All-solid-content photocureable coating for power / energy storage battery insulation as well as preparation method and application of all-solid-content photocureable coating
By using improved all-solid photocuring coatings on the lithium-ion battery cell shell, combined with the proportion adjustment of rheology additives, the problems of low coating utilization rate and environmental pollution in the prior art are solved, and efficient and environmentally friendly Insulating protective coating is formed.
Patent Information
- Application Number
- CN202410588756.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-13
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-05-13
AI Technical Summary
The existing lithium-ion battery cell shell insulation coatings have shortcomings in terms of efficient utilization and environmental friendliness. Sprayed powder coatings require high temperature baking and low recovery rate. UV curing coatings have a high environmental pollution, while dip coating processes have high viscosity. It is difficult to apply all-solid photocuring coatings.
Using an all-solid photocuring coating containing epoxy acrylate resin, polyurethane acrylate, functionalized acrylate, silane coupling agent and rheology additive, the ratio of rheology additives (vapor phase silica, poly Amide wax and bentonite) to improve the rheological properties of the coating, suitable for dip coating processes to form an insulating protective coating of uniform thickness.
It realizes efficient use of all-solid photocuring coatings under dip coating process, reduces product coating costs, improves the mechanical wear resistance, chemical resistance and insulation performance of the coating, and ensures the basic performance requirements of the battery case. , while reducing environmental pollution.
Smart Images

Figure BDA0004836582240000061 
Figure BDA0004836582240000062 
Figure BDA0004836582240000071
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of coatings for electrical insulation of battery core shells, and more specifically to a full-solid light-curing coating for insulation of power / energy storage batteries, and a preparation method and application thereof. Background Art
[0002] As the core component of new energy vehicles, power batteries have always been the focus of researchers. The lithium-ion battery cells in new energy vehicles have relatively high requirements for electrical insulation, and usually require a coating with excellent insulation performance to be attached to the lithium-ion battery cell shell.
[0003] At present, the coatings used for insulation protection of aluminum shells of lithium-ion battery cells mainly include spray powder coatings and UV-curing coatings: 1) The advantage of spray powder coatings is the high coating recovery rate, but the disadvantage is that they require high-temperature baking, which is not energy-efficient, and the battery cells can only be installed and electrolytes can only be filled after spraying; 2) The advantage of spraying UV-curing coatings is low-temperature curing, and the product can be sprayed after the battery cells and electrolytes are installed. The disadvantage is the low coating recovery rate. For example, when ordinary air pressure spraying is used, only about 35% of the components are adsorbed on the surface of the aluminum shell, and about 65% falls on the outside of the aluminum shell or is sucked away by the exhaust duct. The unrecovered coating pollutes the environment and indirectly increases the coating cost of the product.
[0004] The dip coating process is a construction method that uses immersion to achieve the purpose of coating. The operation is to immerse the object to be coated in the paint liquid, lift the object to be coated out of the paint liquid after all parts are stained with the paint liquid, and naturally or forcibly make the excess paint drip back into the paint tank. After drying, a coating film is formed on the surface of the object to be coated, with a coating utilization rate close to 100%. However, the dip coating process has high requirements for the leveling and sagging performance of the coating, and it is easy to have problems such as high film thickness and uneven film thickness of the coated object, especially for all-solid light-curing coatings with high viscosity. The probability of problems is greater. Therefore, there is no relevant report on the application of all-solid light-curing coatings to automotive power batteries using the dip coating process. Summary of the invention
[0005] In view of the shortcomings of the prior art, the first object of the present invention is to provide a full-solid light-curing coating for power / energy storage battery insulation.
[0006] The second object of the present invention is to provide a method for preparing the all-solid photocurable coating as described above.
[0007] The third object of the present invention is to provide an application of the all-solid photocurable coating as described above in the preparation of power / energy storage batteries.
