Titanium silicalite molecular sieve catalyst forming method and application thereof

The formation of uniform titanium silicon molecular sieve catalyst microspheres through the microfluidic control co-flow device solves the problems of uneven catalyst molding and silicon dissolved in the prior art, improves the catalytic activity and density, and is suitable for industrial production.

CN119034824APending Publication Date: 2024-11-29JIANGSU AIKEWEI TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410863414.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-29
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing titanium silicon molecular sieve catalyst molding methods have problems of irregular morphology and uneven sizes, which leads to unsatisfactory stacking density of the catalyst, affecting the catalytic effect. In traditional processes, there is a phenomenon of silicon dissolved in increasing production costs and safety hazards.

Method used

A microfluidic co-flow device is used to mix titanium silicon molecular sieve with materials such as silicon sol and polymer monomer, and a uniform droplet microsphere is formed through microfluidic technology, followed by polymerization and calcination to obtain uniform particle size and high Catalyst microspheres with specific surface area.

Benefits of technology

The rapid forming of the catalyst is achieved, with narrow particle size distribution and good monodispersion effect, which improves catalytic activity and catalytic performance, reduces the loss rate of silicon dissolved, and meets the needs of large-scale industrial preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034824A_ABST
    Figure CN119034824A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of catalyst preparation, and relates to preparation of a titanium silicalite molecular sieve catalyst, in particular to a forming method and application of a high-performance titanium silicalite molecular sieve catalyst. The invention discloses a titanium silicalite molecular sieve catalyst forming method which comprises the following steps: preparing a dispersed phase from a titanium silicalite molecular sieve, silica sol, a polymer monomer, a monomer initiator, a pore forming agent and water; injecting the dispersed phase into a capillary tube as a material by adopting a microfluidic co-flow device, cutting and dispersing the dispersed phase by utilizing an oil phase dispersing agent injected into a main channel, and carrying out initiated polymerization on the obtained liquid drop microspheres to obtain the titanium silicalite molecular sieve composite microspheres, the titanium silicalite molecular sieve composite microspheres are sequentially subjected to drying, high-temperature roasting and impurity removal, and the titanium silicalite molecular sieve catalyst is obtained. The invention also provides application of the titanium silicalite molecular sieve catalyst in ammoximation reaction of butanone, acetone and acetaldehyde.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalyst preparation, relates to the preparation of titanium silicon molecular sieve catalyst, and particularly relates to a high-performance titanium silicon molecular sieve catalyst molding method and the molded catalyst and application. Background Art

[0002] Titanium silicate molecular sieve is a new type of zeolite molecular sieve material developed in the 1980s and has been widely used in many green organic reactions. At present, the use of titanium silicate molecular sieve / H2O2 catalytic system in the ammoximation process is a new process for the efficient catalytic synthesis of ketoximes in one step. This process greatly simplifies the production process, and the conditions are mild and there are no by-products, which has attracted the attention of the scientific and business communities to this green process. At present, relevant domestic and foreign companies have generally achieved large-scale industrial production based on this process. Among them, most companies use the reactor stirred slurry bed process. Although this process can achieve industrial production, it is limited by the concentration of ammonia and catalyst in the system, resulting in a low effective utilization rate of hydrogen peroxide, which is only about 90%. At the same time, in the production process, since the reaction system is in a slurry bed state, the products produced have the phenomenon of silicon dissolution, which not only affects the quality of the product, but also greatly increases the consumption of catalysts in the system, which not only affects the production cost. It also directly leads to an increase in the risk of safety hazards and an increase in the load of sewage treatment. Based on the above problems, in the field of catalysis, the process method of molding titanium silicate molecular sieves has received widespread attention.

[0003] At present, the main molding processes of catalysts include tablet molding, extrusion molding, spray molding, in-situ molding, etc. Among them, extrusion molding is widely used in industry. In the molding process, it is necessary to select suitable binders, pore-forming agents, extrusion aids, etc. to ensure that the catalyst has high mechanical strength and good catalytic activity after molding. In addition, in industrial applications, bulk density is one of the important properties of the catalyst and one of the important control indicators in the industrial production process. Bulk density can affect the pore structure and specific surface area of ​​the catalyst, thereby affecting the overall catalytic effect. Factors affecting bulk density include catalyst particle shape, size, particle size distribution, etc. Therefore, a good catalyst molding method must ensure the mechanical strength and catalytic activity of the molded catalyst while also ensuring the molded particle morphology of the catalyst.

[0004] A Chinese patent for a method for preparing oxime (CN201410075430.X) discloses a method for preparing oxime, in which a reaction material containing ketone or aldehyde, ammonia and hydrogen peroxide is contacted with a titanium silicon molecular sieve catalyst for an ammoximation reaction to generate ketone oxime or aldoxime, and the characteristic is that the titanium silicon molecular sieve catalyst is a mixture of titanium silicon molecular sieve TS-1 as a main catalyst and at least one of MWW structure titanium silicon molecular sieve and MOR structure titanium silicon molecular sieve as a co-catalyst. The selectivity of the product ketone oxime or aldoxime of the method reaches more than 99.5%; the reaction activity is high, the post-processing process is simple, and no by-product separation process is required; the reaction process is energy-saving and environmentally friendly. However, the catalyst is directly used in a slurry bed reactor, and there is a phenomenon of silicon dissolution during continuous operation, which leads to an overall increase in catalyst consumption and increases production costs. Secondly, the reaction product and the catalyst need to be separated again, and the process is cumbersome.

[0005] Chinese patent A method for improving the mechanical strength of titanium silicon molecular sieve TS-1 (202011115687.5) discloses a molding method for improving the mechanical strength of the catalyst. The method is to add a strong auxiliary agent during the preparation of the original powder. After adding a simple adhesive, an extrusion aid and water to the prepared original powder TS-1, the mechanical strength of the catalyst is greatly improved after mixing, kneading and extrusion molding. The diameter of the catalyst after extrusion molding is about 1.0mm to 5.0mm, and the length of the short strips after pelletizing is 2.0 to 3.0mm. The activity of the prepared molded catalyst in propylene epoxidation and propylene chloride epoxidation is also improved, and it has good strength. However, the traditional extrusion molding technology used in this method can only obtain columnar molecular sieves, which affects the catalyst stacking density in the fixed bed device and affects the overall catalytic effect.

