Reactive sintering silicon carbide ceramic as well as preparation method and application thereof

Through ball milling and spray granulation technology, combined with silicone permeable sintering, the problems of limited use of silicon carbide ceramics and low blank density in high temperature environments are solved, the density and mechanical properties of the ceramics are improved, the service life is extended and the service life is expanded. Application field.

CN119039002APending Publication Date: 2024-11-29JIAGENG (JIANGSU) SPECIAL MATERIALS CO LTD

Patent Information

Application Number
CN202411160709.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing silicon carbide ceramic materials are limited in use in high temperature environments, and it is difficult to prepare high density blanks in dry press forming process, resulting in poor ceramic performance.

Method used

By mixing silicon carbide powder and graphite powder for ball milling, a clad powder is formed, and then mixed with components such as binder and dispersant, spray granulation and dry pressure forming, and finally silicone sintering is performed to reduce the forming pressure and increase the pressure. Blank density and uniformity.

Benefits of technology

It significantly reduces the ceramic forming pressure, improves the blank density and sintering performance, extends the service life of the ceramic, and broadens its application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039002A_ABST
    Figure CN119039002A_ABST
Patent Text Reader

Abstract

The invention provides a reactive sintering silicon carbide ceramic and a preparation method and application thereof, the preparation method comprises the following steps: (1) mixing silicon carbide powder and graphite powder, and carrying out primary ball milling to obtain coated powder; (2) performing secondary ball milling on mixed carbon powder, a binder, a dispersing agent, a suspending agent, water and the coated powder obtained in the step (1) to obtain composite slurry; (3) performing spray granulation on the composite slurry obtained in the step (2) to obtain composite powder; (4) performing dry pressing on the composite powder obtained in the step (3) to obtain a ceramic biscuit; and (5) siliconizing and sintering the ceramic biscuit obtained in the step (4) to obtain the reaction sintered silicon carbide ceramic. According to the preparation method provided by the invention, the density of the biscuit is improved while the forming pressure is reduced, the uniformity of the biscuit and the ceramic quality are improved, and large-scale popularization and application are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic materials and relates to a silicon carbide ceramic, in particular to a reaction-sintered silicon carbide ceramic and a preparation method and application thereof. Background Art

[0002] It has been more than a hundred years since the advent of silicon carbide ceramic materials. The leading silicon carbide products on the market include reaction-sintered silicon carbide ceramics, which are mainly formed in two ways: extrusion molding and slip casting. However, the silicon carbide ceramics obtained by the above two molding processes have a high content of free silicon, resulting in poor high-temperature use effects and limited use in high-temperature environments.

[0003] In contrast, dry pressing, as a traditional ceramic forming process, has a preparation process including batching, pulping, granulation, dry pressing, drying, sintering and other steps. It has a wide range of applications and high efficiency, but is limited by dry pressing equipment and powder quality. It is difficult to press out products with high green density, especially for high-hardness wear-resistant materials such as silicon carbide and boron carbide, whose dry pressing pressure often requires more than 200MPa. If the green density is low, the density of the sintered ceramic is often also low, and the ceramic performance is poor; and if the forming pressure is increased too much, it is very easy to damage the mold and equipment.

[0004] Specifically, when the ceramic powder is subjected to force, the ceramic particles contact, squeeze and bond with each other. When the pressure is transmitted, the ceramic particles are displaced, and the loose powder is gradually compressed into a block. Friction will be generated between the ceramic particles and between the ceramic particles and the mold. Due to the high hardness and wear resistance of silicon carbide materials, the silicon carbide blanks prepared by dry pressing often require extremely high molding pressure.

[0005] In addition, for products with large size and high thickness, the pressure loss caused by friction often causes the pressure inside the green body to be too low and the density of the green body to be uneven, which in turn leads to poor quality of the ceramics after sintering the green body.

[0006] It can be seen that how to provide a reaction-sintered silicon carbide ceramic and a preparation method thereof, reduce the molding pressure while increasing the density of the green body, and improve the uniformity of the green body and the quality of the ceramics has become an urgent problem that technical personnel in this field need to solve. Summary of the invention

[0007] The purpose of the present invention is to provide a reaction-sintered silicon carbide ceramic and a preparation method and application thereof. The preparation method reduces the molding pressure while increasing the density of the green blank, improves the uniformity of the green blank and the quality of the ceramic, and is conducive to large-scale promotion and application.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a method for preparing a reaction-sintered silicon carbide ceramic, the preparation method comprising the following steps:

[0010] (1) mixing silicon carbide powder and graphite powder and performing ball milling to obtain a coated powder;

[0011] (2) mixing carbon powder, a binder, a dispersant, a suspending agent, water and the coated powder obtained in step (1) and performing secondary ball milling to obtain a composite slurry;

[0012] (3) spray granulating the composite slurry obtained in step (2) to obtain a composite powder;

[0013] (4) dry-pressing the composite powder obtained in step (3) to obtain a ceramic blank;

[0014] (5) The ceramic green body obtained in step (4) is subjected to silicon infiltration and sintering to obtain reaction-sintered silicon carbide ceramics.

[0015] The present invention eliminates irregular edges and corners on the surface of silicon carbide particles through ball milling, so that silicon carbide gradually approaches spherical particles. Since graphite is soft, it will be coated on the surface of silicon carbide particles during the ball milling process. In addition, the crystal structure of graphite is flaky, and the bonding force between the surfaces is weak, so shearing is easily caused, thereby significantly reducing the friction between silicon carbide particles, improving the fluidity of the obtained powder, and further reducing the molding pressure of the ceramic blank, avoiding the damage of the hard powder to the mold and the press, ensuring production safety, and at the same time improving the density and internal structure uniformity of the blank, further improving the ceramic sintering performance and the mechanical properties of the ceramic product.

[0016] In addition, the graphite layer on the surface of silicon carbide reacts with metallic silicon during the silicon infiltration sintering stage, and the resulting β-silicon carbide is firmly adsorbed on the raw material α-silicon carbide, making the sintered silicon carbide ceramics denser and with fewer defects between particles, further improving the mechanical properties of the ceramics, extending the service life of the ceramics, and broadening the application scenarios, such as kiln manufacturing, aerospace, semiconductor industry, photovoltaic technology and other fields.

[0017] In the present invention, the α-silicon carbide and β-silicon carbide refer to two crystal forms of silicon carbide, respectively, wherein the α-silicon carbide crystal structure is hexagonal or rhombohedral, and the β-silicon carbide crystal structure is cubic. Both of these silicon carbide crystal forms are well known to those skilled in the art, so their physical properties are not specifically described here.

