Antibacterial polyurethane sole, preparation method and polyurethane composition

By using ingredients such as copper nanoparticles-chitosan composites and antioxidants in polyurethane sole materials, the problem of traditional sole materials breeding bacteria and fungi in humid environments has been solved, improving antibacterial properties and yellowing resistance, and prolonging use Lifespan and reduce the risk of environmental pollution.

CN119039771AInactive Publication Date: 2024-11-29温州市添荣鞋材有限公司
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411546597.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-01
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional polyurethane sole materials are prone to breed bacteria and fungi in humid environments, resulting in odor and health risks, and have insufficient yellowing resistance, affecting service life.

Method used

Copper nanoparticle-chitosan complex is used as an antibacterial agent, combined with antioxidants and ultraviolet absorbers, which significantly improves antibacterial properties, yellowing resistance and mechanical properties.

Benefits of technology

It has achieved long-term antibacterial protection, extended service life, reduced environmental pollution, and maintained material color stability, improving the environmental protection and market competitiveness of sole materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039771A_ABST
    Figure CN119039771A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a polyurethane sole, in particular to an antibacterial polyurethane sole, a preparation method and a polyurethane composition. The copper nanoparticle-chitosan compound antibacterial agent is introduced into the polyurethane sole material, and the antioxidant and the ultraviolet light absorber are combined, so that the antibacterial property, the mechanical property, the yellowing resistance and the environmental protection property of the sole material are remarkably improved, and an effective technical solution is provided for developing high-performance and multifunctional shoe products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a polyurethane sole, in particular to an antibacterial polyurethane sole, a preparation method and a polyurethane composition. Background Art

[0002] With the development of society and the improvement of people's living standards, consumers' demand for footwear products is not limited to beauty and comfort. The durability, functionality and health of shoes are also increasingly valued. As an important part of footwear products, the performance of the sole material directly affects the overall quality of the shoes. In recent years, antibacterial property has become an important characteristic of sole materials, especially in occasions such as sports shoes and work shoes that are worn for a long time. It can effectively inhibit the growth of microorganisms such as bacteria and fungi, prevent odor and protect foot health. Therefore, it is particularly important to develop sole materials with good antibacterial properties.

[0003] Polyurethane (PU) is a polymer material widely used in shoe soles. It is widely popular because of its excellent elasticity, wear resistance, shock absorption and good chemical corrosion resistance. However, traditional polyurethane sole materials are prone to breed bacteria and fungi in humid and warm environments, which in turn leads to odor, sole aging and health risks. In order to solve this problem, many researchers have begun to introduce antibacterial agents into polyurethane sole materials to enhance their antibacterial properties.

[0004] At present, common antimicrobial agents include organic antimicrobial agents (such as quaternary ammonium salts and phenolic compounds) and inorganic antimicrobial agents (such as metal nanoparticles such as silver and zinc). Among them, inorganic antimicrobial agents such as silver nanoparticles have received widespread attention and application due to their broad-spectrum antimicrobial properties and low risk of drug resistance. However, silver nanoparticles are expensive and may accumulate in the environment, posing potential ecological risks. In contrast, copper, as a more economical and equally effective antimicrobial agent, has gradually attracted attention. Copper nanoparticles not only have good antimicrobial properties, but also can kill bacteria and fungi by reacting with bacterial cell membranes to produce oxidative stress. In order to further improve the antimicrobial effect and material stability, the composite of copper nanoparticles with chitosan has become a new research direction.

[0005] Chitosan is a natural polysaccharide extracted from the exoskeleton of crustaceans, which has good biocompatibility, antibacterial and biodegradability. The combination of copper nanoparticles and chitosan can make full use of the slow-release properties of chitosan, making the antibacterial effect of copper nanoparticles more lasting and reducing the potential impact on the environment. In addition, chitosan can improve the mechanical properties and antioxidant properties of the composite material, which helps to improve the durability of the polyurethane sole.

[0006] In addition to antibacterial properties, the yellowing resistance of the sole material is also an important performance indicator. The sole is easily yellowed when exposed to ultraviolet and oxygen environments for a long time, which affects the appearance and service life of the shoes. Therefore, adding antioxidants and ultraviolet absorbers to polyurethane sole materials can effectively improve the material's yellowing resistance. Summary of the invention

[0007] In order to solve the above technical problems, the purpose of the present invention is to provide an antibacterial polyurethane sole composition. The composition adopts a copper nanoparticle-chitosan complex as an antibacterial agent and is combined with antioxidants, ultraviolet absorbers and other ingredients to significantly improve the antibacterial performance, yellowing resistance and mechanical properties of the sole material, and has good market application prospects.

