Organosilicon transparent adhesive and application thereof in photovoltaic cell packaging
By adding reinforcement resin, tackifying resin and loaded Pt complex catalyst to the silicone transparent adhesive, the bonding strength and toughness are improved, and the problem of low bonding strength of traditional silicone packaging adhesive is solved, and photovoltaic is realized High reliability packaging of batteries, suitable for low temperature processes of HJT or Topcon photovoltaic cells.
Patent Information
- Application Number
- CN202411231424.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-29
AI Technical Summary
Traditional silicone packaging glue has low bonding strength in photovoltaic cell packaging and cannot meet the sealing requirements in high temperature and high humidity environments. Especially under the low temperature process of HJT or Topcon photovoltaic cells, traditional soldering efficiency and adhesion are insufficient. .
Using a silicone transparent adhesive, the adhesive strength and toughness of the adhesive are improved and the packaging effect is improved by adding reinforcement resin, tackifying resin and loaded Pt complex catalyst. The adhesive includes vinyl silicone oil, vinyl MQ silicone resin, hydrogen-containing silicone oil, tackifying resin and a supported Pt complex catalyst, and is prepared by vacuum stirring to form a high-performance single-component room-temperature cured transparent adhesive.
It achieves high bonding strength, excellent light transmittance and aging resistance, meets the high reliability packaging requirements of photovoltaic cells, and is suitable for packaging of photovoltaic cells and electronic devices.
Smart Images

Figure BDA0005026257930000021 
Figure BDA0005026257930000031 
Figure BDA0005026257930000111
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of organic silicone adhesives, and in particular to an organic silicone transparent adhesive and application thereof in photovoltaic cell packaging. Background Art
[0002] With the continuous development of solar photovoltaic technology, new battery assembly processes and technologies emerge in an endless stream. The original PERC (Passivated Emitter and Rear Cell) process is gradually being replaced by HJT (Heterojunction Technology, amorphous silicon thin film) heterojunction battery process or Topcon (Tunnel Oxide Passivating Contacts) tunnel oxide passivating contact battery process.
[0003] Due to the low-temperature process characteristics of HJT or Topcon photovoltaic cells, the subsequent high-temperature packaging process used by traditional crystalline silicon cells cannot be adopted, and traditional soldering (soldering) is increasingly unable to meet the requirements of the cell assembly process in terms of efficiency and adhesion. Therefore, it is necessary to develop a suitable low-temperature packaging process.
[0004] Organic silicon encapsulant has excellent properties such as high temperature resistance and aging resistance, as well as good electrical insulation, elasticity, acid resistance and coolant resistance, so it can meet the sealing requirements of HJT or Topcon photovoltaic cells. However, since most organic silicon encapsulants use organic silicon as the base material, the main chain contains a large amount of Si-O, the bond length of Si-O is relatively long, and it has a helical molecular structure, so there are problems such as low bonding strength, which cannot meet the packaging requirements of photovoltaic cells. Summary of the invention
[0005] Based on the technical problems existing in the background technology, the present invention proposes a transparent silicone adhesive and its application in photovoltaic cell packaging. The adhesive not only has high bonding strength and light transmittance, but also has good strength and high-humidity aging resistance, thereby meeting the high-reliability packaging requirements of photovoltaic cells.
[0006] The present invention provides a transparent silicone adhesive, which comprises the following raw materials in parts by weight: 100 parts of vinyl silicone oil, 10-30 parts of reinforcing resin, 5-25 parts of hydrogenated silicone oil, 5-20 parts of tackifying resin, 0.1-5 parts of loaded Pt complex catalyst, 0.01-0.5 parts of inhibitor, and 0-30 parts of auxiliary agent.
[0007] In the present invention, by adding a specific amount of reinforcing resin, tackifying resin and loaded Pt complex catalyst into the transparent silicone adhesive, the bonding strength of the adhesive is improved while the strength and toughness properties are also greatly improved. The application in photovoltaic cells can effectively improve the packaging effect.
[0008] Preferably, the viscosity of the vinyl silicone oil is 500-50000 cps, and the vinyl content is 0.1-5 wt%.
[0009] Preferably, the reinforcing resin is vinyl MQ silicone resin or polyvinyl silicone oil;
[0010] Preferably, the reinforcing resin has a viscosity of 1000-20000 cps and a vinyl content of 0.5-3 wt%.
