Nanometer material modified adsorbent for layered oil-water and emulsion efficient separation and adsorption as well as preparation method and application of nanometer material modified adsorbent

Through the use of nanomaterial modified composite adsorbents, the problem of low removal efficiency of oil-based substances in stratified oil and water and emulsions is solved, efficient separation and oil recovery are achieved, and water quality and resource utilization efficiency are improved.

CN119039536APending Publication Date: 2024-11-29SOUTHWEST PETROLEUM UNIV

Patent Information

Application Number
CN202411351633.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently remove oily substances in stratified oil and water and emulsions, resulting in water pollution and waste of resources. The existing resin technology has inefficient efficiency and insufficient recycling capabilities in oil recovery and water quality improvement.

Method used

Using nanomaterial modified composite adsorbent, the modified nanotitanium dioxide and nanosilicon dioxide are combined with acrylate-based materials to form a composite adsorbent with a porous structure, and the hydrophobicity and photocatalytic capacity are used to improve oil-water separation efficiency and oil recovery rate. .

Benefits of technology

It realizes efficient separation and adsorption of layered oil and water and emulsion, improves oil and water separation rate and efficiency, and enhances the oil absorption ratio and emulsion demulsification performance of the resin through the modification of nanomaterials, and the separation efficiency is only reduced by 7.58% during recycling. , significantly improving the effect of resource recycling and water quality improvement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039536A_ABST
    Figure CN119039536A_ABST
Patent Text Reader

Abstract

The invention discloses a nano-material modified composite adsorbent as well as a preparation method and application thereof. Raw materials comprise an oil phase and a water phase, wherein the oil phase is prepared from methyl acrylate, butyl methacrylate, hexadecyl methacrylate, modified nano titanium dioxide, modified nano silicon dioxide, an initiator and a cross-linking agent; the water phase comprises a dispersing agent and water. Inorganic modified materials titanium dioxide and silicon dioxide are introduced into an acrylate polymerization system, the porous structure of the resin is enriched, the oil absorption rate and the oil absorption rate of the resin are increased, meanwhile, the stability of the resin can be enhanced, and the cyclic utilization performance of the resin is improved; the addition of the nano material forms a part of silicon-based ternary block structure, so that the separation capacity of the oil-absorbing resin emulsion is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a nano material modified composite adsorbent for efficient separation and adsorption of stratified oil-water and emulsions and applications thereof. Background Art

[0002] Separated oil-water and emulsified oil are common types of wastewater generated in industrial processes and production activities. These wastewaters contain oil substances and cause pollution to the environment and water resources.

[0003] The presence of stratified oil-water and emulsified oil can cause water pollution and have adverse effects on the aquatic ecosystem. Oil pollution can destroy the ecological balance of microorganisms in the water and threaten the survival of aquatic organisms. These oil loads can be removed by using resins, which can effectively reduce water pollution and protect the ecological environment of the water body. At the same time, the oil in stratified oil-water and emulsified oil contains recoverable value. By using resins to remove oil loads, useful components in wastewater can be recovered, thereby reducing dependence on resources such as crude oil. This is in line with the concept of sustainable development and promotes the effective use of resources. By removing oil, resin technology also helps to improve the overall water quality of the water body. Clear water is not only beneficial to the ecosystem, but also improves the sustainable use of water resources and meets the quality standards for drinking water and agricultural water.

[0004] Therefore, providing a composite adsorbent for efficient separation and adsorption of stratified oil-water and emulsions and a preparation method thereof is a problem to be solved by those skilled in the art. Summary of the invention

[0005] The present invention aims to provide a nano-material modified composite adsorbent for high-efficiency separation and adsorption of stratified oil-water and emulsions, and a preparation method and application thereof.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] A nano-material modified composite adsorbent for high-efficiency separation and adsorption of oil-water and emulsion, the raw materials of which include an oil phase and a water phase;

[0008] The oil phase comprises, by weight, 6-8 parts of methyl acrylate, 6-8 parts of butyl methacrylate, 4-6 parts of hexadecyl methacrylate, 0.5-1.5 parts of modified nano titanium dioxide, 0.5-1.5 parts of modified nano silicon dioxide, 0.5-1.0 parts of initiator, and 0.5-1 parts of crosslinking agent;

[0009] The aqueous phase comprises: by weight, 0.1-0.5 parts of dispersant and 15-30 parts of water.