[0008] In order to achieve the above-mentioned purpose, the present invention adopts the following technical solutions: An antibacterial polyurethane sole composition, comprising the following components in parts by weight: Castor oil polyol, 20-40 parts by weight; Polyether polyol, 60-80 parts by weight; Deionized water, 2.0-5.0 parts by weight; Antibacterial agent, 1.0-3.0 parts by weight; Catalyst, 0.15-0.3 parts by weight; Antioxidant, 0.4-0.8 parts by weight; Ultraviolet light absorber, 0.4-0.8 parts by weight; Isocyanate, 20-40 parts by weight; The antibacterial agent adopts a copper nanoparticle-chitosan complex. The preparation method of the copper nanoparticle-chitosan complex is as follows: copper nanoparticles are prepared by a chemical reduction method, the particle size is controlled between 10-50 nanometers, the copper nanoparticles are dispersed in a chitosan solution, and stirred evenly so that the copper nanoparticles are evenly distributed in the chitosan matrix; and then a solid complex powder is obtained by drying and crushing.

[0009] Preferably, the specific method of the copper nanoparticle-chitosan composite is as follows: 1) Dissolve chitosan in 1.0-3.0% volume percent acetic acid solution; stir with a magnetic stirrer until the chitosan is completely dissolved to form a uniform chitosan solution; 2) Add 0.1-0.5M ascorbic acid solution dropwise to the copper chloride solution while stirring; copper ions are reduced by ascorbic acid to form copper nanoparticles; the formation of copper nanoparticles is confirmed by observing the change in the color of the solution from light blue to dark brown; 3) using an ultrasonic disperser to treat the copper nanoparticle solution for 20-25 minutes to evenly disperse the nanoparticles; 4) Slowly add the prepared copper nanoparticle solution to the chitosan solution, stirring while adding, to form a copper nanoparticle-chitosan composite solution; during the stirring process, slightly heat the solution to 40-50°C, and continue stirring for 1-2 hours to evenly disperse the copper nanoparticles in the chitosan matrix; 5) centrifuging the composite solution at a speed of 8000-10000 rpm for 10-20 minutes to collect the precipitate; washing the precipitate with deionized water several times to remove unreacted components and excess acid; 6) The washed precipitate is dried at 50-60° C. to a constant weight and crushed, or spray-dried to obtain a dry copper-based nanoparticle-chitosan composite powder.

[0010] Preferably, the polyether polyol is selected from polyethylene oxide or polypropylene glycol.

[0011] Preferably, the isocyanate uses MDI (4,4'-diphenylmethane diisocyanate) as the main isocyanate component; a small amount of HDI (trimethylene-1,6-diisocyanate) is added to improve the yellowing stability; the mass ratio of MDI to HDI is 5:1-10:1.

[0012] Preferably, the antioxidant is a phenolic antioxidant; and the ultraviolet absorber is UV-328.

[0013] Preferably, the catalyst is dibutyltin dilaurate or triethylenediamine.

[0014] Preferably, the composition further contains 1-3% (by weight) of nano silicon dioxide.

[0015] Furthermore, the present invention also discloses an antibacterial polyurethane sole, which is prepared by foaming the composition.

[0016] Furthermore, the present invention also discloses a method for preparing the sole, which comprises the following steps: 1) In a reactor, castor oil polyol and polyether polyol are added and stirred evenly; deionized water is added and stirred continuously; copper-based nanoparticle-chitosan composite antibacterial agent is added and dispersed evenly; then, antioxidant and ultraviolet absorber are added and stirred evenly; 2) Add the catalyst to the mixture and stir evenly; control the stirring speed at 600-800 rpm; heat the mixture to 50-60°C and keep the temperature stable; 3) Slowly add isocyanate under stirring conditions, and increase the stirring speed to 1000-1200 rpm to ensure a rapid and uniform reaction; continue stirring for about 10-15 minutes until the reaction is complete; 4) Pour the reacted mixture into a pre-prepared mold for free foaming; after the foaming is completed, keep the material in an oven at 50-60°C for 2-3 hours; 5) Take out the cured material and place it at room temperature for 20-30 hours to completely cure it; remove the material in the mold and perform subsequent processing to obtain the final sole product.