[0011] In the present invention, the reinforcing resin is vinyl MQ silicone resin or polyvinyl silicone oil, which can not only obtain a better reinforcing effect, but also improve the fluidity of the rubber material and ensure the bonding effect.
[0012] Preferably, the hydrogen-containing silicone oil is a side-chain hydrogen-containing silicone oil and / or a terminal hydrogen-containing silicone oil, and the hydrogen content thereof is 0.1-2 wt %.
[0013] Preferably, the structure of the tackifying resin is as follows:
[0014]
[0015] Among them, x, y, z are all greater than 0;
[0016] Preferably, the tackifying resin is obtained by copolymerizing alkenyl succinic anhydride, hydroxyethyl acrylate and methacryloxypropyl tris(trimethylsiloxy)silane in a mass ratio of 1:1-5:20-30.
[0017] In the present invention, the tackifying resin contains multiple reactive polar groups such as anhydride and hydroxyl groups, which can react with other components in the adhesive, thereby connecting the components in the adhesive, improving the mechanical strength of the adhesive and effectively enhancing the adhesion; at the same time, the silane structure contained in the tackifying resin forms a good compatibility with the silicone, further enhancing the reaction connection effect of multiple reactive polar groups such as anhydride and hydroxyl groups.
[0018] Preferably, the supported Pt complex catalyst is a silica-supported platinum-olefin complex;
[0019] Preferably, the silica-supported platinum-olefin complex is obtained by modifying silica with an aminosilane coupling agent, condensing with acryloyl chloride, and then complexing with potassium chloroplatinate.
[0020] In the present invention, the structural formula of the silica-supported platinum-olefin complex is shown in the following formula (1). The inorganic carrier-supported platinum catalyst can avoid the disadvantages of homogeneous catalysts corroding the reactor, difficulty in platinum recovery, and poor reaction efficiency. It also has the advantages of strong loading and high catalytic activity due to good mechanical strength and reaction medium stability, and is helpful for preparing a single-component room-temperature curing transparent organic silicone adhesive with excellent performance.
[0021]
[0022] R is an alkyl group or a nitrogen-containing alkyl group.
[0023] Preferably, the inhibitor is at least one of an acetylenic alcohol compound, a maleate compound or a fumarate compound;
[0024] Preferably, the alkynol compound is at least one of 1-ethynyl-1-cyclohexanol, 3-methyl-1-hexynyl-3-ol, 2-methyl-3-butynyl-2-ol or 3,5-dimethyl-1-hexynyl-3-ol.
[0025] Preferably, the auxiliary agent is at least one of a accelerator, a silane coupling agent, a thixotropic agent or an antioxidant.
[0026] The present invention also proposes a method for preparing the above-mentioned transparent silicone adhesive, comprising: vacuum stirring vinyl silicone oil, reinforcing resin, hydrogen-containing silicone oil, tackifying resin, inhibitor and auxiliary agent to obtain a premix; vacuum stirring a loaded Pt complex catalyst and the premix to obtain the transparent silicone adhesive.
[0027] The present invention also proposes an application of the transparent silicone adhesive in photovoltaic cell packaging.
[0028] Compared with the prior art, the transparent silicone adhesive of the present invention has better bonding strength, light transmittance, anti-aging performance and yellowing resistance, can be widely used in the fields of packaging of photovoltaic cells or electronic devices, and has high practicality. DETAILED DESCRIPTION
[0029] The technical solutions of the present invention are described in detail below through specific embodiments. However, it should be clearly stated that these embodiments are for illustration only and are not to be construed as limiting the scope of the present invention.
