Nano enzyme as well as preparation method and application thereof
By HMD modification of MnFe2O4 nanoenzyme, MnFe2O4@HMD nanoenzyme was formed, which solved the problem of insufficient targeting and killing effect in the treatment of small cell lung cancer, and achieved effective killing and apoptosis induction of small cell lung cancer cells. , providing new therapeutic potential for this field.
Patent Information
- Application Number
- CN202410975410.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-29
AI Technical Summary
The existing MnFe2O4 nanoenzymes lack tumor targeting, making it difficult to effectively treat small-cell lung cancer, and have poor killing effects on cancer cells.
By modifying hyaluronic acid with methacrylic anhydride and dopamine hydrochloride, HA-MA-DA (HMD) was prepared and modified on MnFe2O4 to form MnFe2O4@HMD nanoenzyme, enhancing its killing of small-cell lung cancer cells ability.
MnFe2O4@HMD nanoenzyme can induce ROS in small cell lung cancer cells, consume GSH, promote cell apoptosis, significantly improve the killing effect on H1688 cells, and provide a new strategy for the treatment of small cell lung cancer.
Smart Images

Figure CN119033949A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of medical technology, and in particular to a MnFe2O4@HMD nanozyme and a preparation method and application thereof. Background Art
[0002] Primary lung cancer is a malignant tumor with high morbidity and mortality. Lung cancer can be divided into non-small cell lung cancer (NSCLC) and small cell lung cancer (SCLC). SCLC accounts for about 15% and is the most malignant lung tumor. It grows rapidly, is easy to metastasize, and has a high mortality rate. There has been no progress in the treatment of SCLC in the past 30 years.
[0003] With the rapid development of nanotechnology, various nanomaterials have become powerful tools for cancer treatment. Manganese ferrite (MnFe2O4) nanozyme is a cheap and versatile nanomaterial. Due to its unique physical and chemical properties, it is widely used in magnetic resonance imaging, battery development, sewage treatment, etc. In addition, MnFe2O4 has multiple enzyme activities such as peroxidase (CAT) and catalase (POD), and is also used in anti-cancer research.
[0004] However, simple MnFe2O4 nanozymes lack tumor targeting and often fail to achieve satisfactory anti-cancer effects. Hyaluronic acid (HA) is a natural polymer and also the main component of the extracellular matrix, with good biocompatibility and biodegradability. At the same time, HA is also a natural ligand for the CD44 receptor overexpressed in most cancer cells, and it has received widespread attention as an efficient targeted delivery carrier for tumor treatment. Encapsulation with HA or its derivatives can effectively increase the enrichment of nanozymes at the tumor site and improve its biosafety. At present, the applicant has not found any reports on the use of modified HA to modify MnFe2O4 nanozymes to develop new drugs for the treatment of small cell lung cancer. Summary of the invention
[0005] The main purpose of the present invention is to provide a nanozyme and a preparation method and application thereof. HA (hyaluronic acid) is modified by using MA (methacrylic anhydride) and DA (dopamine) to obtain HA-MA-DA (HMD), and MnFe2O4 nanozyme is modified by using HMD to obtain MnFe2O4@HMD nanozyme. MnFe2O4@HMD has a good killing effect on cancer cells of small cell lung cancer, can induce the production of ROS and the consumption of GSH, and induce apoptosis of small cell lung cancer cells, providing a new strategy for the treatment of small cell lung cancer.
[0006] To achieve the above purpose, the technical solution of the present invention is as follows:
[0007] In a first aspect, the present invention provides a method for preparing a nanozyme, comprising the following steps:
[0008] S1. Modifying hyaluronic acid with methacrylic anhydride and dopamine hydrochloride to obtain HMD;
[0009] S2. Use the HMD to modify MnFe2O4 to obtain MnFe2O4@HMD nanozyme.
[0010] In at least one embodiment, the modification of hyaluronic acid includes the following steps: S11, adding N,N-dimethylformamide to methacrylic anhydride solution, stirring evenly under low temperature conditions to obtain a mixed solution one; S12, adding hyaluronic acid to the mixed solution one, reacting to synthesize HM under room temperature and alkaline conditions, and precipitating, purifying and drying for later use; S13, dissolving HM into an acidic solution, adding 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide, and stirring to obtain a mixed solution two; S14, adding dopamine hydrochloride to the mixed solution three, stirring at room temperature overnight to synthesize HMD, and purifying and drying for later use.