[0010] The nano material modified composite adsorbent for high-efficiency separation and adsorption of stratified oil-water and emulsion prepared by the invention has fast oil absorption rate and high oil-water separation efficiency.

[0011] The saturated adsorption experiment of the composite adsorbent was carried out at room temperature, and benzene, styrene, toluene, tetrachloromethane, dichloromethane and chloroform were tested. The experimental results show that the adsorption time of the resin for tetrachloromethane, dichloromethane and chloroform is 5h, and the saturated oil absorption ratio is 41.72, 44.36 and 54.7g / g, while the saturated adsorption time for benzene, styrene and toluene is 6h, and the saturated oil absorption ratio is 32.13, 30.17 and 34.25g / g.

[0012] Under room temperature conditions, with a surfactant content of 4000 mg / L, an oil content of 3 wt%, a separation time of 6 h, and a resin dosage of 4 g / L, the separation efficiency of the solid adsorbent for CTAB-stabilized water-toluene emulsified oil is 97.78%; after four cycles of the solid adsorbent, the separation efficiency is still 90.2%, with the separation efficiency only decreasing by 7.58%.

[0013] Preferably, the modified nano-titanium dioxide and modified nano-silicon dioxide are products obtained by hydrophobically modifying hydrophilic titanium dioxide and hydrophilic silicon dioxide nanoparticles using a silane coupling agent.

[0014] Preferably, the specific preparation steps of the modified nano titanium dioxide are as follows: adding a silane coupling agent to a hydrophilic titanium dioxide suspension, stirring and reacting for 1-2 hours, washing and drying to obtain the modified nano titanium dioxide. The specific preparation steps of the modified nano silicon dioxide are as follows: adding a silane coupling agent to a hydrophilic silicon dioxide suspension, stirring and reacting for 4-6 hours, washing and drying to obtain the modified nano silicon dioxide.

[0015] Preferably, the concentration of the hydrophilic titanium dioxide suspension is 200 g / L, and the concentration of the hydrophilic silicon dioxide suspension is 10 g / L;

[0016] The amount of the silane coupling agent added is 0.8% of the volume of the hydrophilic titanium dioxide suspension, and the amount of the silane coupling agent added is 2% of the volume of the hydrophilic silicon dioxide suspension;

[0017] The silane coupling agent used in the modified nano titanium dioxide is KH-570, and the silane coupling agent used in the modified nano silicon dioxide is KH-171; KH-570 and KH-171 have a double bond structure, so that the inorganic nanoparticles modified by the silane coupling agent can participate in the acrylate polymerization reaction;

[0018] The stirring speed is 500 r / min, which ensures that the hydrophilic titanium dioxide and the hydrophilic silicon dioxide can be chemically bonded with the silane coupling agent in a dispersed and non-aggregated form;

[0019] The reaction temperature is 40-50°C; the temperature for hydrophobic modification of hydrophilic titanium dioxide and hydrophilic silicon dioxide should not be too high. Too high a temperature will lead to enhanced interaction between nanoparticles, resulting in particle agglomeration, affecting the uniform dispersion of the modifier and reducing the modification effect. Chemical substances used for surface hydrophobic modification are sensitive to high temperatures and may have poor stability at high temperatures, resulting in a weakening or failure of the modification effect.

[0020] Preferably, the preparation method of the hydrophilic titanium dioxide suspension is: adding the hydrophilic titanium dioxide to the dispersion medium, removing the supernatant after ultrasonic treatment, and continuing to add the dispersion medium until the concentration of the suspension is 200g / L. The preparation method of the hydrophilic silicon dioxide suspension is: adding the hydrophilic silicon dioxide to the dispersion medium, removing the supernatant after ultrasonic treatment, and continuing to add the dispersion medium until the concentration of the suspension is 10g / L.