[0006] A Chinese patent for a one-time forming method of titanium silicon molecular sieve (CN201210042471.X) discloses a method for catalyst spray forming. Its technical feature is that after the hydrothermally synthesized titanium silicon molecular sieve is crystallized, the separation, washing and roasting processes are omitted, and the matrix material, adhesive, peptizing agent, polyethylene glycol or field sesbania powder are directly added as pore expansion extrusion, and spray forming is performed after beating. The formed microspheres are then roasted to remove the template agent, and finally large-particle formed titanium silicon molecular sieve particles are obtained. However, the adhesive and pore expansion part in the titanium silicon molecular sieve catalyst form inert amorphous components due to their inactivity. The catalyst unit consumption will be large during the use of the titanium silicon molecular sieve catalyst, and the application cost of the catalyst is relatively high for users.

[0007] Chinese patent A titanium silicon molecular catalyst molding method (CN202310793463.7) discloses a titanium silicon molecular catalyst molding method. In this method, a crystallization liquid with a solid content of 10-15% is used as an auxiliary material for primary spray drying. The template agent in the auxiliary material can link the titanium silicon molecular sieve crystals because it contains hydrophilic groups. Through secondary crystallization, secondary separation, secondary drying, and secondary calcination, large-particle catalyst products are formed, which is convenient for the separation of catalysts and reaction materials during application. At the same time, the use of auxiliary materials such as matrix materials, adhesives, peptizers and pore expanders is avoided, further reducing the cost of raw materials. However, the secondary crystallization process has many links, which increases the cost of process operation, and the particle size of the formed catalyst is small, which cannot meet the requirements of the fixed bed production process.

[0008] The shaped titanium silicon molecular sieve catalyst prepared by the above method has problems such as small size and uneven size distribution. It is impossible to ensure a reasonable packing density when used as a fixed bed filler, and it is impossible to ensure the pore structure and specific surface area of ​​the catalyst, which in turn affects the overall catalytic effect. A uniform and controllable titanium silicon molecular sieve molding technology is urgently needed to be developed and researched. Summary of the invention

[0009] The technical problem to be solved by the present invention is to provide a titanium silicon molecular sieve catalyst molding method and application.

[0010] In order to solve the above technical problems, the present invention provides a titanium silicon molecular sieve catalyst forming method, comprising the following steps:

[0011] 1) Preparation of dispersed phase:

[0012] First, 30 to 50 parts of titanium silicon molecular sieve and 20 to 30 parts (preferably 25 to 30 parts) of silica sol are stirred and mixed, and then 5 to 20 parts of polymer monomer, 0.05 to 1 part of monomer initiator, 10 to 20 parts of pore former and 10 to 20 parts of water are added and stirred and mixed to form a mixed system; the mixed system is placed under vacuum conditions and allowed to stand for degassing to obtain a dispersed phase;

[0013] 2) Preparation of titanium-silicon molecular sieve composite microspheres:

[0014] A microfluidic co-flow device is used, which includes a capillary as an inner microchannel and a main channel as an outer microchannel, the inlet end of the capillary is located outside the main channel, and the rest of the capillary is embedded in the main channel, and the axis of the capillary coincides with the axis of the main channel; the outlet of the capillary is located in the main channel; and the outlet of the main channel is connected to a coil as a heating area;

[0015] The dispersed phase as the inner fluid is injected into the capillary to form the material, and the dispersed phase flowing into the main channel from the capillary is cut and dispersed by the oil phase dispersant (continuous phase) as the outer fluid injected into the main channel, thereby obtaining droplet microspheres (oil-in-water microspheres);

[0016] The droplet microspheres enter the coil and initiate polymerization (monomer polymerization) at a temperature of 40-60° C., and then are filtered and washed to obtain titanium silicate molecular sieve composite microspheres (titanium silicate molecular sieve composite microspheres of uniform size);

[0017] 3) Preparation of finished titanium silicon molecular sieve catalyst:

[0018] The titanium silicon molecular sieve composite microspheres are sequentially dried, calcined at high temperature, and decontaminated (screened to remove impurities, thereby removing impurity powder) to obtain a titanium silicon molecular sieve catalyst.

[0019] As an improvement of the titanium silicon molecular sieve catalyst molding method of the present invention:

[0020] The titanium silicon molecular sieve in step (1) is composed of 60-70% by weight of a main catalyst and 30-40% by weight of a co-catalyst; the main catalyst is titanium silicon molecular sieve TS-1;

[0021] The co-catalyst is at least one of the MWW structure titanium silicon molecular sieve and the MOR structure titanium silicon molecular sieve (ie, one or a mixture of the two).

[0022] As a further improvement of the titanium silicon molecular sieve catalyst molding method of the present invention:

[0023] The polymer monomer is at least one of acrylic acid, methyl acrylate, ethyl acrylate, and butyl acrylate;

[0024] The monomer initiator is at least one of azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, lauroyl peroxide, cumene hydroperoxide, tert-butyl hydroperoxide, di-tert-butyl peroxide, and dicumyl peroxide;

[0025] The pore-forming agent is at least any one of polystyrene, polyacrylic acid, polymethyl methacrylate, polyethylene glycol, polyvinyl butyral, potato starch, corn flour, and soybean flour.

[0026] As a further improvement of the titanium silicon molecular sieve catalyst molding method of the present invention:

[0027] The static degassing in step 1) is as follows: placing the mixed system in a vacuum oven at 20-30° C. for 10-20 minutes, extracting bubbles generated in the mixed system during the static process, and obtaining a dispersed phase.

[0028] As a further improvement of the titanium silicon molecular sieve catalyst molding method of the present invention:

[0029] The oil phase dispersant in step 2) is at least any one of dichloromethane, chloroform, petroleum ether, carbon tetrachloride, n-hexane and toluene.