[0011] Further, in step S11, the methacrylic anhydride solution is obtained by dissolving methacrylic anhydride in deionized water at a concentration of 2% w / v; the amount of N,N-dimethylformamide is 2 / 3 of the volume of the methacrylic anhydride solution; and the low temperature is 4°C;
[0012] Further, in step S12, the amount of hyaluronic acid used is 5 times the amount of methacrylic anhydride; the alkaline condition is to use NaOH to keep the reaction system at pH 8-9; the reaction time for synthesizing HM is 6 hours; the precipitation is to add anhydrous ethanol for precipitation; the purification is to collect the precipitate and wash it with anhydrous ethanol for 3 times, dissolve the precipitate in deionized water and dialyze it for 7 days, changing the water every 6 hours; the drying is freeze-drying;
[0013] Further, in step S13, the HM is dissolved into an acidic solution by dissolving HM in deionized water at a concentration of 2% w / v, and adjusting the pH to 5.5 with HCl; the amount of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (EDC) and N-hydroxysuccinimide is 3 times the amount of the HM substance;
[0014] Furthermore, in step S14, the amount of dopamine hydrochloride used is 3 times the amount of HM substance; the purification is dialyzed in a pH 5.5 HCl solution for 7 days, with water changed every 6 hours; and the drying is freeze-drying.
[0015] In at least one embodiment, the HMD modification of MnFe2O4 includes the following steps: S21, dissolving HMD and MnFe2O4 into aqueous solutions respectively, mixing the two solutions to obtain a mixed solution three; S22, alternately performing magnetic stirring and ultrasound on the mixed solution three multiple times under low temperature conditions to obtain MnFe2O4@HMD; S23, purifying and drying after precipitation to obtain a purified MnFe2O4@HMD nanozyme.
[0016] Further, in step S21, the amount of HMD and MnFe2O4 is 5:1 by mass ratio;
[0017] Further, in step S22, the low temperature is 4°C; the magnetic stirring and ultrasound are alternated every 0.5h, and the reaction lasts for 6h;
[0018] Furthermore, in step S23, the purification is washing the precipitate with deionized water and centrifuging multiple times until the supernatant is clear and transparent and the pH is neutral; and the drying is freeze-drying.
[0019] In at least one embodiment, the method for preparing MnFe2O4 comprises the following steps:
[0020] 1) adding manganese acetate tetrahydrate and ferric citrate into water and completely dissolving them to obtain a mixed solution 4; heating the mixed solution 4 to boiling under stirring, and then slowly dropping a NaOH solution to adjust the pH to 12;
[0021] 2) The reaction system was transferred to a reactor, set at 160°C, reacted for 6 hours, cooled to room temperature, and centrifuged repeatedly with deionized water until the supernatant was clear and transparent and the pH was neutral;
[0022] 3) Finally, wash with anhydrous ethanol and centrifuge, remove the supernatant, and vacuum dry to obtain MnFe2O4 powder.
[0023] In a second aspect, the present invention also provides a nanozyme, which is a MnFe2O4@HMD nanozyme prepared by the above preparation method.
[0024] In a second aspect, the present invention also provides the use of the nanozyme in the preparation of a drug for treating small cell lung cancer.
[0025] Furthermore, the drug comprises the nanozyme and pharmaceutically acceptable excipients.
[0026] Furthermore, the drug is a clinically acceptable preparation. Still further, the preparation is in the form of tablets, capsules, pills, granules, dry suspensions, suspensions, oral solutions and injections.
[0027] The present invention can at least achieve the following technical effects:
[0028] 1. The present invention uses MA and DA to modify HA to obtain HMD, and uses ferric citrate and manganese acetate tetrahydrate as raw materials to synthesize MnFe2O4 nanozyme through an improved coprecipitation method. Finally, MnFe2O4 nanozyme is modified with HMD to obtain MnFe2O4@HMD nanozyme. The preparation process is simple, and the nanozyme particles are small in size and evenly dispersed.