[0017] Furthermore, the present invention also discloses a pair of antibacterial shoes, the sole of the shoe is the above-mentioned sole.

[0018] The present invention adopts the above technical solution, the antibacterial polyurethane sole composition uses copper nanoparticles-chitosan complex as an antibacterial agent, and combines multiple auxiliary components to achieve a series of significant technical effects. Specific beneficial effects include: 1. Enhanced antibacterial properties: The use of copper nanoparticle-chitosan complex as an antibacterial agent provides excellent broad-spectrum antibacterial effect. Copper nanoparticles can effectively destroy bacterial cell membranes and interfere with their metabolism, thereby inhibiting the growth of bacteria and fungi. At the same time, chitosan, as a natural antibacterial substance, not only has independent antibacterial ability, but also can improve the dispersibility and stability of copper nanoparticles. The sustained-release properties of chitosan can ensure the durability of the antibacterial agent in the sole material and provide long-term antibacterial protection. Compared with a single antibacterial agent, this complex can achieve a more efficient and lasting antibacterial effect, effectively reduce the generation of sole odor and the risk of bacterial infection, and improve the health and comfort of the wearer.

[0019] 2. Improve the mechanical properties of materials: The copper nanoparticle-chitosan composite not only has antibacterial function, but also enhances the mechanical properties of polyurethane materials. The addition of chitosan improves the toughness and strength of the composite material, and enhances the wear resistance and impact resistance of the material. This makes the sole material more durable, able to maintain its function and shape during long-term use, and effectively extends the service life of the shoes.

[0020] 3. Improve yellowing resistance: The antioxidant (such as phenolic antioxidant) and ultraviolet absorber (such as UV-328) introduced in the present invention effectively improve the yellowing resistance of the polyurethane sole material. The antioxidant can inhibit the formation of free radicals and prevent the oxidative degradation of the material under light and high temperature conditions; the ultraviolet absorber can absorb ultraviolet rays and protect the material from damage by ultraviolet rays. Through the synergistic effect of these two components, the sole material can maintain good color stability when exposed to sunlight and air for a long time, avoid the occurrence of yellowing, and ensure the aesthetics of the shoes and the satisfaction of consumers.

[0021] 4. Ensure the environmental protection and safety of materials: Using chitosan as the matrix of the composite not only improves the performance of the antibacterial agent, but also enhances the environmental friendliness of the material. Chitosan is a biodegradable natural polysaccharide that is safer and more environmentally friendly than traditional chemically synthesized antibacterial agents. In addition, the use of copper nanoparticles is relatively small, which can ensure the antibacterial effect while reducing the potential pollution of heavy metals to the environment.

[0022] 5. Simplify the preparation process and reduce production costs: The antibacterial polyurethane sole composition of the present invention can be prepared by a conventional chemical reduction method and a simple composite method, and has a simple process, strong controllability, and is suitable for large-scale production. The copper nanoparticles are prepared by a chemical reduction method, which has low cost, is easy to operate, and has low requirements on the equipment and conditions required, thus helping to reduce production costs and improve economic benefits.

[0023] 6. Provide broad application prospects: The antibacterial polyurethane sole composition has multiple excellent properties such as antibacterial, wear-resistant, yellowing-resistant and environmentally friendly, and is suitable for the preparation of various soles, including sports shoes, casual shoes, work shoes, etc. By improving the performance of the sole material, the market competitiveness of footwear products can be improved, meeting consumers' demand for diversified and high-quality footwear products.

[0024] In summary, the present invention significantly improves the antibacterial properties, mechanical properties, yellowing resistance and environmental protection of the sole material by introducing a copper nanoparticle-chitosan composite antibacterial agent into the polyurethane sole material and combining it with an antioxidant and a UV absorber, thereby providing an effective technical solution for the development of high-performance and multifunctional footwear products. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is an electron microscope photograph of the copper nanoparticle-chitosan composite prepared in the present invention. DETAILED DESCRIPTION

[0026] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1: Preparation method of copper-based nanoparticles and chitosan composites Materials preparation: Copper chloride (CuCl2): as a copper source; Ascorbic acid (Vitamin C): as a reducing agent, used to reduce copper ions; Chitosan: molecular weight range: 50,000 to 200,000 Daltons (Da), as a stabilizer and antibacterial matrix; Acetic Acid: 1% acetic acid solution, used to dissolve chitosan; Deionized water: used for solution preparation.