[0030] Example 1
[0031] A transparent silicone adhesive comprises the following raw materials in parts by weight: 100 parts of vinyl silicone oil, 20 parts of vinyl MQ silicone resin, 15 parts of hydrogenated silicone oil, 10 parts of tackifying resin, 1 part of supported Pt complex catalyst, and 0.1 part of 3,5-dimethyl-1-hexyn-3-ol;
[0032] The viscosity of vinyl silicone oil at 25°C is 1000cps, and the vinyl content is 0.8wt%; the hydrogen content of hydrogen-containing silicone oil is 0.3wt%; the viscosity of vinyl MQ silicone resin at 25°C is 8000cps, and the vinyl content is 0.96wt%;
[0033] The tackifying resin is prepared by the following method: alkenyl succinic anhydride, hydroxyethyl acrylate, methacryloyloxypropyl tris(trimethylsiloxy)silane and azobisisobutyronitrile are added into xylene in a mass ratio of 1:3:25:0.3 and ultrasonically dissolved completely, heated to 75° C. and reacted for 12 hours, cooled and then removed xylene to obtain the tackifying resin;
[0034] The supported Pt complex catalyst was prepared by the following method: fumed silica (with a specific surface area of 150 m 2 / g) and 3-aminopropyltriethoxysilane are added to N,N-dimethylformamide in a mass ratio of 1:1 and ultrasonically dispersed uniformly, and the mixture is heated to 100°C, reacted for 12 hours, filtered, washed, and dried in vacuo to obtain aminosilane coupling agent modified silica; aminosilane coupling agent modified silica, acryloyl chloride and triethylamine are added to toluene in a mass ratio of 1:0.02:0.5, stirred and refluxed for 4 hours, filtered, washed, and dried to obtain alkenyl modified silica; alkenyl modified silica and potassium chloroplatinate are added to acetone in a mass ratio of 1:0.05, stirred and refluxed for 48 hours under nitrogen protection, filtered, washed, and dried in vacuo to obtain a loaded Pt complex catalyst with a Pt content of 0.5wt%.
[0035] The preparation method of the above-mentioned transparent silicone adhesive is specifically as follows:
[0036] Under room temperature, the formulated amount of vinyl silicone oil, vinyl MQ silicone resin, hydrogenated silicone oil, tackifying resin and 3,5-dimethyl-1-hexyn-3-ol are sequentially added into a blender and stirred in vacuum for 1 hour to obtain a premix; after the premix is cooled to 30° C., the formulated amount of loaded Pt complex catalyst is added and stirred in vacuum for 30 minutes to obtain the transparent silicone adhesive.
[0037] Example 2
[0038] A transparent silicone adhesive comprises the following raw materials in parts by weight: 100 parts of vinyl silicone oil, 10 parts of vinyl MQ silicone resin, 25 parts of hydrogenated silicone oil, 5 parts of tackifying resin, 5 parts of supported Pt complex catalyst, and 0.5 parts of 1-ethynyl-1-cyclohexanol;
[0039] The viscosity of vinyl silicone oil at 25°C is 1000cps, and the vinyl content is 0.8wt%; the hydrogen content of hydrogen-containing silicone oil is 0.2wt%; the viscosity of vinyl MQ silicone resin at 25°C is 7000cps, and the vinyl content is 1.2wt%;
[0040] The tackifying resin is prepared by the following method: alkenyl succinic anhydride, hydroxyethyl acrylate, methacryloyloxypropyl tris(trimethylsiloxy)silane and azobisisobutyronitrile are added into xylene in a mass ratio of 1:3:25:0.3 and ultrasonically dissolved completely, heated to 75° C. and reacted for 12 hours, cooled and then removed xylene to obtain the tackifying resin;
[0041] The supported Pt complex catalyst was prepared by the following method: fumed silica (with a specific surface area of 150 m 2 / g) and 3-aminopropyltriethoxysilane are added to N,N-dimethylformamide in a mass ratio of 1:1 and ultrasonically dispersed uniformly, and the mixture is heated to 100°C, reacted for 12 hours, filtered, washed, and dried in vacuo to obtain aminosilane coupling agent modified silica; aminosilane coupling agent modified silica, acryloyl chloride and triethylamine are added to toluene in a mass ratio of 1:0.02:0.5, stirred and refluxed for 4 hours, filtered, washed, and dried to obtain alkenyl modified silica; alkenyl modified silica and potassium chloroplatinate are added to acetone in a mass ratio of 1:0.05, stirred and refluxed for 48 hours under nitrogen protection, filtered, washed, and dried in vacuo to obtain a loaded Pt complex catalyst with a Pt content of 0.5wt%.
[0042] The preparation method of the above-mentioned transparent silicone adhesive is specifically as follows:
[0043] Under room temperature, the formulated amount of vinyl silicone oil, vinyl MQ silicone resin, hydrogenated silicone oil, tackifying resin and 1-ethynyl-1-cyclohexanol are sequentially added into a blender and stirred in vacuum for 1 hour to obtain a premix; after the premix is cooled to 30° C., the formulated amount of loaded Pt complex catalyst is added and stirred in vacuum for 30 minutes to obtain the transparent silicone adhesive.