[0018] Furthermore, compared with pressureless sintering and hot-pressing sintering of silicon carbide, the preparation process of the reaction-sintered silicon carbide ceramic provided by the present invention is simpler, the sintering temperature is lower, the cost is lower, and the volume shrinkage of the product after sintering is smaller. The preparation principle of reaction-sintered silicon carbide ceramics is that under high temperature conditions, molten metal infiltrates a carbon-containing silicon carbide blank, and the silicon carbide generated by the reaction of silicon and carbon and the excess metallic silicon (free silicon) fill the pores of the blank, thereby obtaining a high-density silicon carbide ceramic.

[0019] Preferably, the silicon carbide powder in step (1) is graded from at least one silicon carbide coarse powder and at least one silicon carbide fine powder, for example, it can be 1, 2, 3, 4, 5 or 6 kinds, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0020] In the present invention, the various silicon carbide coarse powders / fine powders mentioned above specifically refer to silicon carbide powders with various different particle sizes.

[0021] Preferably, the average particle size D50 of the silicon carbide coarse powder is 20 μm to 150 μm, for example, it can be 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm or 150 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0022] Preferably, the average particle size D50 of the silicon carbide fine powder is 1 μm to 20 μm, for example, it can be 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm or 20 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] Preferably, the difference in average particle size D50 between the coarse silicon carbide powder and the fine silicon carbide powder is 10 μm to 100 μm, for example, it can be 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 85 μm, 90 μm, 95 μm or 100 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0024] The present invention obtains silicon carbide powder by grading silicon carbide coarse powder and silicon carbide fine powder of different particle sizes, and strictly limits the particle size difference range between the coarse powder and the fine powder, so that the fine powder can fully fill the gap between the coarse powder, thereby significantly reducing the porosity, further improving the density of the material, and optimizing the thermal and mechanical properties of the material. This filling effect helps to increase the density of the ceramic blank, thereby improving the mechanical strength and wear resistance of the sintered ceramic.

[0025] In addition, mixing particles of different sizes can effectively increase the contact area between particles, which helps to form stronger inter-particle bonds during the molding process, thereby improving the structural stability of the green billet; in the subsequent dry pressing process, particles of different sizes can more evenly distribute the molding pressure and reduce the uneven stress concentration caused by a single particle size, thereby reducing defects in the green billet. The mixing of particles of different sizes can improve the fluidity of the powder, help to achieve a more uniform distribution of the powder during the molding process, and reduce air inclusions and uneven density.

[0026] Furthermore, the fine powder can promote the siliconization sintering process at a lower temperature due to its larger specific surface area, while the presence of coarse powder helps to maintain the structural stability of the material. This grading can optimize the sintering conditions and achieve a more uniform microstructure.

[0027] Preferably, the average particle size D50 of the graphite powder in step (1) is 0.1 μm to 10 μm, for example, it can be 0.1 μm, 0.2 μm, 0.4 μm, 0.6 μm, 0.8 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] The present invention specifically limits the average particle size D50 of the graphite powder to 0.1 μm to 10 μm, which fully improves the fluidity of the graphite powder when mixed with silicon carbide powder, helps to evenly mix the powder during ball milling and molding, and graphite powder with a smaller particle size is more likely to form a uniform coating layer on the surface of the silicon carbide particles, which helps to reduce the friction between the silicon carbide particles and improve the filling properties of the powder.

[0029] Preferably, the mixing mass ratio of the silicon carbide powder and the graphite powder in step (1) is (70-100):(0.1-20), for example, it can be 70:0.1, 75:2, 80:5, 85:10, 90:12, 95:15 or 100:20, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] The present invention specifically limits the mixing mass ratio of silicon carbide powder and graphite powder to (70-100):(0.1-20), which fully reduces the friction between silicon carbide particles, improves the lubricity of the powder, thereby enhancing the formability of the blank, and avoids the damage of the silicon carbide powder to the mold and the press, thereby ensuring production safety.

[0031] Preferably, the first ball milling in step (1) uses silicon carbide balls as ball milling media, because they are made of the same material as the material being ground, thereby avoiding the introduction of impurity elements due to medium wear. In addition, due to the wear resistance and high hardness of silicon carbide balls, long-term ball milling can be carried out without frequent replacement of ball milling media, thereby reducing maintenance and replacement costs in production.

[0032] Preferably, the mass ratio of the ball to material in the first ball milling in step (1) is 1:(0.5-2), for example, it can be 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9 or 1:2, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] Preferably, the time for the first ball milling in step (1) is 2 h to 10 h, for example, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h or 10 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0034] The present invention limits the time of a ball milling to 2 hours to 10 hours, thereby achieving sufficient mixing and dispersion between silicon carbide powder and graphite powder, ensuring the uniformity of the powder, and appropriate ball milling time helps to optimize the morphology of silicon carbide particles, making them tend to be spherical, reducing irregular edges and corners, and helping to further improve the fluidity and filling density of the powder.

[0035] Preferably, the binder in step (2) comprises any one of polyvinyl alcohol, polyvinyl butyral, phenolic resin or epoxy resin, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of polyvinyl alcohol and polyvinyl butyral, a combination of polyvinyl butyral and phenolic resin, a combination of phenolic resin and epoxy resin, a combination of polyvinyl alcohol, polyvinyl butyral and phenolic resin, or a combination of polyvinyl butyral, phenolic resin and epoxy resin.

[0036] The present invention increases the adhesion between powders and improves the forming performance of the composite slurry by limiting the specific types and different combinations of adhesives, making it easier to form a uniform and dense green billet during the dry pressing process. Different types of adhesives can flexibly adjust the viscosity of the composite slurry to achieve ideal forming requirements, further improving the uniformity and forming efficiency of the green billet.

[0037] Preferably, the dispersant in step (2) comprises any one of polyvinyl pyrrolidone, tetramethylammonium hydroxide or sodium dodecyl sulfonate, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of polyvinyl pyrrolidone and tetramethylammonium hydroxide, a combination of tetramethylammonium hydroxide and sodium dodecyl sulfonate, a combination of polyvinyl pyrrolidone and sodium dodecyl sulfonate, or a combination of polyvinyl pyrrolidone, tetramethylammonium hydroxide and sodium dodecyl sulfonate.

[0038] The present invention reduces the van der Waals force between powder particles and prevents particle agglomeration by limiting the specific types and different combinations of dispersants, thereby improving the dispersibility of the powder and ensuring the uniformity of the composite slurry. Good dispersibility helps to improve the fluidity of the powder, which is crucial for subsequent processes such as spray granulation and dry pressing.