[0028] Preparation steps: 1) Dissolve chitosan (1 g) in 100 mL of 1% acetic acid solution. Stir with a magnetic stirrer until the chitosan is completely dissolved to form a uniform chitosan solution. 2) Prepare 0.01 M copper chloride solution and pour 10 mL of the solution into a beaker; add 0.1 M ascorbic acid solution (reducing agent) dropwise into the copper chloride solution while stirring. Copper ions are reduced by ascorbic acid to form copper nanoparticles; the formation of copper nanoparticles is confirmed by observing the change in solution color (from light blue to dark brown).

[0029] 3) The copper nanoparticle solution was treated with an ultrasonic disperser for 20 minutes to ensure that the nanoparticles were evenly dispersed.

[0030] 4) Slowly add the prepared copper nanoparticle solution to the chitosan solution while stirring to form a copper nanoparticle-chitosan composite solution; during the stirring process, the solution can be slightly heated to 40-50°C to improve solubility and dispersibility, and stirring is continued for 1 hour to ensure that the copper nanoparticles are evenly dispersed in the chitosan matrix.

[0031] 5) The composite solution is centrifuged at a speed of 8000 rpm for 10 minutes to collect the precipitate; the precipitate is washed with deionized water for several times to remove unreacted components and excess acid; the washed precipitate is dried at 60° C. to a constant weight, or the dried copper-based nanoparticle-chitosan composite powder is obtained by spray drying or freeze drying.

[0032] 6) Use scanning electron microscopy (SEM) to observe the morphology and particle size distribution of the composite. Figure 1 shown.

[0033] Example 2: Antimicrobial polyurethane sole composition Recipe Ingredients: Castor oil polyol (JT-805): 30 parts by weight Polyether polyol (polypropylene glycol): 70 parts by weight Deionized water: 3.0 parts by weight Copper nanoparticle-chitosan composite antibacterial agent: 2.0 parts by weight Catalyst (DBTDL): 0.2 parts by weight Antioxidant (Irganox 1010): 0.6 parts by weight Ultraviolet absorber (UV-328): 0.6 parts by weight Isocyanate (MDI / HDI, mass ratio is 8:1): 30 parts by weight The copper nanoparticle-chitosan composite antibacterial agent was prepared by the method described in Example 1.

[0034] Method for preparing shoe soles using the above antibacterial polyurethane shoe sole composition: 1) Mix castor oil polyol and polyether polyol in a reactor and stir evenly; 2) Add deionized water and continue stirring; 3) Add copper nanoparticle-chitosan composite antibacterial agent and stir until evenly dispersed; 4) Add antioxidant and UV absorber and stir evenly; 5) Add catalyst (DBTDL) to the mixture, control the stirring speed at 700 rpm, and heat to 55°C; 6) Slowly add isocyanate (MDI / HDI), increase the stirring speed to 1100 rpm, and continue stirring for 15 minutes; 7) Pour the reacted mixture into a mold for free foaming; 8) After foaming, cure at 55°C for 2.5 hours, leave at room temperature for 24 hours, and take out to obtain the sole material.

[0035] Example 2: Antibacterial polyurethane sole composition with added nano-silicon dioxide Recipe Ingredients: Castor oil polyol (JT-805): 35 parts by weight Polyether polyol (polypropylene glycol): 65 parts by weight Deionized water: 2.5 parts by weight Copper nanoparticle-chitosan composite antibacterial agent: 2.0 parts by weight Nano silicon dioxide: 2.0 parts by weight Catalyst (DBTDL): 0.25 parts by weight Antioxidant (Irganox 1010): 0.5 parts by weight Ultraviolet absorber (UV-328): 0.5 parts by weight Isocyanate (MDI / HDI, mass ratio 7:1): 35 parts by weight The copper nanoparticle-chitosan composite antibacterial agent was prepared by the method described in Example 1.

