Method for recycling valuable metal based on converter steel slag

By designing the coordinated smelting of converter steel slag and tungsten-molybdate slag in the metallurgical industry, and using silicon reducing agents, the problems of low recycling efficiency and environmental pollution in the existing technology have been solved, and efficient and environmentally friendly resource utilization has been achieved.

CN119040642AActive Publication Date: 2024-11-29XIAMEN UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411179803.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-29
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The prior art has low recycling efficiency of converter steel slag and tungsten-molybdate slag in the metallurgical industry, and a large number of additives are required during the ignition smelting process, resulting in environmental pollution and high costs.

Method used

By designing the mixing ratio of converter steel slag and tungsten-molybdate slag, the liquid phase temperature of the mixture is between 1100-1300℃, and using silicon as a reducing agent to perform coordinated smelting to reduce flux use and carbon emissions, realizing valuable metals efficient recycling.

Benefits of technology

It significantly improves the resource utilization rate of valuable metals, simplifies the recycling process, reduces environmental pollution and treatment costs, and is suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040642A_ABST
    Figure CN119040642A_ABST
Patent Text Reader

Abstract

The invention provides a method for recovering valuable metals based on converter steel slag, which comprises the following steps: S1, designing the mixing ratio of the converter steel slag and tungsten-molybdenum acid slag according to the components of the converter steel slag and tungsten-molybdenum acid slag, and enabling the liquid phase temperature of the mixture to be 1100-1300 DEG C; s2, after the mixing proportion of the converter steel slag and the tungsten-molybdenum acid slag is determined, the adding amount of a silicon reducing agent is determined according to the total amount of oxygen elements in highest oxides of valuable metals in a mixture of the converter steel slag and the tungsten-molybdenum acid slag; s3, according to the determined adding proportion of the converter steel slag, the tungsten-molybdenum acid slag and the silicon reducing agent, uniformly mixing the converter steel slag, the tungsten-molybdenum acid slag and the silicon reducing agent to obtain a mixture I; and S4, putting the mixture I into a crucible, heating in an inert atmosphere to completely melt a sample, then carrying out constant-temperature treatment to obtain a stable melt, and after smelting is finished and the melt is cooled to the room temperature, separating metal from a slag phase. Through collaborative smelting of the converter steel slag and the tungsten-molybdenum acid slag, valuable metals in the converter steel slag and the tungsten-molybdenum acid slag can be effectively recovered, and the method has remarkable environmental and economic benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of valuable metal recovery, and in particular to a method for recovering valuable metals based on converter slag. Background Art

[0002] Converter slag and tungsten-molybdenum acid slag are two important industrial solid wastes generated in the process of steel and non-ferrous metal smelting. At present, my country's steel industry produces about 420 million tons of smelting waste slag each year, and the non-ferrous metal industry produces 128 million tons of waste slag each year. However, the resource utilization rate of solid waste in these two industries is generally low. The resource utilization rate of converter slag is less than 30%, and low-grade tungsten-molybdenum acid slag is stored in large quantities within the enterprise, resulting in a large amount of metal resources Waste. Therefore, the efficient recovery of valuable metal resources in metallurgical solid waste is a key issue that needs to be urgently solved for the sustainable development of the metallurgical industry.

[0003] At present, the steel industry mainly uses physical methods and pyrometallurgical smelting methods to recover valuable metals from converter slag. Although the traditional physical method is pollution-free during the recovery process, the recovery efficiency of valuable metals is low. Pyrometallurgical smelting mainly uses carbon as a reducing agent and requires the addition of additional additives. This process will produce a large amount of carbon emissions. Tungsten-molybdenum acid slag is a secondary waste slag after wet treatment in the non-ferrous metal industry. It has a complex composition and low grade of valuable metals. However, its pyrometallurgical smelting recovery process usually requires the addition of a large amount of additives, which increases the recovery cost. Therefore, there is an urgent need for a new technical method that can effectively and synergistically recover the valuable metals in converter slag and tungsten-molybdenum acid slag to achieve efficient resource utilization and environmental protection. Summary of the invention

[0004] In view of the above problems, the purpose of the present invention is to provide a method for recovering valuable metals based on converter slag. Through the coordinated smelting of converter slag and tungstomolybdic acid slag, the valuable metals therein can be effectively recovered, while reducing environmental pollution and processing costs, and having significant environmental and economic benefits.