[0021] Preferably, the hydrophilic titanium dioxide dispersion medium is a mixture of anhydrous ethanol and deionized water in a volume ratio of 1:1, and the hydrophilic silicon dioxide dispersion medium is anhydrous ethanol;

[0022] The ultrasonic treatment temperature is room temperature, the frequency is 35kHz, and the time is 1-2h;

[0023] The particle size of the hydrophilic titanium dioxide and hydrophilic silicon dioxide is 40-50 nm.

[0024] Hydrophilic titanium dioxide and hydrophilic silicon dioxide are selected for modification because of their special properties and advantages, which are suitable for a variety of scenarios. They both have a high specific surface area, which can increase the contact area with the target adsorbate and improve the reactivity of adsorption. Both nanomaterials have good chemical and thermal stability and can maintain their properties under different environmental conditions. This is the key to ensuring the long-term stability of materials in various applications. At the same time, titanium dioxide and silicon dioxide generally have high mechanical strength, which helps to enhance the mechanical properties of the base material. Titanium dioxide has excellent absorption performance for ultraviolet light, and the photocatalytic ability of titanium dioxide further enhances the material's destructive performance on the oil-water interface.

[0025] Preferably, the initiator is benzoyl peroxide;

[0026] The cross-linking agent is N,N-dimethylbisacrylamide;

[0027] The dispersant used is polyvinyl alcohol, which is a surfactant with amphiphilicity. Under mechanical stirring, polyvinyl alcohol allows the oil phase to be stably suspended in the dispersed phase water in the form of spherical droplets, achieving polymerization in droplets. In addition, organic substances with amphiphilic properties, which do not participate in the acrylate polymerization system and can be removed by simple physical or chemical methods after polymerization, such as hexadecyl trimethyl ammonium bromide, can be considered as substitutes.

[0028] According to the above-mentioned method for preparing a nanomaterial modified composite adsorbent for efficient separation and adsorption of stratified oil-water and emulsion, it is characterized by comprising the following specific steps:

[0029] (1) Weighing raw materials by weight: 6-8 parts of methyl acrylate, 6-8 parts of butyl methacrylate, 4-6 parts of hexadecyl methacrylate, 0.5-1.5 parts of modified nano titanium dioxide, 0.5-1.5 parts of modified nano silicon dioxide, 0.5-1.0 parts of initiator, 0.5-1 parts of crosslinking agent, 0.1-0.5 parts of dispersant, and 15-30 parts of water;

[0030] (2) uniformly mixing the methyl acrylate, the butyl methacrylate, the hexadecyl methacrylate, the modified nano titanium dioxide, the modified nano silicon dioxide, the initiator, and the crosslinking agent to obtain an oil phase;

[0031] (3) dissolving the dispersant in the water, stirring and dissolving to obtain an aqueous phase;

[0032] (4) adding the oil phase dropwise to the water phase and stirring to form uniform droplets of the oil phase in the water phase. After reacting for 4-5 hours, cooling, washing and drying are performed in sequence to obtain a solid adsorbent.

[0033] Preferably, the dissolving temperature in step (3) is 40°C;

[0034] The reaction temperature in step (4) is 75-80° C. under a nitrogen environment;

[0035] The drying in step (4) is performed at 40-50° C. until the product reaches a constant weight.

[0036] Preferably, the method of use is: immersing the composite adsorbent in an organic liquid, then leaving it for a certain period of time, and taking out the composite adsorbent after separation is completed. Immersing the composite adsorbent in emulsified oil, placing it in an air shaker for shaking and separation for a certain period of time, and taking out the composite adsorbent after separation is completed.

[0037] Preferably, the organic liquid is toluene, and the emulsified oil is an O / W type emulsified toluene / water mixture.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] The present invention discloses a composite adsorbent with high-efficiency separation and adsorption functions for stratified oil-water and emulsions and a preparation method thereof. Inorganic material-modified nano titanium dioxide and modified nano silicon dioxide are introduced into an acrylate polymerization system to enrich the porous structure of the composite adsorbent, thereby enhancing the oil absorption ratio and oil absorption rate of the resin; in addition, the addition of nano materials forms a partial silicon-based ternary block structure to enhance the emulsion separation ability of the oil-absorbing resin, and at the same time, the photocatalytic ability of titanium dioxide further enhances the demulsification performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. The drawings in this description are only embodiments of the present invention.