[0029] 2. MnFe2O4@HMD nanozymes have a concentration-dependent killing effect on small cell lung cancer cancer cells, especially H1688 cells. H1688 cells show good behavior in the uptake of MnFe2O4@HMD, which helps to deliver the nanozymes into tumor cells. MnFe2O4@HMD can induce H1688 cells to produce ROS and consume GSH, thereby affecting the living environment of the cells. In addition, MnFe2O4@HMD can upregulate the expression of the pro-apoptotic protein Bax in H1688 cells and downregulate the expression of the anti-apoptotic protein Bcl-2, thereby inducing cell apoptosis. In short, MnFe2O4@HMD nanozymes, as a new therapeutic strategy, provide potential hope for the treatment of small cell lung cancer. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 , FTIR absorption spectrum of MnFe2O4@HMD nanozyme.
[0031] Figure 2 , UV-vis absorption spectrum of MnFe2O4@HMD nanozyme.
[0032] Figure 3 , particle size distribution of MnFe2O4@HMD nanozyme.
[0033] Figure 4 , Zeta potential of MnFe2O4@HMD nanozyme.
[0034] Figure 5 , XRD patterns of MnFe2O4@HMD.
[0035] Figure 6 , MnFe2O4(A) and MnFe2O4@HMD(B) (scale bar = 100 nm).
[0036] Figure 7 Cell viability determined by MTT method after H1688 cells were treated with MnFe2O4 or MnFe2O4@HMD; *p<0.05, **p<0.01, ***p<0.001, (x-±s, n=3).
[0037] Figure 8Live / dead staining fluorescence microscopy images of H1688 cells treated with MnFe2O4 or MnFe2O4@HMD (A) (scale bar = 400 μm) and the corresponding quantitative results (B); **p<0.01, ***p<0.001, ****p<0.0001, ( n=3).
[0038] Fig. 9 , Scanning confocal microscopy images of Cy5-MnFe2O4 or Cy5-MnFe2O4@HMD uptake by H1688 cells (A) (scale bar = 200 μm) and the corresponding quantitative results (B); **p<0.01, ***p<0.001, ( n=3).
[0039] Fig.10 , Fluorescence microscopy images of intracellular ROS levels in H1688 cells after treatment with MnFe2O4@HMD (A) (Scale bar = 200 μm) and corresponding quantitative results (B); **p<0.01, ****p<0.0001, ( n=3).
[0040] Fig.11 、Intracellular GSH levels in H1688 cells after treatment with MnFe2O4@HMD; ***p<0.001, ****p<0.0001, ( n=3).
[0041] Fig.12 、The relative protein expression levels of Bax and Bcl-2 in H1688 cells after treatment with different concentrations of MnFe2O4@HMD (A) and the corresponding quantitative results (B); *p<0.05, ***p<0.001, ****p<0.0001, ( n=3). DETAILED DESCRIPTION
[0042] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the technical solution of the present invention is further described in detail in a non-limiting manner in conjunction with the accompanying drawings and specific implementation methods.
[0043] First, the present invention provides a MnFe2O4@HMD nanozyme, which is prepared by the following method: S1, using methacrylic anhydride and dopamine hydrochloride to modify hyaluronic acid to obtain HMD; S2, using the HMD to modify MnFe2O4 to obtain MnFe2O4@HMD nanozyme.
[0044] Specifically, the modification of hyaluronic acid includes the following steps: S11, adding N,N-dimethylformamide to methacrylic anhydride solution, stirring evenly under low temperature conditions to obtain a mixed solution one; S12, adding hyaluronic acid to the mixed solution one, reacting to synthesize HM under room temperature and alkaline conditions, and precipitating, purifying and drying for later use; S13, dissolving HM into an acidic solution, adding 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide, and stirring to obtain a mixed solution two; S14, adding dopamine hydrochloride to the mixed solution three, stirring at room temperature overnight to synthesize HMD, and purifying and drying for later use.
[0045] Specifically, the HMD modification of MnFe2O4 includes the following steps: S21, dissolving HMD and MnFe2O4 into aqueous solutions respectively, mixing the two solutions to obtain a mixed solution three; S22, alternately performing magnetic stirring and ultrasound on the mixed solution three multiple times under low temperature conditions to obtain MnFe2O4@HMD; S23, purifying and drying after precipitation to obtain a purified MnFe2O4@HMD nanozyme.
