Environment-friendly composite modified asphalt and preparation method thereof

Through the blending technology of SEPS modifier with bio-based polyhexylene azelaate and rubber oil, the problem of insufficient storage stability and anti-aging performance of SBS modified asphalt is solved, and the mechanical and low-temperature performance of asphalt is improved. Reduced production costs.

CN119039795APending Publication Date: 2024-11-29SICHUAN JIAOTOU CONSTR ENG CO LTD +2
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411092098.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing SBS modified asphalt has poor storage stability and insufficient anti-aging properties. The mechanical properties, toughness and wear resistance of SEPS are slightly inferior to those of SBS, resulting in higher asphalt production costs.

Method used

Use SEPS modifiers to blend with bio-based polyhexylene azelaate and rubber oil. Through multipolymer modification, the mechanical properties, low-temperature properties and anti-UV aging properties of asphalt are improved, and the amount of SEPS is reduced. to reduce costs.

Benefits of technology

It significantly improves the storage stability, UV aging resistance and low temperature performance of asphalt, reduces the amount of SEPS, reduces the cost of materials, and improves the high-temperature performance and fatigue resistance of asphalt.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004986874400000101
    Figure BDA0004986874400000101
  • Figure BDA0004986874400000111
    Figure BDA0004986874400000111
Patent Text Reader

Abstract

The invention provides environment-friendly composite modified asphalt, which is prepared from the following components in parts by weight: 8 to 12 parts of SEPS modifier, 2 to 4 parts of bio-based poly (hexanediol azelate), 3 to 5 parts of rubber oil and 79 to 87 parts of matrix asphalt, the SEPS modifier is used for carrying out blending modification on SEPS through a multipolymer; the preparation method comprises the following steps: S1, heating the matrix asphalt, adding the rubber oil, and continuously stirring and uniformly mixing to obtain an asphalt mixture I; s2, adding an SEPS modifier into the asphalt mixture I obtained in the step S1 in batches, and continuously stirring and uniformly mixing to obtain an asphalt mixture II; s3, heating the asphalt mixture II obtained in the step S2, carrying out high-speed shearing for a period of time, then adding bio-based poly (hexanediol azelate), and continuously stirring and uniformly mixing to obtain a mixed material; and S4, swelling and developing the mixed material in the step S3 for a period of time at a certain temperature to obtain the environment-friendly composite modified asphalt. The asphalt modifier can improve the mechanical properties of asphalt and reduce the production cost of asphalt.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of asphalt, and in particular to an environmentally friendly composite modified asphalt and a preparation method thereof. Background Art

[0002] With the continuous increase in road traffic, people are increasingly demanding traffic pavements with better fatigue life and high and low temperature performance. Pavement structure and asphalt performance are two key factors affecting the comprehensive performance of pavements, and asphalt performance is particularly important.

[0003] SBS modified asphalt is widely used worldwide for its excellent high-temperature anti-rutting performance. However, in actual engineering, SBS modified asphalt shows weaknesses such as poor storage stability and insufficient anti-aging performance. To address these shortcomings, the application of SBS's similar derivatives SEBS and SIS in the field of modified asphalt has gradually increased. SEBS improves its resistance to thermal oxidative aging by hydrogenating the soft segment into a carbon-carbon single bond, but its storage stability is still insufficient and it is prone to segregation. And because the price of a single SEPS is relatively high, its mechanical properties, strength, toughness and wear resistance are slightly inferior to those of SBS. Therefore, there is an urgent need to improve the mechanical properties of SEPS while reducing the production cost of asphalt. Summary of the invention

[0004] The purpose of the present invention is to provide an environmentally friendly composite modified asphalt and a preparation method thereof, which can improve the mechanical properties, low temperature properties and ductility of asphalt and anti-ultraviolet aging properties, while reducing the production cost of asphalt.

[0005] The embodiments of the present invention are implemented by the following technical solutions:

[0006] An environmentally friendly composite modified asphalt comprises, by weight, 8-12 parts of a SEPS modifier, 2-4 parts of bio-based polyhexanediol azelate, 3-5 parts of rubber oil, and 79-87 parts of a base asphalt; the SEPS modifier is blended and modified with a multi-polymer.