[0039] Preferably, the suspending agent in step (2) comprises any one of carboxymethyl cellulose, hydroxymethyl cellulose, polyacetaldehyde vinyl ester or paraffin, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of carboxymethyl cellulose and hydroxymethyl cellulose, a combination of hydroxymethyl cellulose and polyacetaldehyde vinyl ester, a combination of polyacetaldehyde vinyl ester and paraffin, a combination of carboxymethyl cellulose, hydroxymethyl cellulose and polyacetaldehyde vinyl ester, or a combination of hydroxymethyl cellulose, polyacetaldehyde vinyl ester and paraffin.

[0040] The present invention improves the suspension stability of solid particles in the slurry in the liquid medium by limiting the specific types and different combinations of suspending agents, prevents particle sedimentation, ensures the uniformity of the composite slurry, and improves the rheological properties of the composite slurry, so that it has better fluidity during the spray granulation process.

[0041] Preferably, the mixing mass ratio of the carbon powder, binder, dispersant, suspending agent and water in step (2) is (0.1-30):(3-20):(0.1-1):(0.1-1):(80-120), for example, it can be 0.1:3:0.1:1:80, 0.5:5:0.2:0.8:85, 1:6:0.3:0.7:90, 5:8:0.4:0.6:95, 10:10:0.5:0.5:100, 15:12:0.6:0.4:105, 20:15:0.7:0.3:110, 25:18:0.8:0.2:115 or 30:20:1:0.1:120, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0042] The present invention further optimizes the rheological properties of the composite slurry by limiting the mixing mass ratio of carbon powder, binder, dispersant, suspending agent and water, so that it has ideal formability in the spray granulation process, and the appropriate component ratio helps to improve the microstructural uniformity of the green blank, reduce holes and defects, and thus improve the mechanical properties of the final product.

[0043] Preferably, the secondary ball milling in step (2) uses silicon carbide balls as ball milling media, which not only avoids the introduction of impurity elements due to medium wear, but also, due to the wear resistance and high hardness of the silicon carbide balls, long-term ball milling can be carried out without frequent replacement of the ball milling media, thereby reducing maintenance and replacement costs in production.

[0044] Preferably, the time for the secondary ball milling in step (2) is 5 h to 24 h, for example, 5 h, 6 h, 8 h, 10 h, 12 h, 14 h, 16 h, 18 h, 20 h, 22 h or 24 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0045] The present invention limits the time of secondary ball milling to 5 hours to 24 hours, ensuring that all components (including carbon powder, binder, dispersant, suspending agent and water) are fully mixed in the composite slurry to form a uniform dispersion system, and appropriate ball milling time can further refine the raw material particles, increase the specific surface area of ​​the particles, and help to improve the packing density of the particles in the subsequent molding process and the diffusion rate in the sintering process.

[0046] Preferably, the solid content of the composite slurry in step (2) is 40wt% to 65wt%, for example, it can be 40wt%, 42wt%, 44wt%, 46wt%, 48wt%, 50wt%, 52wt%, 54wt%, 56wt%, 58wt%, 60wt%, 62wt%, 64wt% or 65wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are equally applicable.

[0047] The present invention specifically limits the solid content of the composite slurry to 40wt% to 65wt%, thereby ensuring that the composite slurry has good formability during the spray granulation process, avoiding the molding difficulty caused by too low solid content or the increase in molding pressure caused by too high solid content, and the appropriate solid content can reduce the drying time, speed up the production process, and improve production efficiency.

[0048] Preferably, the viscosity of the composite slurry in step (2) is 300 mPa·s to 1500 mPa·s, for example, it can be 300 mPa·s, 400 mPa·s, 500 mPa·s, 600 mPa·s, 700 mPa·s, 800 mPa·s, 900 mPa·s, 1100 mPa·s, 1200 mPa·s, 1300 mPa·s, 1400 mPa·s or 1500 mPa·s, but is not limited to the listed values, and other unlisted values ​​within the numerical range are equally applicable.

[0049] The present invention specifically limits the viscosity of the composite slurry to 300 mPa·s to 1500 mPa·s, so that it has good fluidity and is convenient for transportation and distribution during the spray granulation process. The appropriate viscosity can prevent the sedimentation of particles in the slurry, maintain the uniformity of the slurry, and avoid stratification and agglomeration.

[0050] Preferably, the spray granulation in step (3) is carried out in a centrifugal spray dryer, and the inlet temperature of the centrifugal spray dryer is 100°C to 300°C, for example, 100°C, 120°C, 140°C, 160°C, 180°C, 200°C, 220°C, 240°C, 260°C, 280°C or 300°C, and the outlet temperature is 80°C to 120°C, for example, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C , 115°C or 120°C, the atomizer frequency is 150Hz to 300Hz, for example, it can be 150Hz, 160Hz, 170Hz, 180Hz, 190Hz, 200Hz, 210Hz, 220Hz, 230Hz, 240Hz, 250Hz, 260Hz, 270Hz, 280Hz, 290Hz or 300Hz, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0051] The present invention sprays and granulates the composite slurry in a centrifugal spray dryer, so that the material particles are quickly dried in hot air, agglomeration and sedimentation separation of the components are avoided, the original uniformity of the slurry is maintained, and spherical particles with uniform particle size distribution and good fluidity are finally obtained.

[0052] Preferably, the feed rate of the spray granulation in step (3) is 3kg / h to 10kg / h, for example, 3kg / h, 3.5kg / h, 4kg / h, 4.5kg / h, 5kg / h, 5.5kg / h, 6kg / h, 6.5kg / h, 7kg / h, 7.5kg / h, 8kg / h, 8.5kg / h, 9kg / h, 9.5kg / h or 10kg / h, but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable.

[0053] The present invention specifically limits the feed flow rate of spray granulation to 3kg / h to 10kg / h, which helps to ensure the formation of uniform and high-quality particles during the spray granulation process and avoids uneven particles caused by too fast or too slow feeding. In addition, the control of the feed flow rate helps to adjust the drying rate of the material and prevent particle cracking caused by too fast drying or reduced production efficiency caused by too slow drying.

[0054] Preferably, the average particle size of the composite powder in step (3) is 60 mesh to 320 mesh, for example, it can be 60 mesh, 80 mesh, 100 mesh, 120 mesh, 140 mesh, 160 mesh, 180 mesh, 200 mesh, 220 mesh, 240 mesh, 260 mesh, 280 mesh, 300 mesh or 320 mesh, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0055] The present invention specifically limits the average particle size of the composite powder to 60 mesh to 320 mesh, so that the particles can achieve a higher packing density, which helps to improve the density of the blank and the mechanical properties of the final product. The moderate particle size range helps the mechanical engagement and chemical bonding between the particles, further improving the structural strength of the blank.