[0041] Figure 1 The comparative scanning electron microscope images of Comparative Example 1 and Example 1 of the present invention are shown;

[0042] Figure 2 This is a comparison diagram of the composite adsorbent before and after demulsification of CTAB-stabilized toluene-in-water emulsified oil by Example 1 of the present invention;

[0043] Figure 3 This is a comparison diagram of the composite adsorbent before and after the adsorption of toluene on the water surface in Example 1 of the application example of the present invention. DETAILED DESCRIPTION

[0044] Embodiments of the present invention are described below. Examples of the embodiments are shown in the accompanying drawings. The embodiments described with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, but are not to be construed as limiting the present invention.

[0045] Example 1

[0046] A method for preparing a nanomaterial-modified composite adsorbent for efficient separation and adsorption of stratified oil-water and emulsions, specifically comprising the following steps:

[0047] (1) Accurately add 30 mL of distilled water and 0.030 g of polyvinyl alcohol into a three-necked flask, heat to 35° C. and immerse in ultrasound for 15 min until the mixture is completely dissolved to obtain an aqueous phase;

[0048] (2) 4.5 g of hexadecyl methacrylate, 5.25 g of methyl acrylate, 5.25 g of butyl methacrylate, 0.150 g of benzoyl peroxide, 0.165 g of N,N-methylenebisacrylamide, 0.12 g of modified nano titanium dioxide, and 0.18 g of modified nano silicon dioxide were mixed to obtain an oil phase;

[0049] (3) adding the oil phase to the water phase, heating to 76°C under a nitrogen environment, and allowing the oil phase to form uniform droplets in the water under mechanical stirring at 200 r / min for 4 hours; after the product is cooled to room temperature, washing with anhydrous ethanol and deionized water, and vacuum drying in an oven at 40°C to constant weight, a composite adsorbent is obtained;

[0050] The preparation method of modified nano titanium dioxide comprises the following specific steps:

[0051] 1) Prepare 50 mL of anhydrous ethanol-water solution in a ratio of 1:1 as a dispersion medium;

[0052] 2) Weigh 5 g of hydrophilic titanium dioxide (50 nm) into 25 mL of dispersion medium, and perform ultrasonic treatment at room temperature and 35 kHz for 1 h to remove excess impurities on the particle surface. After the ultrasonic treatment, remove the supernatant and continue to add dispersion medium to 25 mL to obtain a hydrophilic titanium dioxide suspension;

[0053] 3) Add 50 mL of KH-570 to the hydrophilic titanium dioxide suspension obtained in step 2), react for 1.5 h at 40 ° C, constant temperature and sealed, and 500 r / min strong stirring conditions, cool and separate the solid and liquid, wash the obtained solid particles three times with anhydrous ethanol, and dry at 60 ° C for 8 h to obtain modified nano titanium dioxide.

[0054] The preparation method of modified nano silicon dioxide comprises the following specific steps:

[0055] 1) Measure 500 mL of anhydrous ethanol as a dispersion medium;

[0056] 2) Weigh 2 g of hydrophilic titanium dioxide (50 nm) into 200 mL of dispersion medium, and perform ultrasonic treatment at room temperature and 35 kHz for 1 h to remove excess impurities on the particle surface. After the ultrasonic treatment, remove the supernatant and continue to add dispersion medium to 200 mL to obtain a hydrophilic titanium dioxide suspension;

[0057] 3) Add 50 mL of KH-171 to the hydrophilic titanium dioxide suspension obtained in step 2), react for 1.5 h at 40 ° C, constant temperature and closed, and 500 r / min strong stirring conditions, cool and separate the solid and liquid, wash the obtained solid particles three times with anhydrous ethanol, and dry at 60 ° C for 8 h to obtain modified nano-silica.

[0058] Figure 1The following are scanning electron microscope images of the prepared composite adsorbent, wherein (d) is a surface morphology image of the adsorbent in Example 1 at a magnification of 1KX, (e) is a surface morphology image of the adsorbent in Example 1 at a magnification of 2KX, and (f) is a surface morphology image of the adsorbent in Example 1 at a magnification of 5KX. As shown in the figure, the polymer has a large number of holes and pores of rich types after being modified with nanomaterials.