[0007] The method for preparing the above-mentioned environmentally friendly composite modified asphalt comprises the following steps:

[0008] S1. After heating the base asphalt, add rubber oil, and stir and mix continuously to obtain asphalt mixture I;

[0009] S2, adding SEPS modifier to the asphalt mixture I obtained in step S1 in batches, and continuously stirring and mixing to obtain asphalt mixture II;

[0010] S3, heating the asphalt mixture II obtained in step S2, high-speed shearing for a period of time, then adding bio-based polyhexanediol azelaic acid ester, and continuing to stir and mix evenly to obtain a mixed material;

[0011] S4, swelling the mixture of step S3 at a certain temperature for a period of time to obtain an environmentally friendly composite modified asphalt.

[0012] The technical solution of the embodiment of the present invention has at least the following advantages and beneficial effects:

[0013] 1. The SEPS modifier prepared by blending SEPS, EPDM or TPEE and PP in the present invention has a side chain methyl group in its soft segment structure, which enhances its interaction with asphaltene and significantly improves the storage stability of the modified asphalt. Compared with the traditional method of using sulfur to improve storage stability, it is more in line with the concept of green environmental protection, and can significantly improve the high temperature performance and anti-ultraviolet aging performance of the base asphalt. While improving the overall performance, it can significantly reduce the amount of SEPS, thereby reducing the overall cost of materials.

[0014] 2. The present invention uses bio-based poly(hexanediol nonacid) in combination with a SEPS modifier to significantly improve the low-temperature performance, ductility and UV aging resistance of the base asphalt. Without changing the structure of the SEPS modifier, the interaction force between the SEPS modifier chains can be reduced, while also reducing the glass transition temperature and crystallinity of the SEPS modifier, improving the ductility of the SEPS modifier, reducing stress concentration, and dispersing external forces, thereby improving the elongation at break and fatigue resistance of the SEPS modifier. More importantly, the bio-based poly(hexanediol nonacid) and the SEPS modifier have good compatibility, so they can work stably together to effectively improve the low-temperature performance of the base asphalt, so that it is suitable for use in areas with a wider temperature range. DETAILED DESCRIPTION

[0015] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0016] The following is a detailed description of an environmentally friendly composite modified asphalt and a preparation method thereof provided in an embodiment of the present invention.

[0017] An environmentally friendly composite modified asphalt comprises, by weight, 8-12 parts of a SEPS modifier, 2-4 parts of bio-based polyhexanediol azelate, 3-5 parts of rubber oil, and 79-87 parts of a base asphalt; the SEPS modifier is blended and modified with a multi-polymer.

[0018] Furthermore, the multipolymer includes at least two of EPDM, TPEE and PP.

[0019] Furthermore, the SEPS modifier comprises EPDM, PP, and SEPS in a mass ratio of 52-54:36-37:10-11.

[0020] Furthermore, the SEPS modifier comprises TPEE, PP, and SEPS in a mass ratio of 52-54:36-37:10-11.

[0021] Furthermore, the preparation method of the SEPS modifier is as follows:

[0022] 1) blending at least two of EPDM, TPEE and PP with SEPS, stirring and mixing at a certain temperature for a period of time, and then cooling to obtain a pre-plasticized material;

[0023] 2) pre-vulcanizing the pre-plasticized material obtained in step 1) by a mixer, and then dynamically vulcanizing it by a screw extruder at a high temperature, wherein the dynamic vulcanization temperature is 170-175° C. and the dynamic vulcanization time is 6-8 minutes;

[0024] The present invention can make full use of the weather resistance and elasticity, light weight and molding performance of the material, as well as the tensile strength and high stability of carbon-carbon single bonds by blending SEPS with EPDM or TPEE and PP to significantly improve the high temperature performance and anti-ultraviolet aging performance of the base asphalt, and can significantly reduce the amount of SEPS used while improving the overall performance, thereby reducing the overall material cost;

[0025] However, the inventors found in research and practice that the SEPS modifier has a weak effect on the low-temperature performance and ductility of the base asphalt. Therefore, the present invention uses bio-based poly(hexanediol azelaic acid) to reduce the interaction between the SEPS modifier chains without changing the structure of the SEPS modifier, especially reducing the hydrogen bond and van der Waals force, while also reducing the glass transition temperature and crystallinity of the SEPS modifier, mainly destroying the ordered structure of some crystalline regions, making the polymer more uniform and soft; while in the non-crystalline region, the chain segment mobility can be increased, thereby improving the ductility of the SEPS modifier. More importantly, the bio-based poly(hexanediol azelaic acid) has good compatibility with the SEPS modifier and can be evenly dispersed in the ternary blend matrix of the SEPS modifier, ensuring that the bio-based poly(hexanediol azelaic acid) can effectively act on the entire polymer system, avoiding phase separation and migration problems of the bio-based poly(hexanediol azelaic acid) and thus stably improving the ductility of the SEPS modifier and effectively improving the low-temperature performance of the base asphalt, so that it is suitable for use in areas with a wider temperature range.