[0056] Preferably, the water content of the composite powder in step (3) is 0.5wt% to 1.5wt%, for example, it can be 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt% or 1.5wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0057] The present invention specifically limits the moisture content of the composite powder to 0.5wt% to 1.5wt%, which not only prevents excessive moisture from appearing during the drying process and causing particle cracking or deformation, but also ensures that sufficient moisture is removed from the powder during the drying process, thereby avoiding subsequent molding and sintering problems caused by insufficient drying.

[0058] Preferably, the dry pressing pressure in step (4) is 50 MPa to 150 MPa, for example, it can be 50 MPa, 60 MPa, 70 MPa, 80 MPa, 90 MPa, 100 MPa, 110 MPa, 120 MPa, 130 MPa, 140 MPa or 150 MPa, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0059] In the present invention, the dry pressing pressure is only 50MPa to 150MPa, which is much lower than the traditional dry pressing pressure (≥200MPa). This is mainly due to the high fluidity of silicon carbide powder, thereby avoiding damage to the mold and press by the hard powder, ensuring production safety and reducing preparation costs.

[0060] Preferably, the density of the ceramic blank in step (4) is 2 g / cm 3 Up to 2.5g / cm 3 , for example, it can be 2g / cm 3 , 2.05g / cm 3 , 2.1g / cm 3 , 2.15g / cm 3 , 2.2g / cm 3 , 2.25g / cm 3 , 2.3g / cm 3 , 2.35g / cm 3 , 2.4g / cm 3 , 2.45g / cm 3 or 2.5g / cm 3 , but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0061] In the present invention, the density of the ceramic blank is directly related to the volume density of the silicon carbide ceramic product, which directly affects the strength and service life of the ceramic product. Specifically, the ceramic blank within the above density range has a good microstructure, which helps to form uniform grain growth and reduce pores during the sintering process, thereby improving the overall quality of the sintered body and further improving the compressive strength, flexural strength and hardness of the final product.

[0062] Preferably, during the siliconizing and sintering process in step (5), the mass ratio of the ceramic green body and the metallic silicon is 1:(0.6-1.5), for example, it can be 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4 or 1:1.5, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0063] The present invention limits the mass ratio of the ceramic blank to the metal silicon to 1:(0.6-1.5) during the siliconizing sintering process, that is, accurately controls the amount of metal silicon added, thereby optimizing the reaction between the metal silicon and the silicon carbide blank, ensuring that the required β-silicon carbide is fully generated, thereby improving the performance of the material, and the appropriate amount of metal silicon added helps to control the free silicon content in the final product, avoiding the degradation of material performance due to excessive free silicon.

[0064] Preferably, the heating rate of the siliconizing sintering in step (5) is 3°C / min to 20°C / min, for example, it can be 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min, 11°C / min, 12°C / min, 13°C / min, 14°C / min, 15°C / min, 16°C / min, 17°C / min, 18°C / min, 19°C / min or 20°C / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are equally applicable.

[0065] The present invention specifically limits the heating rate of siliconizing sintering to 3°C / min to 20°C / min, which helps to achieve uniform temperature inside the green blank and avoid thermal stress and cracking caused by rapid heating. Specifically, since an excessively fast heating rate can easily generate thermal stress inside the material, the present invention limits the heating rate to an appropriate range, which can reduce such thermal stress and thus substantially reduce the risk of material cracking.

[0066] Preferably, the temperature of the siliconizing sintering in step (5) is 1500°C to 1800°C, for example, it can be 1500°C, 1550°C, 1600°C, 1650°C, 1700°C, 1750°C or 1800°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0067] The present invention specifically limits the temperature of siliconizing sintering to 1500°C to 1800°C, which promotes a sufficient reaction between the silicon carbide blank and the metallic silicon to generate the desired β-silicon carbide. The above temperature range helps to control the growth rate of the grains and avoid excessively rapid growth of the grains, thereby obtaining a finer and more uniform grain structure.

[0068] Preferably, the time for the siliconizing sintering in step (5) is 0.5h to 5h, for example, it can be 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0069] The present invention specifically limits the siliconizing sintering time to 0.5h to 5h, ensuring that there is sufficient time for the reaction between metallic silicon and the silicon carbide blank to proceed, thereby achieving sufficient siliconizing sintering. The appropriate sintering time can balance production efficiency and product quality, and avoid excessively long sintering time leading to energy waste and reduced production efficiency.

[0070] As a preferred technical solution of the first aspect of the present invention, the preparation method comprises the following steps:

[0071] (1) Silicon carbide powder and graphite powder are mixed in a mass ratio of (70-100):(0.1-20) and ball milled once, using silicon carbide balls as ball milling media, and the ball-to-material mass ratio is 1:(0.5-2), and the ball-graphitizing time is 2h to 10h to obtain a coated powder; the silicon carbide powder is graded from at least one silicon carbide coarse powder and at least one silicon carbide fine powder, and the average particle size D50 of the silicon carbide coarse powder is 20μm to 150μm, the average particle size D50 of the silicon carbide fine powder is 1μm to 20μm, and the difference between the average particle size D50 of the silicon carbide coarse powder and the silicon carbide fine powder is 10μm to 100μm; the average particle size D50 of the graphite powder is 0.1μm to 10μm;

[0072] (2) mixing carbon powder, a binder, a dispersant, a suspending agent, water and the coated powder obtained in step (1) for secondary ball milling, using silicon carbide balls as ball milling media, and the ball milling time is 5h to 24h to obtain a composite slurry with a solid content of 40wt% to 65wt% and a viscosity of 300mPa·s to 1500mPa·s; the binder comprises any one of polyvinyl alcohol, polyvinyl butyral, phenolic resin or epoxy resin or a combination of at least two thereof; the dispersant comprises any one of polyvinyl pyrrolidone, tetramethylammonium hydroxide or sodium dodecyl sulfate or a combination of at least two thereof; the suspending agent comprises any one of carboxymethyl cellulose, hydroxymethyl cellulose, polyvinyl acetate or paraffin or a combination of at least two thereof; the mixing mass ratio of the carbon powder, the binder, the dispersant, the suspending agent and the water is (0.1-30):(3-20):(0.1-1):(0.1-1):(80-120);

[0073] (3) spray granulating the composite slurry obtained in step (2) in a centrifugal spray dryer, with an inlet temperature of 100° C. to 300° C., an outlet temperature of 80° C. to 120° C., an atomizer frequency of 150 Hz to 300 Hz, and a feed flow rate of 3 kg / h to 10 kg / h, to obtain a composite powder having an average particle size of 60 to 320 mesh and a water content of 0.5 wt% to 1.5 wt%;

[0074] (4) Dry-pressing the composite powder obtained in step (3) at 50 MPa to 150 MPa to obtain a density of 2 g / cm3 Up to 2.5g / cm 3 Ceramic blanks;

[0075] (5) The ceramic green body obtained in step (4) is subjected to silicon infiltration sintering, the mass ratio of the ceramic green body to metallic silicon is controlled to be 1:(0.6-1.5), the heating rate is 3°C / min to 20°C / min, and the temperature is kept at 1500°C to 1800°C for 0.5h to 5h to obtain reaction-sintered silicon carbide ceramics.