[0044] Example 3
[0045] A transparent silicone adhesive comprises the following raw materials in parts by weight: 100 parts of vinyl silicone oil, 30 parts of vinyl MQ silicone resin, 5 parts of hydrogenated silicone oil, 20 parts of tackifying resin, 0.1 parts of supported Pt complex catalyst, and 0.01 parts of 3-methyl-1-hexynyl-3-ol;
[0046] The viscosity of vinyl silicone oil at 25°C is 1000cps, and the vinyl content is 0.8wt%; the hydrogen content of hydrogen-containing silicone oil is 0.3wt%; the viscosity of vinyl MQ silicone resin at 25°C is 8000cps, and the vinyl content is 0.96wt%;
[0047] The tackifying resin is prepared by the following method: alkenyl succinic anhydride, hydroxyethyl acrylate, methacryloyloxypropyl tris(trimethylsiloxy)silane and azobisisobutyronitrile are added into xylene in a mass ratio of 1:3:25:0.3 and ultrasonically dissolved completely, heated to 75° C. and reacted for 12 hours, cooled and then removed xylene to obtain the tackifying resin;
[0048] The supported Pt complex catalyst was prepared by the following method: fumed silica (with a specific surface area of 150 m 2 / g) and 3-aminopropyltriethoxysilane are added to N,N-dimethylformamide in a mass ratio of 1:1 and ultrasonically dispersed uniformly, and the mixture is heated to 100°C, reacted for 12 hours, filtered, washed, and dried in vacuo to obtain aminosilane coupling agent modified silica; aminosilane coupling agent modified silica, acryloyl chloride and triethylamine are added to toluene in a mass ratio of 1:0.02:0.5, stirred and refluxed for 4 hours, filtered, washed, and dried to obtain alkenyl modified silica; alkenyl modified silica and potassium chloroplatinate are added to acetone in a mass ratio of 1:0.05, stirred and refluxed for 48 hours under nitrogen protection, filtered, washed, and dried in vacuo to obtain a loaded Pt complex catalyst with a Pt content of 0.5wt%.
[0049] The preparation method of the above-mentioned transparent silicone adhesive is specifically as follows:
[0050] Under room temperature, the formulated amount of vinyl silicone oil, vinyl MQ silicone resin, hydrogenated silicone oil, tackifying resin and 3-methyl-1-hexynyl-3-ol are sequentially added into a blender and stirred in vacuum for 1 hour to obtain a premix; after the premix is cooled to 30° C., the formulated amount of loaded Pt complex catalyst is added and stirred in vacuum for 30 minutes to obtain the transparent silicone adhesive.
[0051] Comparative Example 1
[0052] A transparent silicone adhesive comprises the following raw materials in parts by weight: 100 parts of vinyl silicone oil, 20 parts of vinyl MQ silicone resin, 15 parts of hydrogenated silicone oil, 1 part of a supported Pt complex catalyst, and 0.1 part of 3,5-dimethyl-1-hexyn-3-ol;
[0053] The viscosity of vinyl silicone oil at 25°C is 1000cps, and the vinyl content is 0.8wt%; the hydrogen content of hydrogen-containing silicone oil is 0.3wt%; the viscosity of vinyl MQ silicone resin at 25°C is 8000cps, and the vinyl content is 0.96wt%;
[0054] The supported Pt complex catalyst was prepared by the following method: fumed silica (with a specific surface area of 150 m 2 / g) and 3-aminopropyltriethoxysilane are added to N,N-dimethylformamide in a mass ratio of 1:1 and ultrasonically dispersed uniformly, and the mixture is heated to 100°C, reacted for 12 hours, filtered, washed, and dried in vacuo to obtain aminosilane coupling agent modified silica; aminosilane coupling agent modified silica, acryloyl chloride and triethylamine are added to toluene in a mass ratio of 1:0.02:0.5, stirred and refluxed for 4 hours, filtered, washed, and dried to obtain alkenyl modified silica; alkenyl modified silica and potassium chloroplatinate are added to acetone in a mass ratio of 1:0.05, stirred and refluxed for 48 hours under nitrogen protection, filtered, washed, and dried in vacuo to obtain a loaded Pt complex catalyst with a Pt content of 0.5wt%.
[0055] The preparation method of the above-mentioned transparent silicone adhesive is specifically as follows:
[0056] Under room temperature, the formulated amount of vinyl silicone oil, vinyl MQ silicone resin, hydrogen-containing silicone oil and 3,5-dimethyl-1-hexyn-3-ol are sequentially added into a blender and stirred in vacuum for 1 hour to obtain a premix; after the premix is cooled to 30° C., the formulated amount of loaded Pt complex catalyst is added and stirred in vacuum for 30 minutes to obtain the transparent silicone adhesive.