[0008] In order to achieve the above first object, the present invention adopts the following technical scheme:
[0009] The present invention discloses a full-solid light-curing coating for power / energy storage battery insulation. The full-solid light-curing coating comprises
[0010] Epoxy acrylate resin 10-30 parts;
[0011] 10-30 parts of polyurethane acrylate resin;
[0012] 25-50 parts of functionalized acrylate;
[0013] 1-5 parts of silane coupling agent;
[0014] 5-15 parts of initiator; and
[0015] Rheological additive 0.5-2.5 parts;
[0016] The rheological additive comprises 0.2-2 parts of fumed silica, 0.2-2 parts of polyamide wax and 0.1-2 parts of bentonite.
[0017] Furthermore, the rheological additive comprises 0.5-1 part of fumed silica, 0.5-1 part of polyamide wax and 0.5-1 part of bentonite.
[0018] Furthermore, the mass ratio of the fumed silica, polyamide wax and bentonite is 1:1-2:1-2.
[0019] Further, the fumed silica is a hydrophobic fumed silica, selected from one or more of AEROSIL R972, ER972, R974 of Evonik Industries, Germany; HDK H20, H15, H30 of Wacker Chemical (China) Co., Ltd. and IS-SD2003L, SD2002P, SD1506Y, SD2001L of Hangzhou Yingxing New Materials Co., Ltd.;
[0020] The polyamide wax is selected from one or more of 8100, 8200, and 8300 of Jiangxi Longhai Chemical Co., Ltd.;
[0021] The bentonite is an organic bentonite selected from Bentone 38 and / or SD-2 produced by Shanghai Hi-Tech Chemical Co., Ltd.
[0022] Furthermore, the functionalized acrylate is selected from one or more of monofunctional acrylate, difunctional acrylate and multifunctional acrylate.
[0023] Further, the monofunctional acrylate is selected from one or more of acryloylmorpholine, isobornyl methacrylate, isobornyl acrylate, N-hydroxyethylacrylamide, hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate and hydroxypropyl methacrylate;
[0024] The bifunctional acrylate is selected from one or more of hexylene glycol diacrylate, tricyclodecane dimethanol diacrylate, tricyclodecane dimethanol dimethyl diacrylate, and Boxing New Materials Co., Ltd. B-02;
[0025] The multifunctional acrylate is selected from one or more of tris(2-hydroxyethyl)isocyanuric acid triacrylate, pentaerythritol triacrylate, dipentaerythritol hexaacrylate, propoxylated glycerol triacrylate, ethoxylated trimethylolpropane triacrylate, and Boxing New Materials Co., Ltd. B-05.
[0026] Further, the epoxy acrylate resin is selected from one or more of EBECRYL 3300 of Allnex Resins (China) Co., Ltd., NeoRad E-20 of Covestro Polymers (China) Co., Ltd., and B-100M of Boxing New Materials Co., Ltd.;
[0027] The polyurethane acrylate resin is selected from one or more of EBECRYL 4265 and EBECRYL8254 of Allnex Resins (China) Co., Ltd.; AgiSyn 230A2 and NeoRad E-20 of Covestro Polymers (China) Co., Ltd.; B-2018 of Boxing New Materials Co., Ltd. and W682 of Guangzhou Five Elements Material Technology Co., Ltd.
[0028] Further, the silane coupling agent is selected from one or more of A187 of Momentive High-Tech Materials Group, USA, 2063H of Lubrizol Management (Shanghai) Co., Ltd., KBM803 and KBM403 of Shin-Etsu Chemical Co., Ltd. of Japan;
[0029] The initiator is selected from one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide.
[0030] Furthermore, the all-solid light-curing coating also includes 3-15 parts of filler, 0-1 part of leveling agent, 0-1 part of defoaming agent and 2-5 parts of color paste.
[0031] In order to achieve the above second purpose, the present invention adopts the following technical solutions:
[0032] The present invention discloses a method for preparing the all-solid light-curing coating as described above, comprising the following steps:
[0033] Add epoxy acrylate resin, polyurethane acrylate resin, functional acrylate, silane coupling agent and initiator into a container, mix until uniform, add rheological additive, and continue stirring until uniform.