[0076] In a second aspect, the present invention provides a reaction-sintered silicon carbide ceramic prepared by the preparation method described in the first aspect, wherein the volume density of the reaction-sintered silicon carbide ceramic is ≥3.06 g / cm 3 , for example, it can be 3.06 g / cm 3 、3.07g / cm 3 、3.08g / cm 3 、3.09g / cm 3 or 3.10g / cm 3 , free silicon content ≤10.2wt%, for example, it can be 7wt%, 7.2wt%, 7.4wt%, 7.6wt%, 7.8wt%, 8wt%, 8.2wt%, 8.4wt%, 8.6wt%, 8.8wt%, 9wt%, 9.2wt%, 9.4wt%, 9.6wt%, 9.8wt%, 10wt% or 10.2wt%, and the flexural strength is ≥380MPa, for example, it can be 380MPa, 385MPa, 390MPa, 400MPa, 405MPa, 410MPa, 415MPa, 420MPa, 425MPa, 430MPa, 435MPa or 440MPa, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0077] In a third aspect, the present invention provides an application of the reaction-sintered silicon carbide ceramic as described in the second aspect, wherein the reaction-sintered silicon carbide ceramic is used in kiln manufacturing, aerospace, semiconductor industry or photovoltaic technology.

[0078] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0079] Compared with the prior art, the present invention has the following beneficial effects:

[0080] (1) The present invention eliminates the irregular edges and corners on the surface of silicon carbide particles through ball milling, so that silicon carbide gradually approaches spherical particles. Since graphite is soft, it will be coated on the surface of silicon carbide particles during the ball milling process. In addition, the crystal structure of graphite is flaky, and the bonding force between the surfaces is weak, which is easy to shear, thereby significantly reducing the friction between silicon carbide particles and improving the fluidity of the obtained powder. In addition, the molding pressure of the ceramic blank is reduced, and the damage of the hard powder to the mold and the press is avoided, ensuring production safety. At the same time, the density and internal structure uniformity of the blank are improved, and the ceramic sintering performance and the mechanical properties of ceramic products are further improved.

[0081] (2) The graphite layer on the surface of silicon carbide reacts with metallic silicon during the silicon infiltration sintering stage, and the generated β-silicon carbide is firmly adsorbed on the raw material α-silicon carbide, making the sintered silicon carbide ceramics denser and with fewer defects between particles, further improving the mechanical properties of the ceramics, extending the service life of the ceramics, and broadening the application scenarios. BRIEF DESCRIPTION OF THE DRAWINGS

[0082] Figure 1 This is the microscopic morphology of the silicon carbide powder used in the preparation method provided in Example 1;

[0083] Figure 2 This is the microscopic morphology of the coated powder obtained by the preparation method provided in Example 1;

[0084] Figure 3 This is the microscopic morphology of the composite powder obtained by the preparation method provided in Example 1;

[0085] Figure 4 This is a photo of the ceramic blank obtained by the preparation method provided in Example 1;

[0086] Figure 5 This is a photo of the reaction-sintered silicon carbide ceramic obtained by the preparation method provided in Example 1;

[0087] Figure 6 This is a metallographic photograph of the reaction-sintered silicon carbide ceramic obtained by the preparation method provided in Example 1. DETAILED DESCRIPTION

[0088] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0089] Example 1

[0090] This embodiment provides a reaction-sintered silicon carbide ceramic and a preparation method thereof, the preparation method comprising the following steps:

[0091] (1) 70 parts of silicon carbide powder with D50=60 μm, 20 parts of silicon carbide powder with D50=20 μm, 10 parts of silicon carbide powder with D50=10 μm and 10 parts of graphite powder with D50=1 μm were mixed and ball milled once, using silicon carbide balls as ball milling media, and the ball-to-material mass ratio was 1:1, and the ball-graphite time was 6 h to obtain coated powder; wherein the microscopic morphology of the silicon carbide powder is shown in Figure 1 The microstructure of the coated powder obtained after one ball milling is shown in Figure 2 ;

[0092] (2) adding 12 parts of carbon powder, 10 parts of phenolic resin (molecular weight of 800-1000), 0.5 parts of polyvinyl pyrrolidone (molecular weight of 44000-54000) and 0.5 parts of carboxymethyl cellulose (molecular weight of 5000-8000) to the coated powder obtained in step (1), and then adding 100 parts of distilled water for secondary ball milling, using silicon carbide balls as ball milling media, and the ball milling time is 16 hours, to obtain a composite slurry with a solid content of 52wt% and a viscosity of 1000mPa·s;

[0093] (3) The composite slurry obtained in step (2) was spray granulated in a centrifugal spray dryer at an inlet temperature of 200° C., an outlet temperature of 100° C., an atomizer frequency of 250 Hz, and a feed flow rate of 6 kg / h to obtain a composite powder with an average particle size of 200 mesh and a water content of 1.2 wt% (see Figure 3 );

[0094] (4) The composite powder obtained in step (3) is dry pressed at 100 MPa to obtain a ceramic blank (see Figure 4 );

[0095] (5) The ceramic blank obtained in step (4) is subjected to silicon infiltration sintering, the mass ratio of the ceramic blank to metal silicon is controlled to be 1:1.2, the heating rate is 10°C / min, and the temperature is kept at 1700°C for 2h to obtain a reaction-sintered silicon carbide ceramic (see Figure 5 ).

[0096] Figure 6 This is a metallographic photograph of the reaction-sintered silicon carbide ceramic obtained in this example.