[0057] Comparative Example 2
[0058] A transparent silicone adhesive comprises the following raw materials in parts by weight: 100 parts of vinyl silicone oil, 20 parts of vinyl MQ silicone resin, 15 parts of hydrogenated silicone oil, 10 parts of tackifying resin, 1 part of supported Pt complex catalyst, and 0.1 part of 3,5-dimethyl-1-hexyn-3-ol;
[0059] The viscosity of vinyl silicone oil at 25°C is 1000cps, and the vinyl content is 0.8wt%; the hydrogen content of hydrogen-containing silicone oil is 0.3wt%; the viscosity of vinyl MQ silicone resin at 25°C is 8000cps, and the vinyl content is 0.96wt%;
[0060] The tackifying resin is prepared by the following method: alkenyl succinic anhydride, hydroxyethyl acrylate and azobisisobutyronitrile are added into xylene in a mass ratio of 7.25:21.75:0.3, and ultrasonically dissolved completely, heated to 75° C. and reacted for 12 hours, and cooled and removed xylene to obtain the tackifying resin;
[0061] The supported Pt complex catalyst was prepared by the following method: fumed silica (with a specific surface area of 150 m 2 / g) and 3-aminopropyltriethoxysilane are added to N,N-dimethylformamide in a mass ratio of 1:1 and ultrasonically dispersed uniformly, and the mixture is heated to 100°C, reacted for 12 hours, filtered, washed, and dried in vacuo to obtain aminosilane coupling agent modified silica; aminosilane coupling agent modified silica, acryloyl chloride and triethylamine are added to toluene in a mass ratio of 1:0.02:0.5, stirred and refluxed for 4 hours, filtered, washed, and dried to obtain alkenyl modified silica; alkenyl modified silica and potassium chloroplatinate are added to acetone in a mass ratio of 1:0.05, stirred and refluxed for 48 hours under nitrogen protection, filtered, washed, and dried in vacuo to obtain a loaded Pt complex catalyst with a Pt content of 0.5wt%.
[0062] The preparation method of the above-mentioned transparent silicone adhesive is specifically as follows:
[0063] Under room temperature, the formulated amount of vinyl silicone oil, vinyl MQ silicone resin, hydrogenated silicone oil, tackifying resin and 3,5-dimethyl-1-hexyn-3-ol are sequentially added into a blender and stirred in vacuum for 1 hour to obtain a premix; after the premix is cooled to 30° C., the formulated amount of loaded Pt complex catalyst is added and stirred in vacuum for 30 minutes to obtain the transparent silicone adhesive.
[0064] Comparative Example 3
[0065] A transparent silicone adhesive comprises the following raw materials in parts by weight: 100 parts of vinyl silicone oil, 20 parts of vinyl MQ silicone resin, 15 parts of hydrogen-containing silicone oil, 10 parts of tackifying resin, 1 part of Custer catalyst (Betley, platinum content of 5000 ppm), and 0.1 part of 3,5-dimethyl-1-hexyn-3-ol;
[0066] The viscosity of vinyl silicone oil at 25°C is 1000cps, and the vinyl content is 0.8wt%; the hydrogen content of hydrogen-containing silicone oil is 0.3wt%; the viscosity of vinyl MQ silicone resin at 25°C is 8000cps, and the vinyl content is 0.96wt%;
[0067] The tackifying resin is prepared by the following method: alkenyl succinic anhydride, hydroxyethyl acrylate, methacryloyloxypropyl tris(trimethylsiloxy)silane and azobisisobutyronitrile are added into xylene in a mass ratio of 1:3:25:0.3 and ultrasonically dissolved completely, heated to 75°C and reacted for 12 hours, cooled and xylene removed to obtain the tackifying resin.
[0068] The preparation method of the above-mentioned transparent silicone adhesive is specifically as follows:
[0069] Under room temperature, the formulated amount of vinyl silicone oil, vinyl MQ silicone resin, hydrogenated silicone oil, tackifying resin and 3,5-dimethyl-1-hexyn-3-ol are sequentially added into a blender and stirred in vacuum for 1 hour to obtain a premix; after the premix is cooled to 30° C., the formulated amount of Custer catalyst is added and stirred in vacuum for 30 minutes to obtain the transparent silicone adhesive.