[0036] Method for preparing shoe soles using the above antibacterial polyurethane shoe sole composition: 1) mixing castor oil polyol and polyether polyol in a reactor and stirring uniformly; 2) Add deionized water and nano-silicon dioxide and disperse by ultrasonic for 10 minutes to ensure uniform dispersion; 3) adding copper nanoparticle-chitosan composite antibacterial agent and stirring until uniformly dispersed; 4) Add antioxidant and ultraviolet absorber and stir evenly; 5) Add catalyst (DBTDL) to the mixture, control the stirring speed at 750 rpm, and heat to 50°C; 6) Slowly add isocyanate (MDI / HDI), increase the stirring speed to 1200 rpm, and continue stirring for 15 minutes; 7) pouring the reacted mixture into a mold for free foaming; 8) After the foaming is completed, the material is cured at 50° C. for 3 hours, placed at room temperature for 24 hours, and then taken out to obtain the sole material.

[0037] Comparative Example 1: Polyurethane sole composition without antibacterial agent Recipe Ingredients: Castor oil polyol (JT-805): 30 parts by weight Polyether polyol (polypropylene glycol): 70 parts by weight Deionized water: 3.0 parts by weight Catalyst (DBTDL): 0.2 parts by weight Antioxidant (Irganox 1010): 0.6 parts by weight Ultraviolet absorber (UV-328): 0.6 parts by weight Isocyanate (MDI / HDI, mass ratio is 8:1): 30 parts by weight.

[0038] Method for preparing the sole: 1) mixing castor oil polyol and polyether polyol in a reactor and stirring uniformly; 2) Add deionized water and continue stirring; 3) Add antioxidant and ultraviolet absorber and stir evenly; 4) Add catalyst (DBTDL) to the mixture, control the stirring speed at 700 rpm, and heat to 55°C; 5) Slowly add isocyanate (MDI / HDI), increase the stirring speed to 1100 rpm, and continue stirring for 15 minutes; 6) pouring the reacted mixture into a mold for free foaming; 7) After the foaming is completed, the material is cured at 55° C. for 2.5 hours, placed at room temperature for 24 hours, and then taken out to obtain the sole material.

[0039] Comparative Example 2: Polyurethane sole compositions using different antimicrobial agents Recipe Ingredients: Castor oil polyol (JT-805): 30 parts by weight Polyether polyol (polypropylene glycol): 70 parts by weight Deionized water: 3.0 parts by weight Silver nanoparticle antibacterial agent: 2.0 parts by weight Catalyst (DBTDL): 0.2 parts by weight Antioxidant (Irganox 1010): 0.6 parts by weight Ultraviolet absorber (UV-328): 0.6 parts by weight Isocyanate (MDI / HDI, mass ratio is 8:1): 30 parts by weight Method for preparing the sole: 1) Mix castor oil polyol and polyether polyol in a reactor and stir evenly; 2) Add deionized water and continue stirring; 3) Add silver nanoparticle antibacterial agent and stir until evenly dispersed; 4) Add antioxidant and ultraviolet absorber and stir evenly; 5) Add catalyst (DBTDL) to the mixture, control the stirring speed at 700 rpm, and heat to 55°C; 6) Slowly add isocyanate (MDI / HDI), increase the stirring speed to 1100 rpm, and continue stirring for 15 minutes; 7) Pour the reacted mixture into a mold for free foaming; 8) After foaming, cure at 55°C for 2.5 hours, leave at room temperature for 24 hours, and take out to obtain the sole material.

[0040] Test Example 1 Antibacterial Performance Test Method Experimental steps: 1. Preparation of bacterial suspension: Two common pathogens were selected: Staphylococcus aureus ( Staphylococcus aureus ) and Escherichia coli ( Escherichia coli); Under sterile conditions, culture the bacteria on nutrient agar plates at 37°C for 24 hours; take an appropriate amount of colonies and dilute them with sterile saline to about 10^6 CFU / mL (colony forming units per milliliter).

[0041] 2. Sample processing: The shoe sole material samples (size: 1 cm x 1 cm) of Example 1, Example 2, Comparative Example 1 and Comparative Example 2 were prepared under sterile conditions; each sample was placed in 4 sterile culture dishes.

[0042] 3. Inoculation and incubation: Add 0.1 mL of bacterial suspension to each sample to evenly cover the surface of the sample; cover the culture dish and incubate at 37°C for 24 hours.

[0043] 4. Colony count: After incubation, use a sterile cotton swab to smear the surface of each sample, dip the smeared cotton swab into sterile saline, and dilute it appropriately; inoculate the dilution on a nutrient agar plate and culture it at 37°C for 24 hours; count the number of colonies on the plate and calculate the inhibition rate.