[0026] Furthermore, the preparation method of the bio-based polyhexanediol azelate is as follows:

[0027] a) mixing bio-based azelaic acid and hexanediol for melt esterification, adding a titanium catalyst, and esterifying at a certain temperature under a protective gas atmosphere (such as nitrogen, argon, etc.);

[0028] b) After the water outflow slows down, the temperature is raised and maintained for a period of time until the water outflow completely stops the reaction, thus preparing the bio-based polyhexanediol azelaic acid ester.

[0029] Furthermore, in step a), the titanium-based catalyst is a titanium-based catalyst having a titanium content of not less than 7 ppm; in step a), bio-based azelaic acid and hexanediol are mixed at an acid-to-alcohol molar ratio of 1:1.1-1.5.

[0030] Furthermore, in step a), the esterification is carried out at a temperature of 160-180° C.; in step b), after the water output slows down, the temperature is raised to 190-200° C. and maintained for 10-20 minutes.

[0031] The method for preparing the above-mentioned environmentally friendly composite modified asphalt comprises the following steps:

[0032] S1. After heating the base asphalt, add rubber oil, and stir and mix continuously to obtain asphalt mixture I;

[0033] S2, adding SEPS modifier to the asphalt mixture I obtained in step S1 at least three times, and the amount added each time increases successively, and continuously stirring and mixing to obtain asphalt mixture II;

[0034] S3, heating the asphalt mixture II obtained in step S2, high-speed shearing for a period of time, then adding bio-based polyhexanediol azelaic acid ester, and continuing to stir and mix evenly to obtain a mixed material;

[0035] S4, swelling the mixture of step S3 at a certain temperature for a period of time to obtain an environmentally friendly composite modified asphalt.

[0036] Example 1

[0037] An environmentally friendly composite modified asphalt comprises, by weight, 10 parts of a SEPS modifier, 3 parts of bio-based polyhexanediol azelate, 4 parts of rubber oil, and 83 parts of a base asphalt; the SEPS modifier comprises, by mass ratio, EPDM, PP, and SEPS in a ratio of 53:36:11.

[0038] The method for preparing the above-mentioned environmentally friendly composite modified asphalt comprises the following steps:

[0039] (1) Preparation of SEPS modifier

[0040] 11) EPDM, PP and SEPS were blended and added into a high-speed mixer at a mixing speed of 1400 rpm, mixed at a temperature of 155° C. for 20 minutes, discharged and cooled to obtain a pre-plasticized material;

[0041] 12) The pre-plasticized material obtained in step 11) is pre-vulcanized in an internal mixer, and then dynamically vulcanized at high temperature by a screw extruder, the dynamic vulcanization temperature is 175° C., and the dynamic vulcanization time is 7 minutes;

[0042] (2) Preparation of bio-based polyhexanediol azelaic acid ester

[0043] The bio-based azelaic acid and hexanediol are mixed at an acid-to-alcohol molar ratio of 1:1.1, and a titanium catalyst having a titanium content of not less than 7 ppm is added, and the temperature is maintained at 180° C. for esterification in a nitrogen environment, and the temperature is raised to 190° C. after the water output slows down, and the temperature is maintained for 10 minutes, and the reaction is stopped after the water output is completely stopped, thereby preparing bio-based polyhexanediol azelaic acid ester;

[0044] (3) Preparation of composite modified asphalt

[0045] S1. After heating the base asphalt to 165°C, add rubber oil and stir and mix evenly to obtain asphalt mixture I;

[0046] S2, adding the above-mentioned SEPS modifier to the asphalt mixture I obtained in step S1 in three times, with the amount added increasing each time, and stirring and mixing continuously to obtain asphalt mixture II;

[0047] S3, heating the asphalt mixture II obtained in step S2 to 180° C., and high-speed shearing at 4000 r / min for 1 hour under a constant temperature controller, and then adding bio-based polyhexanediol azelaic acid ester, stirring at a speed of 600 r / min for 15-20 minutes to obtain a mixed material;

[0048] S4. Place the mixture of step S3 in a constant temperature box at 180° C. to swell and develop for 2 hours, thereby obtaining an environmentally friendly composite modified asphalt.