[0097] Example 2

[0098] This embodiment provides a reaction-sintered silicon carbide ceramic and a preparation method thereof, the preparation method comprising the following steps:

[0099] (1) 65 parts of silicon carbide powder with a D50 of 60 μm, 5 parts of silicon carbide powder with a D50 of 2 μm and 15 parts of graphite powder with a D50 of 0.5 μm were mixed and ball milled once, using silicon carbide balls as ball milling media, with a ball-to-material mass ratio of 1:2, and a ball-to-graphite time of 10 h to obtain a coated powder;

[0100] (2) adding 0.1 parts of carbon powder, 3 parts of polyvinyl butyral (molecular weight of 30k-35k), 1 part of tetramethylammonium hydroxide and 0.1 parts of hydroxymethyl cellulose (molecular weight of 6000-8000) to the coated powder obtained in step (1), and then adding 120 parts of distilled water for secondary ball milling, using silicon carbide balls as ball milling media, and the ball milling time is 24 hours to obtain a composite slurry with a solid content of 40wt% and a viscosity of 300mPa·s;

[0101] (3) spray granulating the composite slurry obtained in step (2) in a centrifugal spray dryer at an inlet temperature of 100° C., an outlet temperature of 80° C., an atomizer frequency of 150 Hz, and a feed flow rate of 3 kg / h to obtain a composite powder with an average particle size of 320 mesh and a water content of 1.5 wt%;

[0102] (4) dry pressing the composite powder obtained in step (3) at 150 MPa to obtain a ceramic green body;

[0103] (5) The ceramic green body obtained in step (4) is subjected to silicon infiltration sintering, the mass ratio of the ceramic green body to metallic silicon is controlled to be 1:0.6, the heating rate is 20°C / min, and the temperature is kept at 1800°C for 2h to obtain reaction-sintered silicon carbide ceramics.

[0104] Example 3

[0105] This embodiment provides a reaction-sintered silicon carbide ceramic and a preparation method thereof, the preparation method comprising the following steps:

[0106] (1) Mix 50 parts of silicon carbide powder with D50=150 μm, 25 parts of silicon carbide powder with D50=60 μm, 10 parts of silicon carbide powder with D50=10 μm, 1 part of silicon carbide powder with D50=5 μm and 5 parts of graphite powder with D50=10 μm and perform ball milling once, using silicon carbide balls as ball milling media, and the ball-to-material mass ratio is 1:0.5, and the ball milling time is 2 h to obtain a coated powder;

[0107] (2) adding 30 parts of carbon powder, 20 parts of bisphenol A epoxy resin (molecular weight of 5000-6000), 0.1 parts of sodium dodecyl sulfate, 0.2 parts of polyvinyl acetaldehyde (molecular weight of 20k-40k) and 0.8 parts of paraffin (molecular weight of 300-400) to the coated powder obtained in step (1), and then adding 80 parts of distilled water for secondary ball milling, using silicon carbide balls as ball milling media, and the ball milling time is 5 hours, to obtain a composite slurry with a solid content of 65wt% and a viscosity of 1500mPa·s;

[0108] (3) spray granulating the composite slurry obtained in step (2) in a centrifugal spray dryer at an inlet temperature of 300° C., an outlet temperature of 120° C., an atomizer frequency of 300 Hz, and a feed flow rate of 10 kg / h to obtain a composite powder with an average particle size of 60 mesh and a water content of 0.5 wt%;

[0109] (4) dry pressing the composite powder obtained in step (3) at 50 MPa to obtain a ceramic blank;

[0110] (5) The ceramic green body obtained in step (4) is subjected to silicon infiltration sintering, the mass ratio of the ceramic green body to metallic silicon is controlled to be 1:1.5, the heating rate is 3°C / min, and the temperature is kept at 1500°C for 5 hours to obtain reaction-sintered silicon carbide ceramics.

[0111] Example 4

[0112] This embodiment provides a reaction-sintered silicon carbide ceramic and a preparation method thereof. Except that the silicon carbide powders of various particle sizes in step (1) are uniformly replaced with 100 parts of silicon carbide powder with D50=20 μm, the remaining steps and conditions are the same as those in Example 1 and are not described in detail here.

[0113] Example 5

[0114] This embodiment provides a reaction-sintered silicon carbide ceramic and a preparation method thereof. Except that the mass fraction of graphite powder in step (1) is changed to 25 parts, the remaining steps and conditions are the same as those in Example 1, and thus are not described in detail here.

[0115] Example 6

[0116] This embodiment provides a reaction-sintered silicon carbide ceramic and a preparation method thereof. Except that the average particle size D50 of the graphite powder in step (1) is changed to 15 μm, the remaining steps and conditions are the same as those in Example 1, and thus are not described in detail here.

[0117] Example 7

[0118] This embodiment provides a reaction-sintered silicon carbide ceramic and a preparation method thereof. Except that the average particle size D50 of the graphite powder in step (1) is changed to 0.1 μm, the remaining steps and conditions are the same as those in Example 1, and thus are not described in detail here.

[0119] Example 8

[0120] This embodiment provides a reaction-sintered silicon carbide ceramic and a preparation method thereof. Except that the mass ratio of the ceramic blank to the metallic silicon in step (5) is changed to 1:0.4, the remaining steps and conditions are the same as those in Example 1 and are not described in detail here.

[0121] Comparative Example 1

[0122] This comparative example provides a reaction-sintered silicon carbide ceramic and a preparation method thereof. Except that no graphite powder is added in step (1), that is, silicon carbide powders of various particle sizes are directly ball-milled once, the remaining steps and conditions are the same as those in Example 1, and thus are not described in detail here.

[0123] Comparative Example 2

[0124] This comparative example provides a reaction-sintered silicon carbide ceramic and a preparation method thereof. Except for directly mixing the silicon carbide powders of various particle sizes in step (1) with the various raw materials in step (2) and ball milling them, the remaining steps and conditions are the same as those in Example 1 and are not described in detail here.

[0125] Comparative Example 3

[0126] This comparative example provides a reaction-sintered silicon carbide ceramic and a preparation method thereof. Except for mixing the silicon carbide powder and graphite powder of various particle sizes in step (1) and the various raw materials in step (2) at one time and ball milling, the remaining steps and conditions are the same as those in Example 1, and thus are not described in detail here.

[0127] After testing, the relevant physical property parameters of the intermediate products and final products obtained in Examples 1-8 and Comparative Examples 1-3 are shown in Table 1 below.

[0128] Table 1

[0129]

[0130] In the above table, the angle of repose and the bulk density refer to the angle of repose and the bulk density of the composite powder obtained after the composite slurry is spray granulated, respectively; the bulk density, the free silicon content and the flexural strength refer to the bulk density, the free silicon content and the flexural strength of silicon carbide ceramics, respectively; wherein, the detection method of the flexural strength refers to GB / T6569-2006 Fine Ceramics Flexural Strength Test Method.