[0034] In order to achieve the third object, the present invention adopts the following technical solutions:
[0035] The present invention discloses the use of the all-solid photocurable coating as described above in the preparation of power / energy storage batteries, wherein the application is to use the all-solid photocurable coating to form an insulating protective coating on the surface of a cell casing or other cell insulating components in a power / energy storage battery.
[0036] Furthermore, the surface of the cell shell or other cell insulation components in the power / energy storage battery is dip-coated with the all-solid light-curing coating to form an insulating protective coating.
[0037] Furthermore, the dry film thickness of the insulating protective coating is 80-120 μm, and the thickness difference of the insulating protective coating formed in the entire dip-coating area of the component is no more than 10 μm.
[0038] Furthermore, the battery cell shell is an aluminum battery cell shell.
[0039] The beneficial effects of the present invention are as follows:
[0040] The present invention selects suitable monomers and oligomers, and then initiates polymerization of epoxy acrylate resin, polyurethane acrylate resin, functionalized acrylate and silane coupling agent under the action of a photoinitiator to obtain the coating. The epoxy acrylate resin in the formula can provide the coating with excellent chemical resistance and good insulation. The polyurethane acrylate resin has an urethane bond in its structure, and hydrogen bonds can be formed between molecular chains, so that the coating has excellent mechanical wear resistance and chemical resistance. The functionalized acrylate can be used as an active diluent, and together with the silane coupling agent, it ensures strong adhesion of the coating. Under the joint action of the above monomers and oligomers, the coating has excellent mechanical wear resistance, pressure resistance, high and low temperature impact resistance, chemical resistance, insulation performance, etc., and can meet the basic performance requirements of the battery shell.
[0041] The present invention selects three rheological additives, namely, fumed silica, polyamide wax and bentonite, for combination, and imparts excellent rheological properties to the all-solid light-curing coating by adjusting the ratio of the three rheological additives, so that the all-solid light-curing coating can still obtain a coating film of uniform thickness under the dipping process, thereby improving the utilization rate of the all-solid light-curing coating and reducing the coating cost of the product. DETAILED DESCRIPTION
[0042] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0043] The dip coating process is a commonly used coating process in the field of coatings. It is characterized by high production efficiency, no paint mist, more environmentally friendly, simple operation, and less paint loss. For the dip coating process, the main process parameter is the coating viscosity, which directly affects the appearance and thickness of the paint film. If the coating viscosity is too low and the coating contains too much solvent, it will lead to problems such as the paint film being too thin, severe flow marks, residual paint not dripping, and uneven film thickness in the upper and lower parts. If the coating viscosity is too high, it will lead to problems such as thicker paint film and poor fluidity of the coating. All-solid light-curing coatings usually have a lower viscosity. Therefore, if it is considered to apply all-solid light-curing coatings to the substrate surface by dip coating in actual applications, the first problem to be solved is to improve the rheological properties of the coating to obtain a moderate viscosity.
[0044] Adding rheological additives is one of the most effective methods to adjust the viscosity of coatings and has been widely used in the coatings field. Rheological additives commonly used in coatings include organic bentonite, fumed silica, polyamide wax, hydrogenated castor oil, etc. However, at this stage, the use of these rheological additives focuses more on introducing rheological additives to increase the viscosity of the system and thus obtain better anti-settling effect or storage stability, and less attention is paid to improving the thickness of the paint film and the uniformity of the film thickness.
[0045] The first aspect of the present invention provides a full-solid light-curing coating matched with a dip coating process and applied to power / energy storage battery insulation, wherein the full-solid light-curing coating comprises
[0046] Epoxy acrylate resin 10-30 parts;
[0047] 10-30 parts of polyurethane acrylate resin;
[0048] 25-50 parts of functionalized acrylate;
[0049] 1-5 parts of silane coupling agent;
[0050] 5-15 parts of initiator; and
[0051] Rheological additive 0.5-2.5 parts;
[0052] The rheological additive comprises 0.2-2 parts of fumed silica, 0.2-2 parts of polyamide wax and 0.1-2 parts of bentonite.