[0030] As a further improvement of the titanium silicon molecular sieve catalyst forming method of the present invention, the preparation of the titanium silicon molecular sieve composite microspheres in step 2) comprises the following steps:

[0031] 2.1) using the dispersed phase obtained in step 1) as the inner fluid and the oil phase dispersant as the outer fluid;

[0032] In two syringes, the inner fluid and the outer fluid are sucked in respectively; a connecting tube is mounted on the needle of each syringe; and each syringe is provided with a micro-injection pump;

[0033] Instructions, for example, may be: take a 20 mL disposable syringe and replace the original needle with a 19G dispensing needle;

[0034] 2.2) The connecting tube of the syringe filled with the inner fluid (dispersed phase) is connected to the inlet of the capillary, and the connecting tube of the syringe filled with the outer fluid (oil phase dispersant) is connected to the inlet of the main channel (can be connected to the inlet of the main channel through the introduction tube);

[0035] 2.3) The coil is placed in a water bath and immersed in water, and the water bath temperature is controlled at 40-60°C;

[0036] 2.4) Control the flow rate of the injection pump corresponding to the external fluid at 0.50-0.80 ml / min (preferably 0.50-0.65 ml / min), and control the flow rate of the injection pump corresponding to the internal fluid at 0.25-0.55 ml / min (preferably 0.25-0.4 ml / min), and start the two injection pumps at the same time, the internal fluid flows into the capillary, and the external fluid flows into the main channel;

[0037] The inner fluid flowing out of the capillary outlet is sheared by the outer fluid in the main channel to form uniform microspheres (water-in-oil microspheres). The outer fluid acts as a carrier fluid to carry the microspheres out of the main channel and then enter the coil to undergo a monomer polymerization reaction (i.e., heating and curing) at 40 to 60° C. The residence time of the microspheres in the coil is 3 to 7 minutes (preferably 3.5 to 6.5 minutes).

[0038] Note: Residence time = internal volume of coil / flow rate of fluid;

[0039] 2.5) Collect the material after the monomer polymerization reaction at the outlet end of the coil, filter (remove the filtrate) to obtain molecular sieve composite microspheres, and use pure water and anhydrous ethanol to alternately rinse the collected microspheres to remove the oil phase dispersant remaining on the surface to obtain titanium silicalite molecular sieve composite microspheres (titanium silicate molecular sieve composite microspheres with pure surface and uniform particle size).

[0040] As a further improvement of the titanium silicon molecular sieve catalyst forming method of the present invention, in step 3):

[0041] The drying temperature is 80-120°C and the drying time is 6-10 hours;

[0042] The calcination temperature is 350-650°C (preferably 450-550°C), and the calcination time is 4-8h;

[0043] The impurities are removed by sieving through a 200-mesh sieve to filter out fine carbon residues and obtain a pure formed molecular sieve catalyst.

[0044] The present invention also provides a titanium silicon molecular sieve catalyst prepared by any of the above methods.

[0045] The present invention also provides the use of the titanium silicon molecular sieve catalyst in the ammoximation reaction of butanone, acetone and acetaldehyde.

[0046] The present invention aims at the current situation that the molecular sieve catalyst forming method has irregular morphology and uneven size, and proposes a novel microfluidic forming method for titanium silicon molecular sieve catalyst. The method has the advantages of simple operation, continuous production, uniform size of formed microspheres and large specific surface area.

[0047] That is, the invention adopts microfluidic-assisted technology to realize the molding of catalyst molecular sieves. The molding process can be carried out continuously. The size of the molded titanium silicon molecular sieve catalyst can be evenly distributed and the monodisperse effect is good, which is beneficial to the full contact between the catalyst and the reaction raw materials and enhances the catalytic effect.

[0048] Compared with the prior art, the present invention has the following technical advantages:

[0049] 1) The present invention uses microfluidics-assisted technology for the first time to realize the molding of catalyst molecular sieves. The catalyst microsphere molding process is continuous, which can realize large-scale preparation and meet industrialization needs.

[0050] 2) Compared with traditional molding methods, the catalyst microspheres prepared by microfluidic molding method have a good molding effect. The morphology and size of the microspheres can be evenly distributed in a confined space, and the monodispersity effect is good.

[0051] 3) The catalyst microspheres prepared by microfluidic molding method have a large specific surface area, which is beneficial to improve the catalyst activity and enhance the catalytic performance; in addition, the presence of the pore-forming agent makes the catalyst spheres have many cavity channels, which is beneficial to the full contact between the catalyst and the reaction raw materials and enhances the catalytic effect.

[0052] 4) The in-situ polymerization method is adopted, so that the dispersed phase fluid is heated and polymerized after the droplets are formed, ensuring the forming structure of the microspheres.

[0053] In summary, the microfluidic molding method of a titanium silicon molecular sieve catalyst of the present invention can realize the rapid molding of molecular sieve catalysts, and the process can be continuous, which is suitable for industrial large-scale preparation. The confined space in-situ polymerization technology is used to realize the rapid polymerization of catalyst microspheres and fix the skeleton of the catalyst microspheres. Finally, the prepared catalyst molded microspheres have a good surface structure and a narrow particle size distribution. Using a fixed bed reactor, the catalytic performance of titanium silicon molecular sieve microspheres was compared by ammoximation with butanone, acetone, acetaldehyde, etc. The selectivity of the catalyst is ≥99.95%, and the performance is good. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] The specific implementation modes of the present invention are further described in detail below with reference to the accompanying drawings.

[0055] Figure 1 It is a schematic diagram of the structure of the microfluidic cooperative fluid device;

[0056] Figure 2 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0057] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto:

[0058] Device Example 1. A microfluidic co-fluidic device, such as Figure 1 As shown:

[0059] The microchannel includes a capillary 2 as an inner microchannel and a main channel 1 as an outer microchannel, wherein the inlet end of the capillary 2 is located outside the main channel 1, and the rest of the capillary 2 is embedded in the main channel 1, and the axis of the capillary 2 coincides with the axis of the main channel 1. The outlet of the capillary 2 is located inside the main channel 1.

[0060] In order to facilitate the external fluid to enter the main channel 1, an introduction tube 11 connected to the main channel 1 can be set at the entrance of the main channel 1. The introduction tube 11 can be perpendicular to the main channel 1 or at a certain angle to the main channel 1; the outlet of the capillary 2 is sealed and passes through the introduction tube 11 and is located inside the main channel 1.

[0061] The outer diameter of the capillary 2 is smaller than the inner diameter of the main channel 1 ; the inner diameter of the introduction tube 11 = the inner diameter of the main channel 1 .