[0049] Example 2

[0050] The difference between this embodiment and Embodiment 1 is that: an environmentally friendly composite modified asphalt, calculated by weight, comprises: 9 parts of SEPS modifier, 4 parts of bio-based polyhexanediol azelaic acid ester, 5 parts of rubber oil, and 82 parts of base asphalt; the SEPS modifier comprises: EPDM, PP, and SEPS in a mass ratio of 52:37:11.

[0051] Example 3

[0052] The difference between this embodiment and Embodiment 1 is that: an environmentally friendly composite modified asphalt, calculated by weight, comprises: 11 parts of SEPS modifier, 1 part of bio-based polyhexanediol azelaic acid ester, 3 parts of rubber oil, and 85 parts of base asphalt; the SEPS modifier comprises: TPEE, PP, SEPS in a mass ratio of 54:36:10.

[0053] Example 4

[0054] The difference between this embodiment and Embodiment 1 is that: an environmentally friendly composite modified asphalt, calculated by weight, comprises: 12 parts of SEPS modifier, 2 parts of bio-based poly(hexanediol azelaic acid), 3 parts of rubber oil, and 83 parts of base asphalt; the SEPS modifier comprises: TPEE, PP, and SEPS in a mass ratio of 53:37:10.

[0055] Example 5

[0056] The difference between this embodiment and Embodiment 1 is that: an environmentally friendly composite modified asphalt, calculated by weight, comprises: 8 parts of SEPS modifier, 2 parts of bio-based polyhexanediol azelaic acid ester, 3 parts of rubber oil, and 87 parts of base asphalt; the SEPS modifier comprises: EPDM, PP, and SEPS in a mass ratio of 54:36:10.

[0057] Example 6

[0058] The difference between this embodiment and Embodiment 1 is that: an environmentally friendly composite modified asphalt, comprising, by weight: 8 parts of SEPS modifier, 4 parts of bio-based polyhexanediol azelaic acid ester, 4 parts of rubber oil, and 86 parts of base asphalt; the SEPS modifier comprises, by mass ratio: TPEE, PP, SEPS in an amount of 52:37:11.

[0059] Comparative Example 1

[0060] The difference between this comparative example and Example 1 is that: a SEPS modified asphalt is prepared from the following raw materials in parts by weight: 10 parts of SEPS, 3 parts of bio-based poly(hexanediol azelaic acid), 4 parts of rubber oil, and 83 parts of base asphalt.

[0061] SEPS modified asphalt was prepared as follows:

[0062] After the base asphalt and the SEPS modifier are mixed, high-speed shearing is performed at 180°C for 0.5 hours, and the shearing speed should be maintained at 4000 rpm. After the shearing is completed, bio-based polyhexanediol azelaic acid is added to the intermediate product, and the mixture is uniformly mixed at 600 rpm for 2 hours at 180°C. After swelling, the SEPS modified asphalt is obtained.

[0063] Comparative Example 2

[0064] The difference between this comparative example and Example 1 is that: a SEPS modified asphalt does not contain bio-based polyhexanediol azelaic acid ester.

[0065] Experimental Example 1

[0066] (I) Test materials: Example 1, Comparative Example 1.

[0067] (II) Test methods:

[0068] The modified asphalt prepared as above was sampled separately and subjected to the rotational viscosity, needle penetration, softening point and ductility tests specified in the "Test Procedures for Asphalt and Asphalt Mixtures for Highway Engineering".

[0069] (III) The test results are shown in Table 1:

[0070] Table 1 Comparison of performance test results of Examples 1-3 and Comparative Example 1

[0071] Experimental Project Technical indicators Example 1 Comparative Example 1 Rotational viscosity (135℃) / Pa·S <3 2.36 2.15 Needle penetration (25℃) / 0.1mm 30~60 56 60 Softening point / ℃ >60 87.5 79.4 Elongation (5℃) / cm >20 33.2 34.3

[0072] It can be seen from the results in Table 1 that the composite modified asphalt prepared by the present invention has a larger rotational viscosity, softening point, smaller needle penetration, and similar ductility compared with the SEPS modified asphalt with the same dosage, which indicates that the blending of EPDM, PP, and SEPS effectively improves the mechanical properties of SEPS, and the modified asphalt prepared by the EPDM / PP / SEPS ternary blending modifier has better performance than SPES modified asphalt.

[0073] Experimental Example 2

[0074] (I) Test materials: Example 1, Comparative Example 2.