[0044] 5. Antibacterial rate calculation formula:

[0045] 6. Antibacterial performance test data as shown in Table 1 Table 1 Antibacterial performance test data sample Bacteria Colony count (CFU / mL) Antibacterial rate (%) Example 1 Staphylococcus aureus 152 99.69 Example 1 Escherichia coli 163 99.54 Example 2 Staphylococcus aureus 42 99.92 Example 2 Escherichia coli 65 99.82 Comparative Example 1 Staphylococcus aureus <![CDATA[4.86´10 4 ]]> 0.00 Comparative Example 1 Escherichia coli <![CDATA[3.58´10 4 ]]> 0.00 Comparative Example 2 Staphylococcus aureus 538 98.89 Comparative Example 2 Escherichia coli 841 97.65

[0046] 7. Results Analysis Examples 1 and 2 showed extremely high antibacterial effects, with the antibacterial rates against Staphylococcus aureus and Escherichia coli reaching 99.65% and 99.54%, respectively; this indicates that the copper nanoparticle-chitosan composite antibacterial agent can significantly inhibit the growth of bacteria in the sole material; The antibacterial effect of Example 2 is slightly better than that of Example 1, which may be due to the addition of nano-silicon dioxide, which improves the activity of the material surface and makes the antibacterial agent more effective; Comparative Example 1 (without antimicrobial agent) has almost no antimicrobial effect, indicating that polyurethane materials without antimicrobial agents cannot effectively inhibit bacterial growth; Comparative Example 2 (using silver nanoparticle antimicrobial agent) also showed high antimicrobial performance, but compared with the copper nanoparticle-chitosan composite, the antimicrobial effect was slightly inferior and the cost was higher, indicating that copper-based antimicrobial agents are a more economical and effective choice.

[0047] Test Example 2 Mechanical Properties Test Method 1. Tensile strength test Testing equipment: Universal material testing machine Test standard: ASTM D412 (tensile properties test of rubber materials).

[0048] Test steps: Cut a standard dumbbell-shaped specimen (size: length 75mm, width 4mm) from each sole material sample; clamp the specimen in the fixture of a universal material testing machine; stretch the specimen at a speed of 50mm / min, and record the maximum load when stretched to fracture; calculate the tensile strength (MPa): .

[0049] 2. Tear strength test Testing equipment: Universal material testing machine Test standard: ASTM D624 (tear strength test of rubber materials).

[0050] Test steps: Cut a standard right-angle tear specimen (size: length 100 mm, width 25 mm, V-shaped cut depth 5 mm) from each sole material sample; clamp the sample in the tear fixture of the universal material testing machine; tear the sample at a speed of 50 mm / min, and record the maximum load during tearing; calculate the tear strength (N / mm): .

[0051] 3. Hardness test Testing equipment: Shore hardness tester (Type A) Test standard: ASTMD2240 (rubber material hardness test) Test steps: Place the sole material sample flat on a hard flat plate; place the probe of the Shore A hardness tester vertically on the sample surface; read the value on the hardness tester and record the Shore A hardness.

[0052] 4. Wear resistance test Test equipment: Abrasion tester (DIN abrasion method) Test standard: ASTM D5963 (abrasion resistance test of rubber materials) Test steps: Cut the sole material sample into a standard-sized disc (16 mm in diameter); fix the sample in the rotating fixture of the abrasion tester; apply a standard load of 5 N to the sample and make the sample contact with the wear paper; rotate the sample and record the weight loss (mg) after wear.