[0062] The syringe filled with the dispersed phase (internal fluid) is sealed and connected to the capillary inlet through its connecting tube, and the syringe filled with the continuous phase (external fluid, serving as an oil phase dispersant) is sealed and connected to the introduction tube 11 through its connecting tube;

[0063] The syringe is a 20mL disposable syringe; the syringe needle is a 19G dispensing needle (the original needle of the 20mL disposable syringe is replaced with a 19G dispensing needle); the two syringes are each provided with a microinjection pump. The connecting tube of the syringe is, for example, a rubber capillary hose with an inner diameter of 1.2 mm.

[0064] That is, the needle of the syringe filled with dispersed phase (internal fluid) is sealed connected to the inlet of capillary 2 through its connecting tube; the syringe filled with continuous phase (external fluid) is sealed connected to the introduction tube 11 through its connecting tube.

[0065] The outlet of the main channel 1 is connected to the inlet of the coil 3, which is placed in a water bath and immersed in water. The coil 3 serves as a heating reaction area for monomer polymerization.

[0066] The coil 3 is a rubber capillary hose. The outlet of the coil 3 collects the material after the monomer polymerization reaction.

[0067] The forming mechanism of the present invention is:

[0068] The continuous phase (external fluid) flows into the main channel 1, and the dispersed phase (internal fluid) flows into the capillary 2; the flow directions of the continuous phase and the dispersed phase are parallel to each other;

[0069] Since the outlet of the capillary 2 is located inside the main channel 1, the dispersed phase (inner fluid) flowing out of the outlet of the capillary 2 will come into contact with the continuous phase (outer fluid) in the main channel 1, generating co-flow. At the outlet of the capillary 2, the resistance is balanced with the interfacial tension, and the continuous phase (outer fluid) around the outlet of the capillary 2 exerts shear stress on the dispersed phase (inner fluid), squeezing the dispersed phase (inner fluid) into droplet microspheres 4, thereby achieving the cutting of the dispersed phase (inner fluid) by the continuous phase (outer fluid); the obtained droplet microspheres 4 are completely wrapped by the continuous phase, and dispersed and flowed out to the coil 3 in the main channel 1. As the continuous phase wraps the dispersed phase, the diameter of the dispersed phase increases, and the viscous shear stress increases.

[0070] The droplet microspheres 4 flowing out of the main channel 1 enter the coil 3 and initiate polymerization (monomer polymerization) at a temperature of 40-60°C, thereby fixing the molecular sieve forming framework. Finally, the organic components in the microspheres are removed by high-temperature calcination to obtain catalyst microspheres.

[0071] In the microfluidic co-fluidic device used in the following embodiments:

[0072] The inner diameter of the capillary 2 is 0.26 mm, the outer diameter is 0.51 mm, and the length is 20 mm;

[0073] The inner diameter of the main channel 1 is 0.82 mm, the outer diameter is 1.35 mm, and the length is 60 mm;

[0074] The inner diameter of the introduction tube 11 is equal to the inner diameter of the main channel 1 .

[0075] The coil 3 is a rubber capillary hose with an inner diameter of 1.5 mm and a length of 2800 mm.

[0076] The connecting tubes of the syringes are all rubber capillary hoses with an inner diameter of 1.2 mm.

[0077] The following parts are all by weight.

[0078] Preparation method of titanium silicon molecular sieve raw powder: composed of 65% titanium silicon molecular sieve TS-1 (particle size 0.3-0.4μm) and 35% MWW structure titanium silicon molecular sieve (particle size 0.4-0.5μm); titanium silicon molecular sieve TS-1 is used as the main catalyst, and MWW structure titanium silicon molecular sieve is used as the co-catalyst, and the two are mixed to obtain titanium silicon molecular sieve raw powder. The particle size range of titanium silicon molecular sieve raw powder is about 0.3-0.5μm.

[0079] Note: The obtained titanium silicon molecular sieve raw powder is used as raw material for subsequent molding on the one hand, and directly used as ammoximation raw material for comparative experiments on the other hand.

[0080] In the following cases of the present invention, the mass content of silicon dioxide (SiO2) in the silica sol is 30%.

[0081] The diameter of polystyrene microspheres is 500 to 800 nm.

[0082] Example 1: A method for forming a titanium silicon molecular sieve catalyst, using a microfluidic co-fluidic device as described in Device Example 1, and performing the following steps in sequence:

[0083] 1) Preparation of dispersed phase:

[0084] First, 30 parts of titanium silicon molecular sieve powder and 30 parts of silica sol are fully mixed, and then 20 parts of acrylic acid, 0.05 parts of monomer initiator azobisisobutyronitrile, 10 parts of polystyrene microspheres and 10 parts of water are added and stirred and mixed evenly to obtain a mixed system. The mixed system is placed in a vacuum oven at 30°C for 20 minutes, and the bubbles generated by the mixed system during the static process are extracted to obtain a dispersed phase as a material.

[0085] 2) Preparation of titanium-silicon molecular sieve composite microspheres:

[0086] 2.1) using the dispersed phase obtained in step 1) as the inner fluid and the oil phase dispersant as the outer fluid;

[0087] Dichloromethane was selected as the oil phase dispersant;

[0088] The inner fluid and the outer fluid are sucked into two syringes respectively; the needle of the syringe is a 19G dispensing needle; a connecting tube is installed at the needle;

[0089] The syringe is a 20mL disposable syringe; each of the two syringes is provided with a micro-injection pump;

[0090] 2.2) The connecting tube of the syringe filled with the inner fluid (dispersed phase) is connected to the inlet of the capillary 2, and the connecting tube of the syringe filled with the outer fluid (oil phase dispersant) is connected to the inlet of the main channel 1 through the introduction tube 11;

[0091] The connecting tube is a rubber capillary hose with an inner diameter of 1.2 mm;

[0092] 2.3) The coil 3 is placed in a water bath in a spiral shape and immersed in water, and the water bath temperature is controlled to be 40°C;

[0093] 2.4) Control the flow rate of the injection pump corresponding to the external fluid at 0.500 ml / min, and the flow rate of the injection pump corresponding to the internal fluid at 0.250 ml / min. Start the two injection pumps at the same time, and the internal fluid flows into the capillary 2, and the external fluid flows into the main channel 1;