[0046] In addition, the present invention also provides an improved co-precipitation method for synthesizing MnFe2O4 nanozyme, comprising the following steps: 1) adding manganese acetate tetrahydrate and ferric citrate into water and completely dissolving them to obtain a mixed solution four, heating the mixed solution four to boiling under stirring, and then slowly adding a NaOH solution to adjust the pH to 12; 2) transferring the reaction system to a reactor, setting the conditions to 160°C, reacting for 6 hours and then cooling to room temperature, repeatedly centrifuging with deionized water until the supernatant is clear and transparent and the pH is neutral; 3) finally washing and centrifuging with anhydrous ethanol, absorbing the supernatant, and vacuum drying to obtain MnFe2O4 powder.
[0047] Secondly, the present invention also provides the use of MnFe2O4@HMD nanozyme in the preparation of drugs for treating small cell lung cancer.
[0048] Specifically, the drug comprises MnFe2O4@HMD nanozyme and pharmaceutically acceptable excipients. Excipient components include drug carriers and excipients. An acceptable carrier in a drug can enhance or stabilize the composition, or can be used to promote the preparation of the composition. It may include solvents, dispersion media, coatings, surfactants, antioxidants, isotonic agents, absorption delay agents, salts, drug stabilizers, binders, excipients, disintegrants, lubricants, sweeteners, flavoring agents, dyes, etc. and combinations thereof. Unless conventional carriers are incompatible with active ingredients, they can be considered for use in the preparation of drugs containing nanozymes. The carrier can be selected to minimize adverse side effects of the subject and / or minimize the inactivation of the active ingredient. Excipients refer to substances added to the drug to give the drug a certain shape or a certain concentration. For example, sterile water, saline, polyalkylene glycols (such as polyethylene glycol), vegetable oils or hydrogenated naphthalene, calcium bicarbonate, calcium phosphate, various sugars, various types of starch, cellulose derivatives, gelatin, etc.
[0049] Specifically, the drug described in the present invention can be prepared into any clinically acceptable preparation that is easy to use, and the dosage form of the preparation includes a dosage form for gastrointestinal administration and a dosage form for parenteral administration; more specifically, the dosage form of the preparation can be any one of tablets, capsules, pills, granules, dry suspensions, suspensions, oral solutions and injections.
[0050] The following text will illustrate the preparation method of MnFe2O4@HMD nanozyme and its mechanism of action on small cell lung cancer through several examples.
[0051] Example 1. Preparation of MnFe2O4@HMD
[0052] S1. Manganese acetate tetrahydrate and ferric citrate were added into 50 mL of deionized water in a molar ratio of 1:2 to completely dissolve to obtain a mixed solution 1. The mixed solution 1 was heated to boiling under magnetic stirring, and then 1 M NaOH solution was slowly added dropwise to adjust the pH to 12;
[0053] S2. The reaction system was transferred to a reactor and the conditions were set at 160°C. After reacting for 6 hours, the mixture was cooled to room temperature, washed with deionized water and centrifuged (10,000 rpm, 10 min). The supernatant was removed by suction and centrifuged repeatedly with deionized water until the supernatant was clear and transparent and the pH was neutral.
[0054] S3. Wash with anhydrous ethanol for the last time and centrifuge (10000rpm, 10min), remove the supernatant, and place the precipitate in a vacuum drying oven to dry overnight to obtain dry MnFe2O4 powder. Finally, store the MnFe2O4 at 4°C for future use.