[0053] Due to the differences in the structures of fumed silica, polyamide wax and bentonite and the interactions between them and other components in the coating, the present invention uses the three rheological additives of fumed silica, polyamide wax and bentonite in combination to obtain a better thixotropy improvement effect, thereby eliminating the problems of thick paint film and uneven film thickness in the upper and lower parts of the all-solid light-curing coating during dip coating.
[0054] The fumed silica has a small particle size, a large specific surface area, good compatibility with film-forming resins, is easy to form hydrogen bonds, and has a large thixotropic index. In a specific embodiment, the fumed silica is a hydrophobic fumed silica selected from one or more of AEROSIL R972, ER972, and R974 of Evonik Industries, Germany; HDK H20, H15, and H30 of Wacker Chemical (China) Co., Ltd.; and IS-SD2003L, SD2002P, SD1506Y, and SD2001L of Hangzhou Yingxing New Materials Co., Ltd.
[0055] The polyamide wax has a network structure, has very good heat resistance and storage stability, and has a moderate increase in the viscosity of the system. In a specific embodiment, the polyamide wax is selected from one or more of 8100, 8200, and 8300 of Jiangxi Longhai Chemical Co., Ltd.
[0056] Bentonite has swelling, adhesion, cation exchange, etc., and is easy to achieve various modifications. It can form a main network structure in the coating, giving the coating a certain structural viscosity. In a specific embodiment, the bentonite is an organic bentonite selected from Bentone 38 and / or SD-2 of Haiming Si Deqian (Shanghai) Chemical Co., Ltd.
[0057] In order to obtain better thixotropy, the present invention further optimizes the addition amount of three rheological additives of fumed silica, polyamide wax and bentonite, and the rheological additive comprises 0.5-1 part of fumed silica (preferably 0.5 part), 0.5-1 part of polyamide wax and 0.5-1 part of bentonite. Further, when the fumed silica is less than or equal to the addition amount of polyamide wax and bentonite, the effect is better. In a specific embodiment, when the mass ratio of the fumed silica, polyamide wax and bentonite is 1:1-2:1-2, the improvement effect for the system is better, illustratively, the mass ratio of the fumed silica, polyamide wax and bentonite can be 1:1:1, 1:1:1.5, 1:1:2, 1:1.5:1, 1:1.5:1.5, 1:1.5:2, 1:2:1, 1:2:1.5, 1:2:2, etc.
[0058] Furthermore, the epoxy acrylate resin is selected from one or more of EBECRYL 3300 of Allnex Resins (China) Co., Ltd., NeoRad E-20 of Covestro Polymers (China) Co., Ltd., and B-100M of Boxing New Materials Co., Ltd.
[0059] Furthermore, the polyurethane acrylate resin has an urethane bond in its structure, and hydrogen bonds can be formed between molecular chains to provide the coating with excellent mechanical wear resistance and chemical resistance, including but not limited to one or more of EBECRYL 4265 and EBECRYL 8254 of Allnex Resins (China) Co., Ltd.; AgiSyn 230A2 and NeoRad E-20 of Covestro Polymers (China) Co., Ltd.; B-2018 of Boxing New Materials Co., Ltd. and W682 of Guangzhou Five Elements Material Technology Co., Ltd.
[0060] Further, the functionalized acrylate is selected from one or more of monofunctional acrylate, difunctional acrylate and multifunctional acrylate;
[0061] The monofunctional acrylate is selected from one or more of acryloylmorpholine, isobornyl methacrylate, isobornyl acrylate, N-hydroxyethylacrylamide, hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate and hydroxypropyl methacrylate;
[0062] The bifunctional acrylate is selected from one or more of hexylene glycol diacrylate, tricyclodecane dimethanol diacrylate, tricyclodecane dimethanol dimethyl diacrylate, and Boxing New Materials Co., Ltd. B-02;
[0063] The multifunctional acrylate is selected from one or more of tris(2-hydroxyethyl)isocyanuric acid triacrylate, pentaerythritol triacrylate, dipentaerythritol hexaacrylate, propoxylated glycerol triacrylate, ethoxylated trimethylolpropane triacrylate, and Boxing New Materials Co., Ltd. B-05.