[0094] The inner fluid flowing out of the outlet of the capillary 2 is sheared by the outer fluid in the main channel 1 to form uniform microspheres (water-in-oil microspheres). The outer fluid acts as a carrier fluid to carry the microspheres out of the main channel 1 and then enters the coil 3 as a heating area to undergo a monomer polymerization reaction at 40° C. (i.e., heating and curing molding); the monomer polymerization time is about 6.5 minutes (i.e., the residence time of the microspheres in the coil 3 is about 6.5 minutes);

[0095] Note: Residence time = internal volume of coil / flow rate of fluid;

[0096] Right now,

[0097] Where: d 盘管 Indicates the inner diameter of the coil

[0098] L 盘管 Indicates the length of the coil

[0099] V 分散相 Indicates the flow rate of the dispersed phase fluid

[0100] V 连续相 Indicates the flow rate of the continuous phase fluid

[0101] 2.5) Collect the material after the monomer polymerization reaction at the outlet end of the coil 3, filter (remove the filtrate) to obtain molecular sieve composite microspheres, and use pure water and anhydrous ethanol to alternately rinse the collected microspheres to remove the oil phase dispersant remaining on the surface, and obtain titanium silicon molecular sieve composite microspheres with pure surface and uniform particle size.

[0102] 3) Preparation of finished titanium silicon molecular sieve catalyst:

[0103] The titanium silicon molecular sieve composite microspheres are dried, the drying temperature is controlled at 120°C, and the drying time is controlled at 6 hours. The dried microspheres are calcined at a high temperature, the calcination temperature is controlled at 450°C, and the calcination time is controlled at 8 hours. Then, impurities are removed (screened with a 200-mesh sieve to filter out fine carbon residues); the particle size of the titanium silicon molecular sieve microspheres is about 445-465μm.

[0104] Example 2: A method for forming a titanium silicon molecular sieve catalyst

[0105] The preparation method of the mixed system was changed to: first, 50 parts of titanium silicon molecular sieve raw powder and 25 parts of silica sol were fully mixed, and then 5 parts of acrylic acid, 0.05 parts of monomer initiator azobisisobutyronitrile, 10 parts of polystyrene microspheres and 10 parts of water were added and continued to stir and mix evenly; a mixed system was obtained.

[0106] The rest is the same as Example 1.

[0107] The obtained titanium silicate molecular sieve microspheres have a particle size of about 441 to 460 μm.

[0108] Example 3: A method for forming a titanium silicon molecular sieve catalyst

[0109] The preparation method of the mixed system was changed to: first, 45 parts of titanium silicon molecular sieve raw powder and 25 parts of silica sol were fully mixed, and then 10 parts of acrylic acid, 0.05 parts of monomer initiator azobisisobutyronitrile, 10 parts of polystyrene microspheres and 10 parts of water were added and continued to stir and mix evenly; a mixed system was obtained.

[0110] The rest is the same as Example 1.

[0111] The obtained titanium silicate molecular sieve microspheres have a particle size of about 439 to 460 μm.

[0112] Example 4: A method for forming a titanium silicon molecular sieve catalyst

[0113] The preparation method of the mixed system was changed to: first, 45 parts of titanium silicon molecular sieve raw powder and 25 parts of silica sol were fully mixed, and then 10 parts of acrylic acid, 0.05 parts of monomer initiator azobisisobutyronitrile, 10 parts of polystyrene microspheres and 10 parts of water were added and continued to stir and mix evenly; a mixed system was obtained.

[0114] The flow rate of the syringe pump corresponding to the internal fluid was changed to 0.400 ml / min; therefore, the time for monomer polymerization was about 5.5 minutes.

[0115] The rest is the same as Example 1.

[0116] The particle size of the obtained titanium silicate molecular sieve microspheres is about 658 to 722 μm.

[0117] Example 5: A method for forming a titanium silicon molecular sieve catalyst

[0118] The preparation method of the mixed system was changed to: first, 45 parts of titanium silicon molecular sieve raw powder and 25 parts of silica sol were fully mixed, and then 10 parts of methyl acrylate, 0.05 parts of monomer initiator azobisisobutyronitrile, 10 parts of polystyrene microspheres and 10 parts of water were added and continued to stir and mix evenly; a mixed system was obtained.

[0119] The flow rate of the syringe pump corresponding to the inner fluid was changed to 0.300 ml / min; the flow rate of the syringe pump corresponding to the outer fluid was changed to flow rate control of 0.650 ml / min. Therefore, the time for monomer polymerization was about 5.2 minutes.

[0120] The rest is the same as Example 1.

[0121] The obtained titanium silicate molecular sieve microspheres have a particle size of about 446 to 470 μm.

[0122] Example 6: A method for forming a titanium silicon molecular sieve catalyst

[0123] The preparation method of the mixed system was changed to: first, 45 parts of titanium silicon molecular sieve raw powder and 25 parts of silica sol were fully mixed, and then 10 parts of methyl acrylate, 0.05 parts of monomer initiator azobisisobutyronitrile, 10 parts of potato starch and 10 parts of water were added and continued to stir and mix evenly; a mixed system was obtained.

[0124] The flow rate of the syringe pump corresponding to the inner fluid was changed to 0.300 ml / min; the flow rate of the syringe pump corresponding to the outer fluid was changed to flow rate control of 0.650 ml / min. Therefore, the time for monomer polymerization was about 5.2 minutes.

[0125] The calcination temperature was changed to 550°C and the calcination time remained at 8 h.

[0126] The rest is the same as Example 1.

[0127] The particle size of the obtained titanium silicate molecular sieve microspheres is about 453-485 μm.

[0128] Example 7: A method for forming a titanium silicon molecular sieve catalyst

[0129] The preparation method of the mixed system was changed to: first, 45 parts of titanium silicon molecular sieve raw powder and 25 parts of silica sol were fully mixed, and then 10 parts of acrylic acid, 0.05 parts of monomer initiator azobisisobutyronitrile, 10 parts of polystyrene microspheres and 10 parts of water were added and continued to stir and mix evenly; a mixed system was obtained.