[0053] 5. Mechanical properties test data Test items Example 1 Example 2 Comparative Example 1 Comparative Example 2 Tensile strength(MPa) 15.5 16.8 13.0 14.5 Tear strength(N / mm) 45.3 50.2 35.0 40.5 Hardness(Shore A) 75 78 70 73 Wear resistance(mg) 40 35 50 45 6. Results Analysis Tensile strength: The tensile strength of Example 1 and Example 2 is significantly higher than that of Comparative Example 1 and Comparative Example 2, indicating that the copper nanoparticle-chitosan complex enhances the mechanical strength of polyurethane; Example 2 exhibits higher tensile strength due to the presence of nano-silicon dioxide; Tear strength: The tear strength of Example 1 and Example 2 is also significantly better than that of Comparative Example 1 and Comparative Example 2, showing better tear resistance; The tear strength of Example 2 is the highest, which may be attributed to the additional reinforcement effect provided by nano-silicon dioxide; Hardness: The hardness of Examples 1 and 2 is relatively high, indicating that the addition of antibacterial agents and nano-silicon dioxide increases the surface hardness of the material, making the sole material more wear-resistant; The hardness of Comparative Example 1 is the lowest, indicating that the hardness of the material without antibacterial agent and reinforcing agent is poor; Wear resistance: The wear resistance of Example 1 and Example 2 is better than that of Comparative Example 1 and Comparative Example 2, especially Example 2 shows the smallest wear weight loss, which indicates that nano-silicon dioxide significantly improves the wear resistance of the material; The wear resistance of Comparative Example 1 is the worst, indicating that the material without adding antibacterial agent and reinforcing agent is easy to wear in actual use; Test Example 3 Accelerated Aging Test In this experiment, we used accelerated aging testing to evaluate the yellowing resistance of antimicrobial polyurethane sole compositions. This test accelerates the aging process of the sole material by simulating sunlight and heat exposure conditions and measures the color change of the material. 1. Sample preparation: Cut standard samples with a size of 50 mm × 50 mm × 2 mm from the sole materials of Example 1, Example 2, Comparative Example 3 (the antioxidant and ultraviolet absorber are removed from Comparative Example 1), and Comparative Example 4 (the antioxidant and ultraviolet absorber are removed from Comparative Example 2); ensure that the surface of the sample is flat and has no obvious defects; 2. Aging test equipment: Use an ultraviolet accelerated aging test chamber (such as a QUV aging tester), which is equipped with ultraviolet lamps that can simulate the ultraviolet radiation of sunlight and has a temperature control function.

[0054] 3. Test conditions: UV light source: UVA-340 lamp, wavelength range: 315-400nm; irradiation intensity: 0.89W / m² / nm (at 340nm); test temperature: 60℃; exposure time: continuous exposure for 72 hours.

[0055] 4. Measurement method: Before and after the aging test, use a spectrophotometer to measure the whiteness index (WI) of the sample; the whiteness index reflects the change in material color. The higher the WI value, the whiter the material and the lower the degree of yellowing; record the initial whiteness index before aging ( WI initial ) and the whiteness index after aging ( WI final); Yellowing index calculation:

[0056] The larger the yellowing index is, the worse the material's yellowing resistance is.

[0057] 5. Experimental data of embodiments and comparative examples sample <![CDATA[Initial whiteness index WI initial > <![CDATA[Whiteness Index WI after aging initial > Yellowing Index Example 1 85.0 82.0 3.0 Example 2 85.0 83.5 1.5 Comparative Example 3 85.0 77.0 8.0 Comparative Example 4 85.0 79.5 5.5

[0058] 6. Results Analysis The yellowing index of Example 1 is 3.0, indicating that it exhibits good yellowing resistance under ultraviolet and high temperature conditions; the combination of the copper nanoparticle-chitosan composite with the antioxidant and the ultraviolet absorber effectively reduces the yellowing degree of the material; The yellowing index of Example 2 is 1.5, which is the lowest among all samples; this indicates that the addition of nano-silicon dioxide further enhances the yellowing resistance of the material, allowing it to maintain a high whiteness even when exposed to ultraviolet rays and high temperatures for a long time; The yellowing index of Comparative Example 3 is 8.0, showing obvious yellowing phenomenon; this indicates that without adding antioxidants and ultraviolet absorbers, polyurethane materials are prone to yellowing, affecting appearance and performance; The yellowing index of Comparative Example 4 (using silver nanoparticle antibacterial agent) is 5.5, which is improved compared with Comparative Example 1, but still significantly higher than that of the embodiment; this indicates that the use of silver nanoparticle antibacterial agent alone has limited improvement on yellowing resistance.

Claims

1. An antibacterial polyurethane sole composition, It is characterized in that The composition comprises the following components by weight: Castor oil polyol, 20-40 parts by weight; Polyether polyol, 60-80 parts by weight; Deionized water, 2.0-5.0 parts by weight; Antibacterial agent, 1.0-3.0 parts by weight; Catalyst, 0.15-0.3 parts by weight; Antioxidant, 0.4-0.8 parts by weight; Ultraviolet light absorber, 0.4-0.8 parts by weight; Isocyanate, 20-40 parts by weight; The antibacterial agent adopts a copper nanoparticle-chitosan complex. The preparation method of the copper nanoparticle-chitosan complex is as follows: copper nanoparticles are prepared by a chemical reduction method, the particle size is controlled between 10-50 nanometers, the copper nanoparticles are dispersed in a chitosan solution, and stirred evenly so that the copper nanoparticles are evenly distributed in the chitosan matrix; and then a solid complex powder is obtained by drying and crushing.

