voltage, a cut-off current of 0.025C, and left to stand for 5 minutes. The thickness of the lithium-ion battery was tested (this was the thickness before storage). The fully charged battery was placed in an open circuit at (60±2)°C for 35 days. After 35 days of storage, it was placed in an open circuit at room temperature for 2 hours. The thickness after storage was measured, and the thickness expansion rate of the lithium-ion battery was calculated:

[0099] Thickness expansion rate = [(thickness after storage - thickness before storage) / thickness before storage] × 100%

[0100] 3) Furnace temperature pass rate test

[0101] The batteries prepared in the examples and comparative examples were discharged at 0.2C at 25°C to the lower limit voltage, charged at a rate of 0.7C to the cut-off voltage, the cut-off current was 0.02C, and left to stand for 5 minutes. The voltage and thickness of the lithium-ion battery were tested, and photos were taken for record. The fully charged battery was placed in an oven and heated at a rate of 5±2°C / min. When the temperature in the box reached 130°C±2°C, the temperature was kept constant and continued for 60 minutes. Then the voltage and internal resistance of the battery were tested, pictures were taken after the test, and the battery voltage and surface temperature were monitored. If the battery smokes, catches fire or explodes, it is considered that the furnace temperature test has failed. "10 / 10" in the furnace temperature pass rate means that out of 10 test batteries, 10 batteries passed the furnace temperature test; "5 / 10" means that out of 10 test batteries, 5 batteries passed the furnace temperature test.

[0102] Table 2

[0103]

[0104]

[0105] It should be noted that, in this article, the terms "comprise", "include" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the method and device in the embodiment of the present invention is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.

[0106] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. An electrochemical device, characterized in that: The electrochemical device comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer located on at least one side of the surface of the negative electrode current collector, wherein the negative electrode active material layer comprises a negative electrode active material, wherein the negative electrode active material comprises a silicon-based material, wherein the separator comprises a base film and a ceramic layer disposed on at least one functional surface of the base film, wherein the ceramic layer comprises a first inorganic particle and a second inorganic particle, wherein the particle size of the first inorganic particle is greater than the particle size of the second inorganic particle, wherein the electrolyte comprises a functional additive, wherein the functional additive comprises an unsaturated siloxane compound, and wherein the electrochemical device satisfies the relationship 0.05≤10*A / (B+C)≤47; Wherein, the mass content of the unsaturated siloxane compound in the electrolyte is A wt%, 0.1≤A≤10; The mass ratio of the first inorganic particles to the second inorganic particles is B, 0.05≤B≤10; The mass content of the silicon-based material in the negative electrode active material is C wt%, 1≤C≤20.

2. The electrochemical device according to claim 1, characterized in that The unsaturated siloxane compound comprises a compound represented by formula I; R1, R2, R3 are the same or different and are independently selected from halogen, cyano, substituted or unsubstituted C 1-12 Alkyl, substituted or unsubstituted C 1-12 Alkoxy, substituted or unsubstituted C 3-12 Cycloalkyl, substituted or unsubstituted C 2-12 Alkenyl, substituted or unsubstituted C 3-12 Cycloalkenyl, substituted or unsubstituted C 6-12 Aryl; if substituted, the substituent is halogen, cyano, C 1-3 Alkyl, C 3-12 Cycloalkyl, C 2-12 Alkenyl, C 3-12 Cycloalkenyl, C 2-12 Alkynyl or C 6-12 Aryl; n is an integer of 0-5; Preferably, R1, R2, and R3 are the same or different and are independently selected from halogen, cyano, substituted or unsubstituted C 1-6 Alkyl, substituted or unsubstituted C 1-6 Alkoxy, substituted or unsubstituted C 3-6 Cycloalkyl, substituted or unsubstituted C 2-6 Alkenyl, substituted or unsubstituted C 3-6 Cycloalkenyl, substituted or unsubstituted C 6-10 Aryl; if substituted, the substituent is halogen, cyano, C 1-3 Alkyl, C 3-6 Cycloalkyl, C 2-6 Alkenyl, C 3-6 Cycloalkenyl, C 2-6 Alkynyl or C 6-10 Aryl; More preferably, R1, R2, and R3 are the same or different and are independently selected from halogen, cyano, substituted or unsubstituted C 1-3 Alkyl, substituted or unsubstituted C 1-3 Alkoxy, substituted or unsubstituted C 3-5 Cycloalkyl, substituted or unsubstituted C 2-3 Alkenyl, substituted or unsubstituted C 3-5 Cycloalkenyl, substituted or unsubstituted C 6-8 Aryl; if substituted, the substituent is halogen, cyano, C 1-3 Alkyl, C 3-5 Cycloalkyl, C 2-3 Alkenyl, C 3-5 Cycloalkenyl, C 2-3 Alkynyl or C 6-8 Aryl; Further preferably, the unsaturated siloxane compound comprises at least one of the compounds represented by Formula II to Formula VII; 3. The electrochemical device according to claim 1 or 2, characterized in that: 0.1≤A≤5, preferably, 0.2≤A≤2.