[0075] (II) Test methods:

[0076] The modified asphalt prepared above was sampled and subjected to 60°C temperature scanning, multiple stress creep recovery test and 25°C linear amplitude scanning test using a dynamic shear rheometer. A -18°C low-temperature bending test was performed using a bending beam rheometer. Another sample was taken and the asphalt was subjected to UV aging using a UVA-340 light source for a total duration of 8 hours. After the aging was completed, the same performance test was performed.

[0077] (III) The test results are shown in Table 2:

[0078] The performance test data of the modified asphalt obtained in this example are shown in Table 2.

[0079] Table 2 Comparison of rheological properties test results of Examples 1-3 and Comparative Example 2

[0080]

[0081]

[0082] It can be seen from the data in Table 2 that the low-temperature bending performance and UV aging resistance of the composite modified asphalt prepared by the present invention only show a slight decline, and the recovery rate is high; while in the control example, due to the absence of bio-based poly(hexanediol azelaic acid), the low-temperature performance, ductility and UV aging resistance of the base asphalt are relatively weak.

[0083] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An environmentally friendly composite modified asphalt, characterized in that: The invention comprises, by weight: 8-12 parts of SEPS modifier, 2-4 parts of bio-based polyhexanediol azelate, 3-5 parts of rubber oil and 79-87 parts of matrix asphalt; the SEPS modifier is blended and modified with a multi-polymer.

2. The environmentally friendly composite modified asphalt according to claim 1, characterized in that: The multipolymer includes at least two of EPDM, TPEE and PP.

3. The environmentally friendly composite modified asphalt according to claim 2, characterized in that: The SEPS modifier comprises EPDM, PP and SEPS in a mass ratio of 52-54:36-37:10-11.

4. The environmentally friendly composite modified asphalt according to claim 2, characterized in that: The SEPS modifier comprises TPEE, PP and SEPS in a mass ratio of 52-54:36-37:10-11.

5. The environmentally friendly composite modified asphalt according to claim 3 or 4, characterized in that: The preparation method of the SEPS modifier is as follows: 1) blending at least two of EPDM, TPEE and PP with SEPS, stirring and mixing at a certain temperature for a period of time, and then cooling to obtain a pre-plasticized material; 2) The pre-plasticized material obtained in step 1) is pre-vulcanized by an internal mixer, and then dynamically vulcanized by a screw extruder at a high temperature, wherein the dynamic vulcanization temperature is 170-175° C. and the dynamic vulcanization time is 6-8 minutes.

6. The environmentally friendly composite modified asphalt according to claim 1, characterized in that: The preparation method of the bio-based polyhexanediol azelate is as follows: a) mixing bio-based azelaic acid and hexanediol for melt esterification, adding a titanium catalyst, and esterifying at a certain temperature under a protective gas atmosphere; b) After the water outflow slows down, the temperature is raised and maintained for a period of time until the water outflow completely stops the reaction, thus preparing the bio-based polyhexanediol azelaic acid ester.

7. The environmentally friendly composite modified asphalt according to claim 6, characterized in that: In step a), the titanium-based catalyst is a titanium-based catalyst having a titanium content of not less than 7 ppm; in step a), bio-based azelaic acid and hexanediol are mixed at an acid-to-alcohol molar ratio of 1:1.1-1.

5.

8. The environmentally friendly composite modified asphalt according to claim 6, characterized in that: In step a), the esterification is carried out at a temperature of 160-180° C.; in step b), the temperature is raised to 190-200° C. after the water output slows down and maintained for 10-20 minutes.

9. A method for preparing an environmentally friendly composite modified asphalt according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1. After heating the base asphalt, add rubber oil, and stir and mix continuously to obtain asphalt mixture I; S2, adding SEPS modifier to the asphalt mixture I obtained in step S1 in batches, and continuously stirring and mixing to obtain asphalt mixture II; S3, heating the asphalt mixture II obtained in step S2, high-speed shearing for a period of time, then adding bio-based polyhexanediol azelaic acid ester, and continuing to stir and mix evenly to obtain a mixed material; S4, swelling the mixture of step S3 at a certain temperature for a period of time to obtain an environmentally friendly composite modified asphalt.

10. The method for preparing the environmentally friendly composite modified asphalt according to claim 9, characterized in that: In S2, the SEPS modifier is added at least three times, and the amount added each time increases successively.

Citation Information

Cited By

  • Rigidity-toughness synergistic enhanced heavy-duty pavement composite material and preparation method thereof

    CN121022127A