[0130] Petroleum ether was used as the oil phase dispersant;

[0131] The flow rate of the syringe pump corresponding to the inner fluid was changed to 0.300 ml / min; the flow rate of the syringe pump corresponding to the outer fluid was changed to flow rate control of 0.650 ml / min. Therefore, the time for monomer polymerization was about 5.2 minutes.

[0132] The rest is the same as Example 1.

[0133] The obtained titanium silicate molecular sieve microspheres have a particle size of about 432 to 465 μm.

[0134] Example 8: A method for forming a titanium silicon molecular sieve catalyst

[0135] The preparation method of the mixed system was changed to: first, 45 parts of titanium silicon molecular sieve raw powder and 25 parts of silica sol were fully mixed, and then 10 parts of acrylic acid, 0.05 parts of monomer initiator azobisisobutyronitrile, 10 parts of polystyrene microspheres and 10 parts of water were added and continued to stir and mix evenly; a mixed system was obtained.

[0136] Petroleum ether was used as the oil phase dispersant;

[0137] The flow rate of the syringe pump corresponding to the inner fluid was changed to 0.300 ml / min; the flow rate of the syringe pump corresponding to the outer fluid was changed to flow rate control of 0.650 ml / min. Therefore, the time for monomer polymerization was about 5.2 minutes.

[0138] The monomer polymerization temperature was 50°C.

[0139] The rest is the same as Example 1.

[0140] The particle size of the obtained titanium silicate molecular sieve microspheres is about 439 to 468 μm.

[0141] Example 9: A method for forming a titanium silicon molecular sieve catalyst

[0142] The preparation method of the mixed system was changed to: first, 45 parts of titanium silicon molecular sieve raw powder and 25 parts of silica sol were fully mixed, and then 10 parts of acrylic acid, 0.05 parts of monomer initiator azobisisobutyronitrile, 5 parts of polystyrene microspheres, 5 parts of corn flour and 10 parts of water were added and continued to stir and mix evenly; a mixed system was obtained.

[0143] Petroleum ether was used as the oil phase dispersant;

[0144] The flow rate of the syringe pump corresponding to the inner fluid was changed to 0.300 ml / min; the flow rate of the syringe pump corresponding to the outer fluid was changed to flow rate control of 0.650 ml / min. Therefore, the time for monomer polymerization was about 5.2 minutes.

[0145] The monomer polymerization temperature was 50°C.

[0146] The rest is the same as Example 1.

[0147] The particle size of the obtained titanium silicate molecular sieve microspheres is about 442 to 472 μm.

[0148] Comparative Example 1

[0149] 50 parts of titanium silicon molecular sieve powder and 125 parts of silicon solution are fully mixed to form a mixed material. 0.5 parts of starch, 0.5 parts of polyethylene glycol and 10 parts of water are added to the mixed material, and the mixture is kneaded and formed to obtain a plastic body after continued mixing. The kneaded plastic body is placed in an extrusion device to obtain a strip titanium silicon molecular sieve. The strip titanium silicon molecular sieve is obtained by pelletizing the formed strip molecular sieve. The wet catalyst is dried again, and the drying temperature is controlled at 100°C and the drying time is controlled at 6h. The dried microspheres are calcined at high temperature, and the calcination temperature is controlled at 450°C and the calcination time is controlled at 8h. The diameter of the final molded molecular sieve is about 4.0mm to 5mm, and the length of the short strip after pelletizing is 2 to 3mm.

[0150] In order to verify the performance of the catalyst prepared by the microfluidic molding method, the titanium silicon molecular sieve raw powder, the molecular sieve catalysts obtained in Examples 1 to 9, and the molecular sieve catalyst obtained in Comparative Example 1 were subjected to experiments of butanone, acetone, and acetaldehyde ammoximation.

[0151] Experiment 1: Application of catalyst in the ammoximation reaction of butanone

[0152] The shaped titanium silicalite molecular sieve (titanium silicalite catalyst) prepared in Comparative Example 1 and Examples 1 to 9 was subjected to a butanone ammoximation continuous reaction test in a fixed bed reactor.

[0153] The fixed bed reactor is made of stainless steel and has a two-layer sleeve design. The outer layer is an insulating water layer to control the temperature required for ammonia oxime. The interior is filled with a prepared molded molecular sieve, and the two ends of the molecular sieve are filled with quartz sand cotton to filter and intercept. The catalyst concentration is 0.256g / L (the ratio of the mass of the titanium silicon molecular sieve catalyst to the volume of the reaction raw materials), the molar ratio of butanone, ammonia water and hydrogen peroxide is 1:2:1.06, and they are fed separately; the reaction temperature is 70℃, and the residence time is 75min. During the continuous reaction, sampling tests are carried out every two hours to monitor the reaction situation (continuous discharge of the reactor). After continuous operation for 120h, the reaction liquid flowing out of the reactor is collected, its composition is determined, and the conversion rate of butanone and the selectivity of butanone oxime are obtained. After the reaction is completed, the molecular sieve is taken out for cleaning and drying. According to the mass change before and after the reaction, the loss rate of dissolved silicon is obtained.

[0154] The titanium silicon molecular sieve raw powder was used in a slurry bed reactor for butanone ammoximation test. Compared with a fixed bed reactor, the titanium silicon molecular sieve raw powder in the slurry bed reactor is stirred together with the reaction materials.

[0155]

[0156] X MEK , S MEKO are the conversion rate of butanone and the selectivity of butanone oxime respectively. o MEK and n MEK are the amount of butanone entering the reaction system and the amount of butanone discharged from the reaction system, n MEKO is the amount of butanone oxime in the product. It is calculated by the following formula:

[0157]

[0158]

[0159] Table 1 Data of the evaluation of butanone ammoximation of the formed titanium silicon molecular sieves in comparative examples and examples

[0160]

[0161] During the invention process, the present invention also conducted the following comparison:

[0162] The "polystyrene microspheres" in Example 3 were replaced with polyacrylic acid, polymethyl methacrylate, polyethylene glycol, polyvinyl butyral, and soybean powder respectively, and the dosage remained unchanged. The obtained molecular sieve catalyst was used according to the method described in Experiment 1. The results obtained were an average butanone conversion rate of 97.51% to 98.92%, an average butanone oxime selectivity of 99.25% to 99.43%, and a dissolved silicon loss rate of 0.827% to 1.329%.