4. The electrochemical device according to any one of claims 1 to 3, characterized in that: The functional additives further include other functional additives, and the other functional additives include at least one of 1,3-propane sultone, 1,3-propylene sultone, fluoroethylene carbonate, vinyl sulfate, maleic anhydride, citraconic anhydride, succinic anhydride, succinonitrile, adiponitrile, ethylene glycol bis(propionitrile) ether, and 1,3,6-hexanetrinitrile; Preferably, in the electrolyte, the mass content of other functional additives is 0.1-15wt%.

5. The electrochemical device according to any one of claims 1 to 4, characterized in that: The electrolyte further comprises an organic solvent and an electrolyte lithium salt; Preferably, the organic solvent comprises carbonate and / or carboxylate; Preferably, the electrolyte lithium salt includes at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium difluorobisoxalate phosphate, lithium tetrafluorooxalate phosphate, lithium oxalate phosphate, lithium bisoxalate borate, lithium difluorooxalate borate, lithium tetrafluoroborate, lithium bistrifluoromethylsulfonyl imide and lithium bisfluorosulfonyl imide; Preferably, in the electrolyte, the mass content of the electrolyte lithium salt is 10-15wt%.

6. The electrochemical device according to any one of claims 1 to 5, characterized in that: The particle size Dv50 of the first inorganic particles is 0.5 μm-1.5 μm; and / or The particle size Dv50 of the second inorganic particles is 0.05 μm to 0.3 μm.

7. The electrochemical device according to any one of claims 1 to 6, characterized in that: The first inorganic particles and the second inorganic particles independently include at least one of silicon dioxide, boehmite, magnesium oxide, magnesium hydroxide, aluminum oxide, zinc oxide, zirconium dioxide, titanium oxide, boron nitride, and aluminum nitride.

8. The electrochemical device according to any one of claims 1 to 7, characterized in that: The thickness of the ceramic layer is 0.5 μm-4 μm; and / or The base film has a thickness of 3 μm-9 μm.

9. The electrochemical device according to any one of claims 1 to 8, characterized in that: The silicon-based material comprises a silicon-carbon negative electrode material and / or a silicon-oxygen negative electrode material; and / or The negative electrode active material further comprises a carbon-based material; preferably, the carbon material comprises at least one of natural graphite, artificial graphite, mesophase carbon microbeads, soft carbon, hard carbon and graphene.

10. The electrochemical device according to any one of claims 1 to 9, characterized in that: The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer coated on one side or both sides of the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active material; Preferably, the positive electrode active material comprises LiNi x Co y Mn z M 1-x-y-z O2 or LiLPO4, wherein 0≤x≤1, 0≤y≤1, 0≤z≤1, 0≤x+y+z≤1, M includes at least one of Mn and Al, M includes at least one of Mg, Zn, Ga, Ba, Al, Fe, Cr, Sn, V, Sc, Ti, Nb, Mo, Zr, Ta, W, B, F, Si, and L includes at least one of Mn and Fe.

Citation Information

Patent Citations

  • Non-aqueous electrolyte of silicon-based anode lithium ion battery

    CN106129473A

  • High-stability lithium ion battery diaphragm, preparation method thereof and lithium ion battery

    CN107342387A

  • Preparation method of inorganic diaphragm type lithium ion battery, battery cell and lithium ion battery

    CN109742292A

  • High-nickel-silicon-based lithium ion battery electrolyte and high-nickel-silicon-based lithium ion battery

    CN117936902A

  • Electrochemical device

    CN118398894A

Cited By

  • Separator, secondary battery cell and electrical apparatus

    WO2026157485A1