[0131] From Table 1, we can see that:

[0132] (1) The angle of repose of the composite powder obtained in Examples 1-3 is 26°-27.3°, that is, the powder has good fluidity and a bulk density of 0.85-0.9 g / cm 3 , that is, the powder is packed tightly; the density of the obtained ceramic blank is 2.05-2.2g / cm 3 The volume density of the obtained silicon carbide ceramic is 3.06-3.1g / cm 3 , free silicon content is 7.64-10.2wt%, and flexural strength is 382-438MPa.

[0133] (2) Compared with Example 1, in Example 4, the silicon carbide powders of various particle sizes in step (1) are uniformly replaced by 100 parts of silicon carbide powder with D50 = 20 μm, that is, the silicon carbide powder is not obtained by grading the silicon carbide coarse powder and the silicon carbide fine powder of different particle sizes. As a result, the loose density of the composite powder obtained in Example 4 is significantly reduced, and the density of the obtained ceramic blank and the volume density of the silicon carbide ceramic are reduced to varying degrees. The flexural strength of the silicon carbide ceramic finally obtained is significantly lower than that of Example 1.

[0134] (3) Compared with Example 1, in Example 5, the mass fraction of graphite powder in step (1) is changed to 25 parts, that is, the mixing mass ratio of silicon carbide powder and graphite powder is changed to 100:25. Although the angle of repose of the composite powder obtained in Example 5 is further reduced and the loose density is further increased, that is, the fluidity and filling density of the powder are better than those in Example 1, the density of the obtained ceramic blank and the volume density of the silicon carbide ceramic are both lower than those in Example 1, and the free silicon content is significantly increased, and the flexural strength is significantly reduced.

[0135] (4) Compared with Example 1, the average particle size D50 of the graphite powder was adjusted in Examples 6 and 7, respectively. As a result, the fluidity and filling density of the obtained composite powder were deteriorated, and the density of the obtained ceramic blank and the volume density of the silicon carbide ceramic were both lower than those in Example 1, the free silicon content was significantly increased, and the flexural strength was significantly reduced.

[0136] (5) Compared with Example 1, in Example 8, the mass ratio of the ceramic blank and metallic silicon in step (5) is changed to 1:0.4, resulting in a significant decrease in the volume density of the obtained silicon carbide ceramic, a significant increase in the free silicon content, and a significant decrease in the flexural strength.

[0137] (6) Compared with Example 1, in Comparative Example 1, no graphite powder was added in step (1), that is, silicon carbide powders of various particle sizes were directly ball-milled once. As a result, the fluidity and filling density of the obtained composite powder were deteriorated, and the density of the obtained ceramic blank and the volume density of the silicon carbide ceramic were both lower than those of Example 1, the free silicon content was significantly increased, and the flexural strength was significantly reduced.

[0138] (7) Compared with Example 1, in Comparative Example 2, the silicon carbide powder of various particle sizes in step (1) is directly mixed with the various raw materials in step (2) and ball milled. As a result, the fluidity and filling density of the obtained composite powder are deteriorated, and the density of the obtained ceramic blank and the volume density of the silicon carbide ceramic are both lower than those in Example 1, the free silicon content is significantly increased, and the flexural strength is significantly reduced.

[0139] (8) Compared with Example 1, in Comparative Example 3, the silicon carbide powder and graphite powder of various particle sizes in step (1) are mixed with the various raw materials in step (2) at one time and ball milled. As a result, the fluidity and filling density of the obtained composite powder are deteriorated, and the density of the obtained ceramic blank and the volume density of the silicon carbide ceramic are both lower than those in Example 1, the free silicon content is significantly increased, and the flexural strength is significantly reduced.

[0140] It can be seen that the present invention eliminates the irregular edges and corners on the surface of silicon carbide particles through ball milling, so that silicon carbide gradually approaches spherical particles. Since graphite is soft, it will be coated on the surface of silicon carbide particles during the ball milling process. In addition, the crystal structure of graphite is flaky, and the bonding force between the surfaces is weak, so shearing is easily caused, thereby significantly reducing the friction between silicon carbide particles and improving the fluidity of the obtained powder, thereby reducing the molding pressure of the ceramic blank, avoiding damage to the mold and the press by the hard powder, ensuring production safety, and at the same time improving the density and internal structure uniformity of the blank, further improving the ceramic sintering performance and the mechanical properties of ceramic products.

[0141] In addition, the graphite layer on the surface of silicon carbide reacts with metallic silicon during the sintering stage, and the resulting β-silicon carbide is firmly adsorbed on the raw material α-silicon carbide, making the sintered silicon carbide ceramics denser and with fewer defects between particles, further improving the mechanical properties of the ceramics, extending the service life of the ceramics, and broadening the application scenarios.

[0142] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing reaction-sintered silicon carbide ceramics, It is characterized in that The preparation method comprises the following steps: (1) mixing silicon carbide powder and graphite powder and performing a ball milling to obtain a coated powder; (2) mixing carbon powder, a binder, a dispersant, a suspending agent, water and the coated powder obtained in step (1) and performing secondary ball milling to obtain a composite slurry; (3) spray granulating the composite slurry obtained in step (2) to obtain a composite powder; (4) dry-pressing the composite powder obtained in step (3) to obtain a ceramic blank; (5) The ceramic green body obtained in step (4) is subjected to silicon infiltration and sintering to obtain reaction-sintered silicon carbide ceramics.

2. The preparation method according to claim 1, It is characterized in that The silicon carbide powder in step (1) is graded from at least one silicon carbide coarse powder and at least one silicon carbide fine powder; Preferably, the average particle size D50 of the silicon carbide coarse powder is 20 μm to 150 μm; Preferably, the average particle size D50 of the silicon carbide fine powder is 1 μm to 20 μm; Preferably, the difference in average particle size D50 between the coarse silicon carbide powder and the fine silicon carbide powder is 10 μm to 100 μm; Preferably, the average particle size D50 of the graphite powder in step (1) is 0.1 μm to 10 μm; Preferably, the mixing mass ratio of the silicon carbide powder and the graphite powder in step (1) is (70-100):(0.1-20); Preferably, the first ball milling in step (1) uses silicon carbide balls as ball milling media; Preferably, the mass ratio of ball to material in the first ball milling in step (1) is 1:(0.5-2); Preferably, the time for the first ball milling in step (1) is 2 h to 10 h.