[0064] Further, the silane coupling agent is selected from one or more of A187 of Momentive High-Tech Materials Group, USA, 2063H of Lubrizol Management (Shanghai) Co., Ltd., KBM803 and KBM403 of Shin-Etsu Chemical Co., Ltd. of Japan;
[0065] The initiator is selected from one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone (referred to as initiator 1173), bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (referred to as initiator 819) and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (referred to as TPO).
[0066] Furthermore, the all-solid photocurable coating also contains 3-15 parts of filler, 0-1 parts of leveling agent, 0-1 parts of defoaming agent and 2-5 parts of color paste; in a specific embodiment, the all-solid photocurable coating contains 3-5 parts of filler, 0.3-1 parts of leveling agent, 0.3-1 parts of defoaming agent and 2-3 parts of color paste.
[0067] Exemplarily, the filler is selected from HY-A05 talc powder of Shenzhen Haiyang Powder Technology Co., Ltd., the leveling agent is selected from BYK361N and / or BYK UV3535 of BYK Additives (Shanghai) Co., Ltd., the defoaming agent is selected from BYK1790 and / or BYK1788 of BYK Additives (Shanghai) Co., Ltd., and the color paste is selected from color paste W1008-UV and / or B6153-UV of Guangdong Kedi New Materials Technology Co., Ltd.
[0068] A second aspect of the present invention provides a method for preparing the all-solid light-curing coating as described above, comprising the following steps:
[0069] 1) adding epoxy acrylate resin, polyurethane acrylate resin, functionalized acrylate, silane coupling agent and initiator into a container and mixing until uniform;
[0070] 2) Add rheological additive, filler, leveling agent, defoamer and color paste, and continue stirring until uniform.
[0071] Furthermore, the stirring rate of step 1) is 600-800 rpm, and the stirring time is 10-15 minutes, and the stirring rate of step 2) is 600-800 rpm, and the stirring time is 15-20 minutes.
[0072] The third aspect of the present invention provides a dip coating process for forming an insulating protective coating using the all-solid light-curing coating as described above, wherein the dip coating process adopts a secondary dip coating process and specifically comprises the following steps:
[0073] Place the all-solid light-curing coating in a coating tank with stirring and heating functions, preheat it to 45-55°C, immerse the parts to be dip-coated in the coating tank for one dip-coating, take them out after dipping, and cure them with a high-pressure mercury lamp, electrodeless lamp or LED. After curing, immerse the parts into the coating tank again for a second dip-coating, take them out after dipping, and cure them with a high-pressure mercury lamp, electrodeless lamp or LED.
[0074] Furthermore, the dry film thickness of the insulating protective coating is 80-120 μm, and the thickness difference of the insulating protective coating formed in the entire dip-coating area of the component is no more than 10 μm.
[0075] The component may be a cell casing in a power / energy storage battery, such as an aluminum casing, or may be other cell insulation components.
[0076] The following is further described by examples.
[0077] Examples 1-3
[0078] This group of examples provides three all-solid light-curing coating formulations, and the specific ingredients are shown in Table 1.
[0079] Table 1
[0080]
[0081] According to the formula in Table 1, epoxy acrylate resin, polyurethane acrylate resin, functionalized acrylate, silane coupling agent and initiator are added into a container and mixed until uniform. Then, fumed silica, polyamide wax, bentonite, filler, leveling agent, defoamer and color paste are added and stirred until uniform to obtain a full-solid light-curing coating.
[0082] Comparative Examples 1-7
[0083] This group of comparative examples provides seven all-solid light-curing coating formulations, and the specific ingredients are shown in Table 2.