[0059] Example 2

[0060] A method for preparing a nanomaterial-modified composite adsorbent for efficient separation and adsorption of stratified oil-water and emulsions, specifically comprising the following steps:

[0061] (1) Accurately add 30 mL of distilled water and 0.030 g of polyvinyl alcohol into a three-necked flask, heat to 35° C. and immerse in ultrasound for 15 min until the mixture is completely dissolved to obtain an aqueous phase;

[0062] (2) 4.5 g of hexadecyl methacrylate, 5.25 g of methyl acrylate, 5.25 g of butyl methacrylate, 0.150 g of benzoyl peroxide, 0.165 g of N,N-methylenebisacrylamide and 0.06 g of modified nano-titanium dioxide were mixed uniformly (the preparation method was the same as that in Example 1) to obtain an oil phase;

[0063] (3) adding the oil phase to the water phase, heating to 76°C under a nitrogen environment, and allowing the oil phase to form uniform droplets in the water under mechanical stirring at 200 r / min for 4 hours; after the product is cooled to room temperature, washing with anhydrous ethanol and deionized water, and vacuum drying in an oven at 40°C to constant weight, a composite adsorbent is obtained;

[0064] Example 3

[0065] A method for preparing a nanomaterial-modified composite adsorbent for efficient separation and adsorption of stratified oil-water and emulsions, specifically comprising the following steps:

[0066] (1) Accurately add 30 mL of distilled water and 0.030 g of polyvinyl alcohol into a three-necked flask, heat to 35° C. and immerse in ultrasound for 15 min until the mixture is completely dissolved to obtain an aqueous phase;

[0067] (2) 4.5 g of hexadecyl methacrylate, 5.25 g of methyl acrylate, 5.25 g of butyl methacrylate, 0.150 g of benzoyl peroxide, 0.165 g of N,N-methylenebisacrylamide and 0.18 g of modified nano-silica were mixed uniformly (the preparation method was the same as that in Example 1) to obtain an oil phase;

[0068] (3) The oil phase was added to the water phase, the temperature was raised to 76°C under a nitrogen environment, and the oil phase was allowed to form uniform droplets in the water under mechanical stirring at 200 r / min, and the reaction was continued for 4 hours. After the product was cooled to room temperature, it was washed with anhydrous ethanol and deionized water, and vacuum dried in an oven at 40°C to constant weight to obtain a composite adsorbent.

[0069] Comparative Example 1

[0070] A method for preparing a solid adsorbent comprises the following steps:

[0071] (1) Accurately add 30 mL of distilled water and 0.030 g of polyvinyl alcohol into a three-necked flask, heat to 35°C and immerse in ultrasound for 15 min until completely dissolved to obtain an aqueous phase;

[0072] (2) 4.5 g of hexadecyl methacrylate, 5.25 g of methyl acrylate, 5.25 g of butyl methacrylate, 0.150 g of benzoyl peroxide, and 0.165 g of N,N-methylenebisacrylamide were mixed to obtain an oil phase;

[0073] (3) The oil phase was added to the water phase, the temperature was raised to 76°C under a nitrogen environment, and the oil phase was allowed to form uniform droplets in the water under mechanical stirring at 200 r / min, and the reaction was continued for 4 hours. After the product was cooled to room temperature, it was washed with anhydrous ethanol and deionized water, and vacuum dried in an oven at 40°C to constant weight to obtain a composite adsorbent.

[0074] Figure 1 The following are scanning electron microscope images of the prepared composite adsorbent, wherein (a) is a surface morphology image of the adsorbent in comparative example 1, at a magnification of 1KX, (b) is a surface morphology image of the adsorbent in comparative example 1, at a magnification of 2KX, and (c) is a surface morphology image of the adsorbent in comparative example 1, at a magnification of 5KX. As shown in the figure, the polymer has a rough wrinkled surface and a certain number of microporous structures before being modified by nanomaterials.