2. The antibacterial polyurethane sole composition according to claim 1, It is characterized in that The specific method of copper nanoparticle-chitosan composite is as follows: 1) Dissolve chitosan in 1.0-3.0% volume percent acetic acid solution; stir with a magnetic stirrer until the chitosan is completely dissolved to form a uniform chitosan solution; 2) Add 0.1-0.5 M ascorbic acid solution dropwise to the copper chloride solution while stirring; copper ions are reduced by ascorbic acid to form copper nanoparticles; the formation of copper nanoparticles is confirmed by observing the change in the color of the solution from light blue to dark brown; 3) using an ultrasonic disperser to treat the copper nanoparticle solution for 20-25 minutes to evenly disperse the nanoparticles; 4) Slowly add the prepared copper nanoparticle solution to the chitosan solution, stirring while adding, to form a copper nanoparticle-chitosan composite solution; during the stirring process, slightly heat the solution to 40-50°C, and continue stirring for 1-2 hours to evenly disperse the copper nanoparticles in the chitosan matrix; 5) centrifuging the composite solution at a speed of 8000-10000 rpm for 10-20 minutes to collect the precipitate; washing the precipitate with deionized water several times to remove unreacted components and excess acid; 6) The washed precipitate is dried at 50-60° C. to a constant weight and crushed, or spray-dried to obtain a dry copper-based nanoparticle-chitosan composite powder.

3. The antibacterial polyurethane sole composition according to claim 1, It is characterized in that The polyether polyol is selected from polyethylene oxide or polypropylene glycol.

4. The antibacterial polyurethane sole composition according to claim 1, It is characterized in that The isocyanate uses 4,4'-diphenylmethane diisocyanate as the main isocyanate component; trimethylene-1,6-diisocyanate is added to improve the yellowing stability; the mass ratio of MDI to HDI is 5:1-10:

1.

5. The antibacterial polyurethane sole composition according to claim 1, It is characterized in that The antioxidant is a phenolic antioxidant; and the ultraviolet absorber is UV-328.

6. The antibacterial polyurethane sole composition according to claim 1, It is characterized in that The catalyst is dibutyltin dilaurate or triethylenediamine.

7. The antibacterial polyurethane sole composition according to claim 1, It is characterized in that The composition is also added with 1-3% by weight of nano silicon dioxide.

8. An antibacterial polyurethane sole, which is prepared by foaming the composition according to any one of claims 1 to 7.

9. The method for preparing the sole according to claim 8, It is characterized in that The method comprises the following steps: 1) In a reactor, castor oil polyol and polyether polyol are added and stirred evenly; deionized water is added and stirred continuously; copper-based nanoparticle-chitosan composite antibacterial agent is added and dispersed evenly; Then, add antioxidant and UV absorber and stir well; 2) Add the catalyst to the mixture and stir evenly; control the stirring speed at 600-800 rpm; heat the mixture to 50-60°C and keep the temperature stable; 3) Slowly add isocyanate under stirring conditions, and increase the stirring speed to 1000-1200 rpm to ensure a rapid and uniform reaction; continue stirring for about 10-15 minutes until the reaction is complete; 4) Pour the reacted mixture into a pre-prepared mold for free foaming; after the foaming is completed, keep the material in an oven at 50-60°C for 2-3 hours; 5) Take out the cured material and place it at room temperature for 20-30 hours to completely cure it; remove the material in the mold and perform subsequent processing to obtain the final sole product. 10.An antibacterial shoe, It is characterized in that The sole of the shoe is the sole according to claim 8.

Citation Information

Patent Citations

  • Anionic polyurethane sole material

    CN103570910A

  • Low-density high-strength high-yellowing-resistant TPU for soles, and preparation method thereof

    CN110627983A

  • Chitosan microsphere loaded nano silver antibacterial polypropylene material, composite antibacterial agent and preparation method thereof

    CN110804247A

  • Full-biodegradable freshness protection bag and preparation method thereof

    CN116875010A

  • Polyurethane antibacterial composite material and preparation method thereof

    CN117511181A