[0055] S4. HA was dissolved in deionized water at a concentration of 2% w / v, and 2 / 3 of the volume of N,N-dimethylformamide (DMF) was added to the HA solution at 4°C and stirred to obtain a mixed solution II;
[0056] S5. Add 5 times the amount of MA (methacrylic anhydride) relative to the amount of HA (hyaluronic acid) substance to the mixed solution 2 at room temperature, and use 1M NaOH to keep the reaction system at pH 8-9, and react at room temperature for 6 hours to synthesize HA-MA (HM); add an equal volume of anhydrous ethanol to the reaction system to precipitate the product, collect the precipitate and wash it with anhydrous ethanol for 3 times, dissolve the precipitate in deionized water and dialyze it for 7 days, changing the water every 6 hours, obtain purified HM, freeze-dry it, and store it at -20°C for use;
[0057] S6. HM was dissolved in deionized water at a concentration of 2% w / v, the pH was adjusted to about 5.5 with 1 M HCl, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (EDC) and N-hydroxysuccinimide (NHS) in an amount 3 times that of the HM substance were added to the solution, and the mixture was stirred for 1 h at pH 5.5 to obtain a mixed solution III;
[0058] S7. Add 3 times the amount of dopamine hydrochloride as the amount of HM substance to the mixed solution 3, maintain the pH at about 5.5, stir at room temperature overnight to synthesize HMD, and dialyze in a pH 5.5 HCl solution for 7 days, changing the water every 6 hours to purify the synthesized HMD, freeze-dry the HMD solution, and store it at -20°C for later use;
[0059] S8. The MnFe2O4 synthesized in S3 and the HMD synthesized in S7 were weighed at a mass ratio of 5:1, and each was dissolved in 100 mL of deionized water. The two solutions were mixed to obtain a mixed solution IV. The mixed solution IV was subjected to alternating magnetic stirring and ultrasound at 4°C, alternating every 0.5 h, and reacted for a total of 6 h to obtain MnFe2O4@HMD. The precipitate was washed with deionized water and centrifuged 6 times until the supernatant was clear and transparent and the pH was neutral. The precipitate was freeze-dried to obtain purified MnFe2O4@HMD, and stored at -20°C for future use.
[0060] Example 2. Characterization of MnFe2O4@HMD
[0061] The MnFe2O4@HMD prepared in Example 1 was taken, and its FTIR absorption spectrum, UV-vis absorption spectrum, particle size, and potential were detected. Its crystal structure was analyzed by XRD, and its morphology was observed by transmission electron microscopy.
[0062] Figure 1The FTIR absorption spectrum of MnFe2O4@HMD is shown in Figure 2. Compared with MnFe2O4, MnFe2O4@HMD has a higher absorption peak at about 1287 cm -1 A new absorption peak appears at (red arrow), which may be the vibration of the aryloxy group. -1 The new absorption peak appears at (black arrow), which is related to the stretching vibration of the COC group on HMD.
[0063] Figure 2 The figure shows the UV-vis absorption spectrum of MnFe2O4@HMD. MnFe2O4 has no obvious characteristic ultraviolet absorption peak, while MnFe2O4@HMD has enhanced absorption at 200-250nm due to the loading of HMD.
[0064] Figure 3 The figure shows the particle size of MnFe2O4@HMD. The average particle sizes of MnFe2O4 and MnFe2O4@HMD measured by DLS are 20.6nm and 27.1nm respectively. The modification of HMD increases the particle size of nanozyme.
[0065] Figure 4 The Zeta potential of MnFe2O4@HMD is shown in Figure 2. The Zeta potential of MnFe2O4 and MnFe2O4@HMD are -5.34±0.82mV and -14.57±1.81mV, respectively. The modification of HMD reduces its Zeta potential.
[0066] Figure 5 The XRD patterns of MnFe2O4@HMD are shown. Compared with the XRD patterns of standard manganese ferrite (JCPDS card no.10-0319), the XRD patterns of MnFe2O4 and MnFe2O4@HMD show obvious X-ray diffraction peaks at 111, 220, 311, 222, 400, 422, 511, and 440 lattice planes. After modification with HMD, the crystal form of the nanozyme did not change significantly.
[0067] Figure 6 Shown is the transmission electron microscope image of MnFe2O4@HMD. Both MnFe2O4 and MnFe2O4@HMD are uniform spherical particles, and the particle sizes of the two nanozymes are evenly dispersed.
[0068] Example 3. Cytotoxicity of MnFe2O4@HMD
[0069] The cytotoxicity of MnFe2O4@HMD was detected by MTT assay and live / dead cell staining.