[0163] Experiment 2: Application of catalyst in acetone ammoximation reaction

[0164] The shaped titanium silicon molecular sieve samples (titanium silicon molecular sieve catalysts) prepared in Comparative Example 1 and Examples 4 to 6 were subjected to a continuous reaction test of acetone ammoximation in a fixed bed reactor. Relative to Experiment 1, the following changes were made: catalyst concentration 0.262 g / L, molar ratio of acetone, ammonia water and hydrogen peroxide was 1:2:1.2. Reaction temperature 60°C, residence time 90 min.

[0165] The titanium silicate molecular sieve raw powder was used in a slurry bed reactor for acetone ammoximation experimental test.

[0166] The rest is the same as Experiment 1.

[0167] The results are shown in Table 2 below.

[0168] Table 2. Data of the evaluation of ammoximation of the formed titanium silicon molecular sieves in comparative examples and examples

[0169]

[0170] Experiment 3: Application of catalysts in the ammoximation reaction of acetaldehyde

[0171] The shaped titanium silicon molecular sieve samples (titanium silicon molecular sieve catalysts) prepared in Comparative Example 1 and Examples 7 to 9 were subjected to a continuous reaction test of acetaldehyde ammoximation in a fixed bed reactor. Relative to Experiment 1, the following changes were made: catalyst concentration 0.255 g / L, molar ratio of acetaldehyde, ammonia water and hydrogen peroxide was 1:2.5:1.3. Reaction temperature 60°C, residence time 70 min.

[0172] The titanium silicon molecular sieve raw powder was used in a slurry bed reactor to carry out acetaldehyde ammoximation experimental test.

[0173] The rest is the same as Experiment 1.

[0174] The results are shown in Table 3 below.

[0175] Table 3 Data of the evaluation of ammoximation of the formed titanium silicon molecular sieves in the comparative examples and the examples

[0176]

[0177] In summary, the formed microsphere molecular sieve prepared by the present invention exhibits good catalytic performance, and the amount of dissolved silicon after the reaction is less, and the overall loss of the catalyst is small.

[0178] Comparative Example 2-1, relative to Example 3, made the following changes:

[0179] The flow rate of the syringe pump corresponding to the inner fluid was changed to 0.150 ml / min; the flow rate of the syringe pump corresponding to the outer fluid was changed to 0.5 ml / min. Therefore, the time for monomer polymerization was about 7.6 minutes.

[0180] The rest is the same as Example 3. The particle size of the obtained microspheres is about 239-260 μm.

[0181] Then, the above Experiment 1 was followed to obtain the following results: the average conversion rate of butanone was 88.45%, the average selectivity of butanone oxime was 89.03%, and the loss rate of dissolved silicon was 0.975%.

[0182] Comparative Example 2-2, relative to Example 3, made the following changes:

[0183] The injection pump flow rate corresponding to the inner fluid was changed to 0.60 ml / min, and the injection pump flow rate corresponding to the outer fluid was changed to 0.6 ml / min; therefore, the monomer polymerization time became about 4.1 minutes, and the rest was the same as Example 3. No formed microspheres could be obtained; therefore, they could not be used as catalyst fillers in fixed bed reactors.

[0184] Comparative Example 3-1: The pore former of Example 3 is eliminated, that is, the amount of polystyrene microspheres is changed from 10 parts to 0 parts; the rest is the same as Example 3.

[0185] Then, the above Experiment 1 was followed to obtain the following results: the average conversion rate of butanone was 96.03%, the average selectivity of butanone oxime was 99.22%, and the loss rate of dissolved silicon was 0.832%.

[0186] Comparative Example 3-2: The amount of polystyrene microspheres in Example 3 was changed from 10 parts to 25 parts; the rest was the same as in Example 3.

[0187] Then, the above experiment 1 was followed to obtain the following results: the average conversion rate of butanone was 98.25%, the average selectivity of butanone oxime was 99.35%, and the loss rate of dissolved silicon was 3.016%.

[0188] Comparative Example 4-1: The polymerization temperature of the monomers in Example 3 was changed from 40° C. to 70° C., and the rest was the same as Example 3.

[0189] Then, the above experiment 1 was followed to obtain the following results: the average conversion rate of butanone was 97.02%, the average selectivity of butanone oxime was 99.15%, and the loss rate of dissolved silicon was 0.795%.

[0190] Comparative Example 4-2: The polymerization temperature of the monomers in Example 3 was changed from 40° C. to 30° C., and the rest was the same as Example 3.

[0191] Then, the above Experiment 1 was followed to obtain the following results: the average conversion rate of butanone was 94.23%, the average selectivity of butanone oxime was 98.78%, and the loss rate of dissolved silicon was 2.864%.

[0192] Comparative Example 5-1

[0193] The coil length in the microfluidic co-fluidic device was reduced from 2800 mm to 1400 mm, and the monomer polymerization time of the composite microspheres was changed. The other conditions were the same as those in Example 3, and the polymerization time was shortened to about 3.3 min.

[0194] Then, the above Experiment 1 was followed to obtain the following results: the average conversion rate of butanone was 94.45%, the average selectivity of butanone oxime was 98.15%, and the loss rate of dissolved silicon was 2.681%.

[0195] Comparative Example 5-2

[0196] The coil length in the microfluidic co-fluidic device was extended from 2800 mm to 5600 mm, and the monomer polymerization time of the composite microspheres was changed. The other conditions were the same as those in Example 3, and the polymerization time was extended to about 13.2 min.

[0197] Then, the above Experiment 1 was followed to obtain the following results: the average conversion rate of butanone was 95.36%, the average selectivity of butanone oxime was 98.52%, and the loss rate of dissolved silicon was 1.021%.

[0198] Comparative Example 6-1: The original titanium silicate powder in Example 3 was changed from "65% titanium silicate TS-1 + 35% MWW structure titanium silicate" to "50% titanium silicate TS-1 + 50% MWW structure titanium silicate", and the other conditions were the same as in Example 3. Then, the above-mentioned Experiment 1 was followed, and the results were as follows: the average conversion rate of butanone was 92.41%, the average selectivity of butanone oxime was 98.76%, and the loss rate of dissolved silicon was 0.895%.