[0084] Table 2
[0085]
[0086]
[0087] According to the formula in Table 2, epoxy acrylate resin, polyurethane acrylate resin, functionalized acrylate, silane coupling agent and initiator are added into the container and mixed until uniform. Then, fumed silica, polyamide wax, bentonite, filler, leveling agent, defoamer and color paste are added and stirred until uniform to obtain a full-solid light-curing coating.
[0088] Performance Testing
[0089] The all-solid light-curing coatings prepared in Examples 1-3 and Comparative Examples 1-7 are used in the cell casing of a power / energy storage battery. The specific method of use is as follows:
[0090] Place the all-solid light-curing coating in a coating tank with stirring and heating functions, preheat it to 45-55°C, immerse the battery cell shell in the coating tank, and perform a dip coating. After the dip coating is completed, take it out and cure it with a high-pressure mercury lamp, electrodeless lamp or LED. The curing light intensity is UVA200-300mw / cm 2 , energy is 2000-2500mj / cm 2After the curing is completed, the parts are immersed in the paint tank again for a second dip coating. After the dipping is completed, they are taken out and cured with a high-pressure mercury lamp, an electrodeless lamp or an LED. The expected dry film thickness after two dip coatings is 90-100μm. The obtained paint film is tested for the following items. The test methods and specific requirements are shown in Table 3.
[0091] Table 3
[0092]
[0093] The test results of Examples 1-3 are shown in Table 4.
[0094] Table 4
[0095]
[0096]
[0097] Note: Slightly poor leveling is an evaluation result between leveling OK and leveling NG. It is an intermediate state representation set according to the leveling scale requirements of different customers, but it is also considered leveling OK according to general requirements in the industry.
[0098] The test results of Comparative Examples 1-7 are shown in Table 5.
[0099] Table 5
[0100]
[0101]
[0102] in conclusion:
[0103] The present invention uses fumed silica, polyamide wax and bentonite in combination and combines them in a specific weight ratio, thereby greatly improving the construction performance of the all-solid light-curing coating under the dipping process, so that the insulating layer formed at different positions has a uniform film thickness, is flat and smooth, has good adhesion, and has excellent mechanical wear resistance, pressure resistance, high and low temperature impact resistance, chemical resistance, insulation performance and other paint film resistances.
[0104] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. A full solid light-curing coating for power / energy storage battery insulation, characterized in that: By weight, the all-solid light-curing coating comprises Epoxy acrylate resin 10-30 parts; 10-30 parts of polyurethane acrylate resin; 25-50 parts of functionalized acrylate; 1-5 parts of silane coupling agent; 5-15 parts of initiator; as well as Rheological additive 0.5-2.5 parts; The rheological additive comprises 0.2-2 parts of fumed silica, 0.2-2 parts of polyamide wax and 0.1-2 parts of bentonite.
2. The all-solid light-curing coating according to claim 1, characterized in that: The rheological additive comprises 0.5-1 part of fumed silica, 0.5-1 part of polyamide wax and 0.5-1 part of bentonite; Preferably, the mass ratio of the fumed silica, polyamide wax and bentonite is 1:1-2:1-2.
3. The all-solid light-curing coating according to claim 1, characterized in that: The fumed silica is a hydrophobic fumed silica, selected from one or more of AEROSIL R972, ER972, and R974 of Evonik Industries of Germany; HDK H20, H15, and H30 of Wacker Chemicals (China) Co., Ltd. and IS-SD2003L, SD2002P, SD1506Y, and SD2001L of Hangzhou Yingxing New Materials Co., Ltd.; The polyamide wax is selected from one or more of 8100, 8200, and 8300 of Jiangxi Longhai Chemical Co., Ltd.; The bentonite is an organic bentonite selected from Bentone 38 and / or SD-2 produced by Shanghai Hi-Tech Chemical Co., Ltd.