[0075] Application Examples

[0076] Disperse 2 parts of surfactant hexadecyltrimethylammonium bromide (CTAB) in 500 parts of water, add 3 parts of toluene after complete dissolution, and stir continuously for 10 minutes at room temperature with a stirring speed of 1000-1500 rpm to obtain surfactant-stabilized O / W toluene / water emulsified oil;

[0077] The adsorbents prepared in Examples 1-3 and Comparative Example 1 were added to the emulsified oil at 5 g / L, and then the reagent bottles were placed in an air shaker for emulsion separation for 4 hours, and then the solid adsorbent was taken out. The oil content of the separated emulsified oil was determined by ultraviolet spectrophotometry; at the same time, the recyclability of the solid adsorbent was studied, and the relevant results are as follows:

[0078] The separation efficiency of the composite adsorbent for CTAB-stabilized toluene-in-water emulsion is 98.4%; the saturated separation time is 6 hours. In addition, the composite adsorbent is recycled for 5 times, and the separation efficiency is still 90.2%, and the separation efficiency is only reduced by 7.58%. After 7 regeneration cycles, the separation efficiency is reduced to 70.23%. ; Among them, if Figure 2 This is a comparison chart of the composite adsorbent in Example 1 before and after demulsification of CTAB-stabilized toluene-in-water emulsified oil. Figure 3 This is a comparison diagram of toluene on the water surface before and after the composite adsorbent of Example 1. As can be seen from the figure, the composite adsorbent has good separation performance of stratified oil-water and emulsified oil.

[0079] The separation efficiency of the composite adsorbent for CTAB-stabilized toluene-in-water emulsion is 37.4% and the saturated separation time is 6 hours. In addition, the composite adsorbent is recycled for 5 times, and the separation efficiency is still 30.6%, and the separation efficiency is only reduced by 6.8%.

[0080] The separation efficiency of the composite adsorbent for CTAB-stabilized toluene-in-water emulsion is 92.3% and the saturated separation time is 8h. In addition, the composite adsorbent is recycled for 5 times, and the separation efficiency is still 84.6%, and the separation efficiency is only reduced by 7.7%.

[0081] The separation efficiency of the solid adsorbent of Comparative Example 1 for CTAB-stabilized toluene-in-water emulsion was 28.7% and the saturated separation time was 8h. In addition, the composite adsorbent was recycled for 5 times, and the separation efficiency was still 21.2%, and the separation efficiency only decreased by 7.5%.

[0082] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A nanomaterial modified composite adsorbent for efficient separation and adsorption of oil-water and emulsion, characterized in that: The raw materials include an oil phase and a water phase; The oil phase comprises, by weight, 6-8 parts of methyl acrylate, 6-8 parts of butyl methacrylate, 4-6 parts of hexadecyl methacrylate, 0.5-1.5 parts of modified nano titanium dioxide, 0.5-1.5 parts of modified nano silicon dioxide, 0.5-1.0 parts of initiator, and 0.5-1 parts of crosslinking agent; The aqueous phase comprises: by weight, 0.1-0.5 parts of dispersant and 15-30 parts of water.

2. According to claim 1, a nano-material modified composite adsorbent for efficient separation and adsorption of oil-water and emulsion, characterized in that: The modified nano titanium dioxide and modified nano silicon dioxide are products obtained by hydrophobically modifying hydrophilic titanium dioxide and hydrophilic silicon dioxide using a silane coupling agent.

3. The nanomaterial modified composite adsorbent for efficient separation and adsorption of oil-water and emulsion according to claim 2, characterized in that: The specific preparation steps of the modified nano titanium dioxide are as follows: adding a silane coupling agent to a hydrophilic titanium dioxide suspension, stirring and reacting for 1-2 hours, washing and drying to obtain the modified nano titanium dioxide; The specific preparation steps of the modified nano-silica are as follows: adding a silane coupling agent into a hydrophilic silica suspension, stirring and reacting for 4-6 hours, washing and drying to obtain the modified nano-silica.