[0070] Performance Test:
[0071] The transparent silicone adhesives obtained in the above examples and comparative examples were subjected to the following performance tests. The results are shown in Table 1 below.
[0072] The tensile strength / elongation at break is measured according to standard GB / T528-2009;
[0073] The light transmittance is measured according to the standard GB / T2410-2008, specifically the light transmittance of a 0.45mm thick film at 400-700nm;
[0074] The bonding strength is measured according to the standard ASTM D1002, specifically, a 5mm×5mm bonding area is marked on a 2mm thick glass sheet, and the transparent silicone adhesive is evenly coated thereon, with a film thickness of 0.2mm, and then bonded to a 2mm thick stainless steel sheet, and fully cured at 130°C for 30min to obtain a test sample, and the shear strength is measured at a peeling speed of 50mm / min;
[0075] The moisture and heat resistance performance is measured by placing the above test samples in a high temperature and high humidity oven, leaving them at 85°C and 85% relative humidity for 1000 hours, and then measuring their shear strength at a peeling speed of 50mm / min.
[0076] Table 1 Performance test results of the yellowing-resistant adhesives described in Examples and Comparative Examples
[0077]
[0078] It can be seen from the above table that the transparent silicone adhesive of the present invention has excellent mechanical, bonding and aging resistance properties.
[0079] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A transparent silicone adhesive, characterized in that: The invention comprises the following raw materials in parts by weight: 100 parts of vinyl silicone oil, 10-30 parts of reinforcing resin, 5-25 parts of hydrogen-containing silicone oil, 5-20 parts of tackifying resin, 0.1-5 parts of loaded Pt complex catalyst, 0.01-0.5 parts of inhibitor and 0-30 parts of auxiliary agent.
2. The transparent silicone adhesive according to claim 1, characterized in that: The viscosity of the vinyl silicone oil is 500-50000 cps, and the vinyl content is 0.1-5 wt %.
3. The transparent silicone adhesive according to claim 1 or 2, characterized in that: The reinforcing resin is vinyl MQ silicone resin or polyvinyl silicone oil; Preferably, the reinforcing resin has a viscosity of 1000-20000 cps and a vinyl content of 0.5-3 wt%.
4. The transparent silicone adhesive according to any one of claims 1 to 3, characterized in that: The hydrogen-containing silicone oil is a side-chain hydrogen-containing silicone oil and / or a terminal hydrogen-containing silicone oil, and its hydrogen content is 0.1-2 wt %.
5. The transparent silicone adhesive according to any one of claims 1 to 4, characterized in that: The structure of the tackifying resin is as follows: Among them, x, y, z are all greater than 0; Preferably, the tackifying resin is obtained by copolymerizing alkenyl succinic anhydride, hydroxyethyl acrylate and methacryloxypropyl tris(trimethylsiloxy)silane in a mass ratio of 1:1-5:20-30.
6. The transparent silicone adhesive according to any one of claims 1 to 5, characterized in that: The supported Pt complex catalyst is a silica-supported platinum-olefin complex; Preferably, the silica-supported platinum-olefin complex is obtained by modifying silica with an aminosilane coupling agent, condensing with acryloyl chloride, and then complexing with potassium chloroplatinate.
7. The transparent silicone adhesive according to any one of claims 1 to 6, characterized in that: The inhibitor is at least one of an alkynol compound, a maleate compound or a fumarate compound; Preferably, the alkynol compound is at least one of 1-ethynyl-1-cyclohexanol, 3-methyl-1-hexynyl-3-ol, 2-methyl-3-butynyl-2-ol or 3,5-dimethyl-1-hexynyl-3-ol.
8. The transparent silicone adhesive according to any one of claims 1 to 7, characterized in that: The auxiliary agent is at least one of a accelerator, a silane coupling agent, a thixotropic agent or an antioxidant.
9. A method for preparing the transparent silicone adhesive according to any one of claims 1 to 8, characterized in that: include: The vinyl silicone oil, reinforcing resin, hydrogen-containing silicone oil, tackifying resin, inhibitor and auxiliary agent are vacuum stirred to obtain a premix; The loaded Pt complex catalyst and the premix are vacuum stirred to obtain the organosilicon transparent adhesive.
10. Use of the transparent silicone adhesive according to any one of claims 1 to 8 in photovoltaic cell packaging.
Citation Information
Cited By
Single-component high-strength fast-curing adhesive and preparation method thereof
CN121343503A