[0070] For the MTT method, the H1688 cells in the logarithmic growth phase were digested and seeded in 96-well plates at a density of 5000 and 6000 cells per well, respectively. After 24 hours of culture, fresh culture medium was added to the control group, and fresh culture medium containing nanozymes was added to the nanozyme treatment group, with a final concentration of 0-800 μg / mL, and 3 duplicate wells for each concentration. After continuing to culture for 24 hours, 10% of the volume of the culture medium MTT solution (5 mg / mL) was added to each well. After incubation at 37°C for 4 hours, the culture medium was discarded, 150 μL DMSO was added to each well, and the plates were placed on a shaker and shaken for 10 minutes. The absorbance (OD value) at 490 nm was detected by a multifunctional microplate reader, and the cell viability was calculated according to the following formula:
[0071] Cell survival rate of the treated group (%) = (OD value of the treated group - OD value of the blank well) / (OD value of the control group - OD value of the blank well) × 100%.
[0072] like Figure 7 As shown in the figure, MnFe2O4 has a small cytotoxicity to H1688 cells, and when the concentration is 800μg / mL, the cell viability is still above 43%. However, MnFe2O4@HMD has a stronger killing effect on H1688 cells, and at a concentration of 800μg / mL, the cell viability is only about 16%.
[0073] For live / dead cell staining, the cell treatment was the same as above. Each group of cells was stained according to the instructions of the Calcein AM / PI kit, observed and photographed under a fluorescence microscope, and the live / dead cell status of H1688 cells after treatment with 600 μg / mL MnFe2O4 and MnFe2O4@HMD was compared, and the live / dead cell percentage of each group was counted.
[0074] like Figure 8 As shown, there was almost no red fluorescence in the Ctrl group, while at 600 μg / mL, MnFe2O4@HMD showed more cells with red signals than MnFe2O4. According to statistics, the proportion of dead cells in the two treatment groups was 21.9%±3.1% and 43.1%±4.0%, respectively, which further demonstrated that MnFe2O4@HMD had a stronger killing effect on H1688 cells.
[0075] Example 4: Confocal microscopy to observe the uptake of nanozymes by cells
[0076] The experimental steps are as follows:
[0077] (1) Preparation of Cy5-modified nanozymes: Under light-proof conditions, appropriate amounts of MnFe2O4 and MnFe2O4@HMD nanozymes were dispersed in 10 μg / mL Cy5-PEG-SH, and ultrasonic and magnetic stirring were performed alternately every 0.5 h. The reaction lasted for 6 h, and the mixture was centrifuged at 10,000 rpm for 10 min. The supernatant was discarded, dissolved in deionized water, and the centrifugation and washing steps were repeated for about 10 times until the supernatant was clear and transparent and the pH was neutral. After freeze-drying, the precipitate was obtained to obtain Cy5-MnFe2O4 and Cy5-MnFe2O4@HMD, which were stored at -20°C for future use.
[0078] (2) Cell uptake assay: H1688 cells in the logarithmic growth phase were cultured at 1×10 5 / well were inoculated in a 6-well plate with a cover glass. When the cell density reached about 80%, fresh culture medium or fresh culture medium containing 600μg / mL Cy5-MnFe2O4 and Cy5-MnFe2O4@HMD was replaced. After culturing for 3 hours, the culture medium was removed, and the cells were gently washed 2 to 3 times with 4℃ PBS. The cells were fixed with 4% paraformaldehyde solution at room temperature for 30 minutes, then stained with DAPI for 15 to 20 minutes, and gently washed 2 to 3 times with 4℃ PBS. Finally, the slides were sealed with anti-fluorescence quencher, and the images were observed and taken with a laser confocal microscope. The whole process should be carried out under light-proof conditions, and the images were quantified using Image J software.
[0079] like Fig. 9 As shown, after H1688 cells were treated with Cy5-MnFe2O4@HMD, more red Cy5 signals were observed under confocal microscopy than those in the Cy5-MnFe2O4 treatment group. The average fluorescence intensities of Cy5 in the two groups were 23.19±1.59 and 12.97±1.90, respectively, indicating that H1688 cells had more uptake of Cy5-MnFe2O4@HMD, and the modification of HMD improved the tumor cell targeting ability of the nanozyme.