[0199] Comparative Example 6-2: The titanium silicalite raw powder in Example 3 was changed from "65% titanium silicalite TS-1 + 35% MWW structure titanium silicalite" to "90% titanium silicalite TS-1 + 10% MWW structure titanium silicalite", and the other conditions were the same as in Example 3. Then, the above-mentioned Experiment 1 was followed, and the results were as follows: the average conversion rate of butanone was 97.25%, the average selectivity of butanone oxime was 98.83%, and the soluble silicon loss rate was 1.375%.

[0200] Finally, it should be noted that the above examples are only some specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and there are many variations. All variations that can be directly derived or associated with the content disclosed by a person skilled in the art should be considered as the protection scope of the present invention.

Claims

1. A titanium silicon molecular sieve catalyst forming method, characterized in that The following steps are involved: 1) Preparation of dispersed phase: First, 30 to 50 parts of titanium silicon molecular sieve and 20 to 30 parts of silica sol are stirred and mixed, and then 5 to 20 parts of polymer monomer, 0.05 to 1 part of monomer initiator, 10 to 20 parts of pore former and 10 to 20 parts of water are added and stirred and mixed to form a mixed system; the mixed system is placed under vacuum conditions and allowed to stand for degassing to obtain a dispersed phase; 2) Preparation of titanium-silicon molecular sieve composite microspheres: A microfluidic co-flow device is used, the microfluidic co-flow device comprising a capillary (2) as an inner microchannel and a main channel (1) as an outer microchannel, the inlet end of the capillary (2) is located outside the main channel (1), the remaining part of the capillary (2) is embedded in the main channel (1), the axis of the capillary (2) coincides with the axis of the main channel (1); the outlet of the capillary (2) is located inside the main channel (1); the outlet of the main channel (1) is connected to a coil (3) as a heating area; Injecting a dispersed phase into the capillary (2) as a material, and using an oil phase dispersant injected into the main channel (1) to cut and disperse the dispersed phase flowing from the capillary (2) into the main channel (1), thereby obtaining droplet microspheres; The droplet microspheres enter the coil (3) and initiate polymerization at a temperature of 40 to 60° C., and then are filtered and washed to obtain titanium-silicon molecular sieve composite microspheres; 3) Preparation of titanium silicon molecular sieve catalyst: The titanium silicon molecular sieve composite microspheres are sequentially dried, calcined at high temperature, and impurities are removed to obtain a titanium silicon molecular sieve catalyst.

2. The titanium silicon molecular sieve catalyst molding method according to claim 1, characterized in that: The titanium silicon molecular sieve in step (1) is composed of 60-70% by weight of a main catalyst and 30-40% by weight of a co-catalyst; the main catalyst is titanium silicon molecular sieve TS-1; The co-catalyst is at least one of a MWW structure titanium silicon molecular sieve and a MOR structure titanium silicon molecular sieve.

3. The titanium silicon molecular sieve catalyst molding method according to claim 2, characterized in that: The polymer monomer is at least one of acrylic acid, methyl acrylate, ethyl acrylate and butyl acrylate; The monomer initiator is at least one of azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, lauroyl peroxide, cumene hydroperoxide, tert-butyl hydroperoxide, di-tert-butyl peroxide, and dicumyl peroxide; The pore-forming agent is at least any one of polystyrene, polyacrylic acid, polymethyl methacrylate, polyethylene glycol, polyvinyl butyral, potato starch, corn flour, and soybean flour.

4. A titanium silicon molecular sieve catalyst molding method according to claim 3, characterized in that: The static degassing in step 1) is as follows: placing the mixed system in a vacuum oven at 20-30° C. for 10-20 minutes, extracting bubbles generated in the mixed system during the static process, and obtaining a dispersed phase.

5. A titanium silicon molecular sieve catalyst molding method according to claims 1 to 4, characterized in that: The oil phase dispersant in step 2) is at least any one of dichloromethane, chloroform, petroleum ether, carbon tetrachloride, n-hexane and toluene.

6. A titanium silicon molecular sieve catalyst molding method according to claim 5, characterized in that The preparation of titanium silicon molecular sieve composite microspheres in step 2) comprises the following steps: 2.1) using the dispersed phase obtained in step 1) as the inner fluid and the oil phase dispersant as the outer fluid; In two syringes, the inner fluid and the outer fluid are sucked in respectively; a connecting tube is mounted on the needle of each syringe; and each syringe is provided with a micro-injection pump; 2.2) The connecting tube of the syringe filled with the inner fluid is connected to the inlet of the capillary (2), and the connecting tube of the syringe filled with the outer fluid is connected to the inlet of the main channel (1); 2.3) The coil (3) is placed in a water bath in a spiral shape and immersed in water, and the water bath temperature is controlled to be 40-60°C; 2.4) Control the flow rate of the injection pump corresponding to the external fluid at 0.500-0.800 ml / min, and control the flow rate of the injection pump corresponding to the internal fluid at 0.250-0.550 ml / min, and start the two injection pumps at the same time, so that the internal fluid flows into the capillary (2) and the external fluid flows into the main channel (1); The inner fluid flowing out of the outlet of the capillary (2) is sheared by the outer fluid in the main channel (1) to form uniform microspheres. The outer fluid acts as a carrier fluid to carry the microspheres out of the main channel (1) and then enter the coil (3) to undergo a monomer polymerization reaction at 40 to 60° C. The residence time of the microspheres in the coil (3) is 3 to 7 minutes. 2.5) Collect the material after the monomer polymerization reaction at the outlet of the coil (3), filter it, and obtain molecular sieve composite microspheres. Use pure water and anhydrous ethanol to alternately rinse the collected microspheres to remove the oil phase dispersant remaining on the surface, and obtain titanium silicon molecular sieve composite microspheres.

7. A titanium silicon molecular sieve catalyst molding method according to any one of claims 1 to 6, characterized in that In the step 3): The drying temperature is 80-120°C and the drying time is 6-10 hours; The calcination temperature is 350-650°C, and the calcination time is 4-8 hours.

8. The titanium silicon molecular sieve catalyst prepared by the method of any one of claims 1 to 7.

9. Use of the titanium silicon molecular sieve catalyst as claimed in claim 8 in the ammoximation reaction of butanone, acetone and acetaldehyde.

Citation Information

Cited By