4. The all-solid light-curing coating according to claim 1, characterized in that: The functionalized acrylate is selected from one or more of monofunctional acrylate, difunctional acrylate and multifunctional acrylate; Preferably, the monofunctional acrylate is selected from one or more of acryloylmorpholine, isobornyl methacrylate, isobornyl acrylate, N-hydroxyethylacrylamide, hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate and hydroxypropyl methacrylate; The bifunctional acrylate is selected from one or more of hexylene glycol diacrylate, tricyclodecane dimethanol diacrylate, tricyclodecane dimethanol dimethyl diacrylate, and Boxing New Materials Co., Ltd. B-02; The multifunctional acrylate is selected from one or more of tris(2-hydroxyethyl)isocyanuric acid triacrylate, pentaerythritol triacrylate, dipentaerythritol hexaacrylate, propoxylated glycerol triacrylate, ethoxylated trimethylolpropane triacrylate, and Boxing New Materials Co., Ltd. B-05.
5. The all-solid light-curing coating according to claim 1, characterized in that: The epoxy acrylate resin is selected from one or more of EBECRYL 3300 of Allnex Resins (China) Co., Ltd., NeoRad E-20 of Covestro Polymers (China) Co., Ltd., and B-100M of Boxing New Materials Co., Ltd.; The polyurethane acrylate resin is selected from one or more of EBECRYL 4265 and EBECRYL8254 of Allnex Resins (China) Co., Ltd.; AgiSyn 230A2 and NeoRad E-20 of Covestro Polymers (China) Co., Ltd.; B-2018 of Boxing New Materials Co., Ltd. and W682 of Guangzhou Five Elements Material Technology Co., Ltd.
6. The all-solid light-curing coating according to claim 1, characterized in that: The silane coupling agent is selected from one or more of A187 of Momentive Advanced Materials Group, USA, 2063H of Lubrizol Management (Shanghai) Co., Ltd., KBM803 and KBM403 of Shin-Etsu Chemical Co., Ltd. of Japan; The initiator is selected from one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide.
7. The all-solid light-curing coating according to claim 1, characterized in that: The all-solid light-curing coating further comprises 3-15 parts of filler, 0-1 parts of leveling agent, 0-1 parts of defoaming agent and 2-5 parts of color paste.
8. The method for preparing a full-solid light-curing coating according to any one of claims 1 to 7, characterized in that: The steps include: Add epoxy acrylate resin, polyurethane acrylate resin, functional acrylate, silane coupling agent and initiator into a container, mix until uniform, add rheological additive, and continue stirring until uniform.
9. Use of the all-solid light-curing coating according to any one of claims 1 to 7 in the preparation of power / energy storage batteries, characterized in that: The application is to use the all-solid light-curing coating to form an insulating protective coating on the surface of the cell shell or other cell insulation components in the power / energy storage battery.
10. The use according to claim 9, characterized in that: Dip-coating the all-solid light-curing coating on the surface of the cell shell or other cell insulation components in the power / energy storage battery to form an insulating protective coating; Preferably, the dry film thickness of the insulating protective coating is 80-120 μm, and the thickness difference of the insulating protective coating formed in the entire dip-coated area of the component is not greater than 10 μm; Preferably, the battery cell casing is an aluminum battery cell casing.
Citation Information
Patent Citations
Colorful ultraviolet (UV) light solidifying paint
CN102212311A
Unsaturated polyester material with excellent covering power, black edge covering capacity and combination property and preparation method of unsaturated polyester material
CN109762450A
All-solid-content light-cured insulating glue and preparation process thereof
CN114561184A
Coating having macroscopic texture and process for making same
US20010038910A1
Combination of crosslinkers to improve coating properties
US20230012924A1
Cited By
High-temperature-resistant UV insulating paint applied to new energy battery and preparation method of high-temperature-resistant UV insulating paint
CN120005431A
Insulation protective agent for high-voltage and low-voltage joints of new energy automobile and preparation method of insulation protective agent
CN121555080A
New energy vehicle high-low voltage connector insulation protective agent and preparation method thereof
CN121555080B
Coating for surface of garden process scissors, preparation method and production equipment
CN122037775A