[0080] Example 5: DCF-HA staining to detect the effect of nanozymes on ROS levels in H1688 cells
[0081] The effect of different concentrations of MnFe2O4@HMD on the ROS level of H1688 cells was detected. The cells were plated as above, and when the cell density reached about 80%, the cells were treated with 0, 50, 100, 200, 400, and 800 μg / mL of MnFe2O4@HMD nanozymes for 6 hours, and then DCF-HA staining was performed, incubated at 37°C for 0.5 hours, and gently washed with PBS 2 to 3 times. The cells were observed and photographed using a fluorescence microscope, and the fluorescence intensity was quantified and analyzed using ImageJ software.
[0082] like Fig.10As shown in the figure, it was observed by fluorescence microscopy that with the increase of MnFe2O4@HMD concentration, the ROS fluorescence signal in H1688 cells gradually increased. According to statistics, the ROS fluorescence intensities corresponding to 0, 50, 100, 200, 400, and 800 μg / mL were 4.2±0.7, 6.7±0.5, 8.9±0.4, 13.6±1.7, 22.3±2.0, and 31.6±3.1, respectively.
[0083] Example 6: GSH kit to detect the effect of nanozymes on GSH levels in H1688 cells
[0084] The effects of different concentrations of MnFe2O4@HMD on the GSH level of H1688 cells were detected, and the cell treatment was the same as above. In order to eliminate the influence of different cell viability under different concentrations of MnFe2O4@HMD treatment on GSH detection, after nanozyme treatment, the cells in each group were digested and counted, and 1×10 5 Cells were treated and the test solution was prepared according to the instructions of the glutathione detection kit. The sample absorption curve at a wavelength of 300-600nm was scanned using an ELISA reader, or the OD value at A412 of each treatment group was detected. The GSH level of the Ctrl group was defined as 100%, and the GSH level was calculated according to the following formula:
[0085] GSH level in treatment group (%) = (OD value of treatment group - OD value of blank well) / (OD value of Ctrl group - OD value of blank well) × 100%.
[0086] like Fig.11 As shown in the figure, with the increase of MnFe2O4@HMD nanozyme treatment concentration, the absorption curve detected at 300-600nm gradually flattens, indicating that the GSH level in H1688 cells decreases with the increase of MnFe2O4@HMD concentration. According to statistics, when the MnFe2O4@HMD concentration is 50, 100, 200, 400, and 800 μg / mL, the corresponding cellular GSH levels are 82.9%±2.1%, 70.7%±1.6%, 52.8%±1.9%, 41.4%±2.9%, and 25.7%±3.8%, respectively.
[0087] Example 7: Western blot detection of the expression of apoptosis-related proteins Bax and Bcl-2 in H1688 cells treated with MnFe2O4@HMD
[0088] After treating H1688 cells with 0, 50, 100, 200, 400, and 800 μg / mL of MnFe2O4@HMD nanozymes for 12 h, the cell proteins of each group were extracted and the loading working solution was prepared. A 10% PAGE electrophoresis gel was prepared for electrophoresis at room temperature. The protein was transferred to the NC membrane in an ice bath and blocked with 5% skimmed milk powder blocking solution for 1 h. The NC membrane strips were cut according to the marker position and placed in the corresponding primary antibody dilution solution. The strips were incubated on a shaker at 4 °C overnight. The strips were thoroughly washed with PBST and placed in the secondary antibody dilution solution. The proteins were developed using an ultrasensitive ECL chemiluminescence reagent, and the grayscale value was analyzed using Image J software.
[0089] like Fig.12 As shown in the figure, with the increase of MnFe2O4@HMD nanozyme concentration, the expression of pro-apoptotic protein Bax in H1688 cells gradually increased, and the expression of anti-apoptotic protein Bcl-2 gradually decreased. According to statistics, at the concentrations of 50, 100, 200, 400, and 800 μg / mL, the expression of Bax was 104.7% ± 2.0%, 118.0% ± 6.8%, 139.6% ± 4.6%, 172.7% ± 3.1%, and 178.2% ± 5.5%, respectively; the expression of Bcl-2 was 95.5% ± 3.9%, 72.5% ± 6.3%, 45.4% ± 4.8%, 31.0% ± 4.6%, and 16.9% ± 2.3%, respectively. The above results suggest that MnFe2O4@HMD can induce apoptosis of H1688 cells in a concentration-dependent manner.