3. The preparation method according to claim 1 or 2, It is characterized in that The binder in step (2) comprises any one of polyvinyl alcohol, polyvinyl butyral, phenolic resin or epoxy resin, or a combination of at least two thereof; Preferably, the dispersant in step (2) comprises any one of polyvinyl pyrrolidone, tetramethylammonium hydroxide or sodium dodecyl sulfate, or a combination of at least two thereof; Preferably, the suspending agent in step (2) comprises any one of carboxymethyl cellulose, hydroxymethyl cellulose, polyvinyl acetate or paraffin, or a combination of at least two thereof.

4. The preparation method according to any one of claims 1 to 3, It is characterized in that The mixing mass ratio of the carbon powder, binder, dispersant, suspending agent and water in step (2) is (0.1-30):(3-20):(0.1-1):(0.1-1):(80-120); Preferably, the secondary ball milling in step (2) uses silicon carbide balls as ball milling media; Preferably, the time of the secondary ball milling in step (2) is 5 h to 24 h; Preferably, the solid content of the composite slurry in step (2) is 40wt% to 65wt%; Preferably, the viscosity of the composite slurry in step (2) is 300 mPa·s to 1500 mPa·s.

5. The preparation method according to any one of claims 1 to 4, It is characterized in that The spray granulation in step (3) is carried out in a centrifugal spray dryer, and the inlet temperature of the centrifugal spray dryer is 100° C. to 300° C., the outlet temperature is 80° C. to 120° C., and the atomizer frequency is 150 Hz to 300 Hz; Preferably, the feed rate of the spray granulation in step (3) is 3 kg / h to 10 kg / h; Preferably, the average particle size of the composite powder in step (3) is 60 mesh to 320 mesh; Preferably, the water content of the composite powder in step (3) is 0.5wt% to 1.5wt%.

6. The preparation method according to any one of claims 1 to 5, It is characterized in that The pressure of the dry pressing in step (4) is 50 MPa to 150 MPa; Preferably, the density of the ceramic blank in step (4) is 2 g / cm 3 Up to 2.5g / cm 3 .

7. The preparation method according to any one of claims 1 to 6, It is characterized in that During the siliconizing and sintering process of step (5), the mass ratio of the ceramic blank to the metallic silicon is 1:(0.6-1.5); Preferably, the heating rate of the siliconizing sintering in step (5) is 3°C / min to 20°C / min; Preferably, the temperature of the siliconizing sintering in step (5) is 1500° C. to 1800° C.; Preferably, the siliconizing and sintering time in step (5) is 0.5 h to 5 h.

8. The preparation method according to any one of claims 1 to 7, It is characterized in that The preparation method comprises the following steps: (1) Silicon carbide powder and graphite powder are mixed in a mass ratio of (70-100):(0.1-20) and ball milled once, using silicon carbide balls as ball milling media, and the ball-to-material mass ratio is 1:(0.5-2), and the ball-graphitizing time is 2h to 10h to obtain a coated powder; the silicon carbide powder is graded from at least one silicon carbide coarse powder and at least one silicon carbide fine powder, and the average particle size D50 of the silicon carbide coarse powder is 20μm to 150μm, the average particle size D50 of the silicon carbide fine powder is 1μm to 20μm, and the difference between the average particle size D50 of the silicon carbide coarse powder and the silicon carbide fine powder is 10μm to 100μm; the average particle size D50 of the graphite powder is 0.1μm to 10μm; (2) mixing carbon powder, a binder, a dispersant, a suspending agent, water and the coated powder obtained in step (1) for secondary ball milling, using silicon carbide balls as ball milling media, and the ball milling time is 5h to 24h to obtain a composite slurry with a solid content of 40wt% to 65wt% and a viscosity of 300mPa·s to 1500mPa·s; the binder comprises any one of polyvinyl alcohol, polyvinyl butyral, phenolic resin or epoxy resin or a combination of at least two thereof; the dispersant comprises any one of polyvinyl pyrrolidone, tetramethylammonium hydroxide or sodium dodecyl sulfate or a combination of at least two thereof; the suspending agent comprises any one of carboxymethyl cellulose, hydroxymethyl cellulose, polyvinyl acetate or paraffin or a combination of at least two thereof; the mixing mass ratio of the carbon powder, the binder, the dispersant, the suspending agent and the water is (0.1-30):(3-20):(0.1-1):(0.1-1):(80-120); (3) spray granulating the composite slurry obtained in step (2) in a centrifugal spray dryer, with an inlet temperature of 100° C. to 300° C., an outlet temperature of 80° C. to 120° C., an atomizer frequency of 150 Hz to 300 Hz, and a feed flow rate of 3 kg / h to 10 kg / h, to obtain a composite powder having an average particle size of 60 to 320 mesh and a water content of 0.5 wt% to 1.5 wt%; (4) Dry-pressing the composite powder obtained in step (3) at 50 MPa to 150 MPa to obtain a density of 2 g / cm 3 Up to 2.5g / cm 3 Ceramic blanks; (5) The ceramic green body obtained in step (4) is subjected to silicon infiltration sintering, the mass ratio of the ceramic green body to metallic silicon is controlled to be 1:(0.6-1.5), the heating rate is 3°C / min to 20°C / min, and the temperature is kept at 1500°C to 1800°C for 0.5h to 5h to obtain reaction-sintered silicon carbide ceramics.

9. A reaction-bonded silicon carbide ceramic prepared by the preparation method according to any one of claims 1 to 8, It is characterized in that The volume density of the reaction-sintered silicon carbide ceramic is ≥3.06 g / cm 3 , free silicon content ≤10.2wt%, flexural strength ≥380MPa.

10. An application of the reaction-sintered silicon carbide ceramic as claimed in claim 9, It is characterized in that The reaction-sintered silicon carbide ceramics are used in kiln furniture manufacturing, aerospace, the semiconductor industry or photovoltaic technology.

Citation Information

Patent Citations

  • Low-cost light-weight highly-bulletproof B4C / SiC composite ceramic bulletproof plate and preparation method thereof

    CN105601280A

  • Preparation method of silicon carbide composite ceramic

    CN107778012A

  • Heat-resistant and wear-resistant member for 3-5 group compound semiconductor manufacturing apparatus

    JP2010153699A

  • Manufacturing Method of Silicon Carbide Ceramic Seals byLiquid Phase Reaction Sintering

    KR1020000067656A

Cited By

  • Silicon carbide ceramic material with complex shape and preparation method thereof

    CN120081671A

  • Complex shaped silicon carbide ceramic material and method for producing the same

    CN120081671B

  • A double-sided slip casting process for reaction-sintered silicon carbide ceramics