4. A composite adsorbent for efficient separation and adsorption of stratified oil-water and emulsion according to claim 3, characterized in that: The concentration of the hydrophilic titanium dioxide suspension is 200 g / L, the amount of the silane coupling agent added is 0.8% of the volume of the hydrophilic titanium dioxide suspension, and the silane coupling agent is KH-570; the stirring speed is 500 r / min; the reaction temperature is 40-50° C.; the concentration of the hydrophilic silicon dioxide suspension is 10 g / L, the amount of the silane coupling agent added is 2% of the volume of the hydrophilic silicon dioxide suspension, and the silane coupling agent is KH-171; The stirring speed is 500r / min; the reaction temperature is 40-50°C.

5. The nanomaterial modified composite adsorbent for efficient separation and adsorption of oil-water and emulsion according to claim 4, characterized in that: The preparation method of the hydrophilic titanium dioxide suspension is as follows: adding the hydrophilic titanium dioxide into a dispersion medium, removing the supernatant after ultrasonic treatment, and continuing to add the dispersion medium until the concentration of the suspension reaches 200 g / L; Similarly, the preparation method of the hydrophilic titanium dioxide suspension is: adding hydrophilic silicon dioxide to a dispersion medium, removing the supernatant after ultrasonic treatment, and continuing to add dispersion medium until the concentration of the suspension reaches 10 g / L.

6. The nanomaterial modified composite adsorbent for efficient separation and adsorption of oil-water and emulsion according to claim 5, characterized in that: The dispersion medium of modified nano titanium dioxide is a mixture of anhydrous ethanol and deionized water in a volume ratio of 1:1; the dispersion medium of modified nano silicon dioxide is anhydrous ethanol; the ultrasonic treatment temperature of the two materials is room temperature, the frequency is 35kHz, and the time is 1-2h; the particle size of the hydrophilic titanium dioxide and hydrophilic silicon dioxide is 40-50nm.

7. The nanomaterial modified composite adsorbent for efficient separation and adsorption of oil-water and emulsion according to claim 1, characterized in that: The initiator is benzoyl peroxide; the crosslinking agent is N,N-dimethylbisacrylamide; and the dispersant is polyvinyl alcohol.

8. A method for preparing a nanomaterial modified composite adsorbent for efficient separation and adsorption of oil-water and emulsion according to any one of claims 1 to 7, characterized in that: The specific steps include: (1) Weighing raw materials by weight: 6-8 parts of methyl acrylate, 6-8 parts of butyl methacrylate, 4-6 parts of hexadecyl methacrylate, 0.5-1.5 parts of modified nano titanium dioxide, 0.5-1.5 parts of modified nano silicon dioxide, 0.5-1.0 parts of initiator, 0.5-1 parts of crosslinking agent, 0.1-0.5 parts of dispersant, and 15-30 parts of water; (2) uniformly mixing the methyl acrylate, the butyl acrylate, the butyl methacrylate, the modified nano titanium dioxide, the modified nano silicon dioxide, the initiator, and the crosslinking agent to obtain an oil phase; (3) dissolving the dispersant in the water, stirring and dissolving to obtain an aqueous phase; (4) adding the oil phase dropwise to the water phase and stirring to form uniform droplets of the oil phase in the water phase. After reacting for 4-5 hours, cooling, washing and drying are performed in sequence to obtain a solid adsorbent.

9. A nano-material modified composite adsorbent for efficient separation and adsorption of oil-water and emulsion according to claim 8, characterized in that: The dissolving temperature in step (3) is 40°C; The reaction temperature in step (4) is 75-80° C. under a nitrogen environment; The drying in step (4) is performed at 40-50° C. until the product reaches a constant weight.

10. Use of the nanomaterial modified composite adsorbent according to any one of claims 1 to 7 in separation and adsorption of emulsified oil.

Citation Information

Patent Citations

  • Preparation method for resin adsorbent compounded with straw activated carbon

    CN104841387A

  • Water-absorbing foam based on double emulsifiers and preparation method of water-absorbing foam

    CN115215961A

  • Solid adsorbent for separating emulsified oil-water mixture as well as preparation method and application of solid adsorbent

    CN116726885A

  • Magnetic composite adsorbent for one-step separation and adsorption of emulsified oil as well as preparation method and application of magnetic composite adsorbent

    CN117123200A

  • Oil absorbent

    JP1995102248A

Cited By

  • Polystyrene foam recycling method based on suspension process

    CN122668436A