Claims
1. A method for preparing a nanozyme, characterized in that: The steps include: S1. Modifying hyaluronic acid with methacrylic anhydride and dopamine hydrochloride to obtain HMD; S2. Use the HMD to modify MnFe2O4 to obtain MnFe2O4@HMD nanozyme.
2. The preparation method according to claim 1, characterized in that The modification of the hyaluronic acid comprises the following steps: S11, adding N,N-dimethylformamide to the methacrylic anhydride solution, stirring evenly at low temperature to obtain a mixed solution 1; S12, adding hyaluronic acid to the mixed solution 1, reacting to synthesize HM under room temperature and alkaline conditions, and precipitating, purifying and drying for later use; S13, dissolving HM into an acidic solution, adding 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide, and stirring to obtain a mixed solution II; S14. Add dopamine hydrochloride to the mixed solution 3, stir at room temperature overnight to synthesize HMD, and purify and dry it for later use.
3. The preparation method according to claim 2, characterized in that: In step S11, the methacrylic anhydride solution is obtained by dissolving methacrylic anhydride in deionized water at a concentration of 2% w / v; the amount of N,N-dimethylformamide used is 2 / 3 of the volume of the methacrylic anhydride solution; and the low temperature is 4° C.; In step S12, the amount of hyaluronic acid used is 5 times the amount of methacrylic anhydride; the alkaline condition is to use NaOH to keep the reaction system at pH 8-9; the reaction time for synthesizing HM is 6 hours; the precipitation is to add anhydrous ethanol for precipitation; the purification is to collect the precipitate and wash it with anhydrous ethanol for 3 times, dissolve the precipitate in deionized water and dialyze it for 7 days, changing the water every 6 hours; the drying is freeze-drying; In step S13, the HM is dissolved into an acidic solution by dissolving HM in deionized water at a concentration of 2% w / v, and adjusting the pH to 5.5 with HCl; the amount of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (EDC) and N-hydroxysuccinimide is 3 times the amount of the HM substance; In step S14, the amount of dopamine hydrochloride used is 3 times the amount of HM substance; the purification is dialyzed in a pH 5.5 HCl solution for 7 days, with water changed every 6 hours; and the drying is freeze-drying.
4. The preparation method according to claim 1, characterized in that: The HMD modification of MnFe2O4 comprises the following steps: S21, dissolving HMD and MnFe2O4 into aqueous solutions respectively, and mixing the two solutions to obtain a mixed solution three; S22, subjecting the mixed solution to magnetic stirring and ultrasonic treatment three times alternately under low temperature conditions to obtain MnFe2O4@HMD; S23, purify and dry after precipitation to obtain purified MnFe2O4@HMD nanozyme.
5. The preparation method according to claim 4, characterized in that: In step S21, the HMD and MnFe2O4 are used in a mass ratio of 5:1; In step S22, the low temperature is 4°C; the magnetic stirring and ultrasound are alternated every 0.5h, and the reaction lasts for 6h; In step S23, the purification is washing the precipitate with deionized water and centrifuging for multiple times until the supernatant is clear and transparent and the pH is neutral; the drying is freeze-drying.
6. The preparation method according to claim 1, characterized in that: The preparation method of MnFe2O4 comprises the following steps: 1) adding manganese acetate tetrahydrate and ferric citrate into water and completely dissolving them to obtain a mixed solution 4; heating the mixed solution 4 to boiling under stirring, and then slowly dropping a NaOH solution to adjust the pH to 12; 2) The reaction system was transferred to a reactor, set at 160°C, reacted for 6 hours, cooled to room temperature, and centrifuged repeatedly with deionized water until the supernatant was clear and transparent and the pH was neutral; 3) Finally, wash with anhydrous ethanol and centrifuge, remove the supernatant, and vacuum dry to obtain MnFe2O4 powder.
7. A nanozyme prepared by the preparation method described in any one of claims 1 to 6.
8. Use of the nanozyme as claimed in claim 7 in the preparation of a drug for treating small cell lung cancer.
9. The use according to claim 8, characterized in that The drug comprises the nanozyme and pharmaceutically acceptable excipients.
10. The use according to claim 8, characterized in that The medicine is a clinically acceptable preparation.
Citation Information
Cited By
Preparation and application of Zn-S-N doped porous carbon loaded FeNx nano enzyme
CN120459321A