[0005] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0006] A method for recovering valuable metals based on converter slag comprises the following steps:

[0007] S1: Design the mixing ratio of the two waste slags according to the composition of converter steel slag and tungsten-molybdenum acid slag, so that the liquid phase temperature of the mixture is between 1100-1300℃;

[0008] S2: After determining the mixing ratio of converter steel slag and tungsten-molybdic acid slag, determine the amount of silicon reducing agent to be added according to the total amount of oxygen element in the highest oxide of the valuable metal in the mixture of converter steel slag and tungsten-molybdic acid slag;

[0009] S3: according to the determined addition ratio of converter slag, tungsto-molybdic acid slag and silicon reducing agent, the three are uniformly mixed to obtain a mixture I;

[0010] S4: Mixture I is placed in a crucible, and heated in an inert atmosphere to melt the sample completely, followed by a constant temperature treatment to obtain a stable melt. After the smelting is completed and cooled to room temperature, the metal and slag phases are separated.

[0011] Furthermore, the main components of the converter slag include SiO2, CaO, FeO / Fe2O3, Al2O3, MnO2, and P2O5; the main components of the tungstomolybdic acid slag include WO3, MoS2, CoO, Ta2O5, Nb2O5, NiO, CuO, SiO2, and Na2O.

[0012] Furthermore, S1 specifically includes the following steps:

[0013] The mass fraction of each oxide in converter slag and tungsto-molybdic acid slag was determined by X-ray fluorescence spectrometry.

[0014] According to the mass fractions of CaO, SiO2, Na2O and Al2O3 in the mixture formed by converter slag and tungsto-molybdic acid slag, find the corresponding component point in the CaO-Na2O-SiO2-Al2O3 multi-element phase diagram, and determine the temperature of the liquid phase region where it is located, that is, the temperature at which the mixed raw materials are completely melted to form a liquid phase;

[0015] The mass ratio of converter slag to tungsten-molybdate slag is adjusted so that the liquid phase temperature of the mixture is between 1100-1300℃.

[0016] Furthermore, the valuable metals in the mixture of converter steel slag and tungstomolybdic acid slag in S2 include W, Mo, Co, Ta, Nb, Ni, Cu, and Fe.

[0017] Furthermore, the molar ratio of the total amount of elemental silicon in the silicon reducing agent in S2 to the total amount of oxygen in the highest oxide of the valuable metal is 1:2.

[0018] Furthermore, the silicon reducing agent is selected from any one or more combinations of high-purity silicon powder, industrial silicon blocks, and photovoltaic silicon cutting powder.

[0019] Furthermore, the mixture I in S4 is heated to 1400-1500° C. in an inert atmosphere to melt all the samples.

[0020] Furthermore, after the sample in S4 was completely melted, it was kept warm for 2 h to obtain a stable melt.

[0021] Furthermore, the crucible is a ceramic crucible such as corundum, magnesium oxide ceramics, etc.

[0022] Furthermore, the inert atmosphere in S4 is an argon atmosphere.

[0023] The beneficial effects of the present invention are as follows:

[0024] 1) The present invention utilizes components such as CaO, SiO2, and MgO in steel slag, and reduces the use of other fluxes through component regulation. In addition, the components in steel slag are utilized to capture low-grade strategic metals in tungsten-molybdenum acid slag, thereby achieving efficient recovery of all elements. This method reduces the use of flux, reduces the use of additives in the pyrometallurgical smelting process, reduces corresponding environmental pollution problems, and especially reduces carbon emissions. This method simplifies the solid waste recovery process by synergistically treating solid wastes from two metallurgical industries, is easy to operate, and is suitable for large-scale industrial applications. The present invention provides a new technical path for sustainable development for the metallurgical industry, significantly improves the resource utilization rate of converter steel slag and tungsten-molybdenum acid slag, and has important environmental and economic benefits.

[0025] 2) Both converter slag and tungsten-molybdic acid slag have the characteristics of high melting points. Direct smelting of the two requires high temperature and high energy consumption, which is difficult to achieve in the actual production process. The present invention fully utilizes the useful components in the two waste slags through the coordinated smelting of converter slag and tungsten-molybdic acid slag, realizes efficient recovery of valuable metals, reduces the use of external flux, and improves the resource utilization rate of converter slag and tungsten-molybdic acid slag.

[0026] 3) After the Fe, Mn, P and other elements in the steel slag are reduced, they form larger Fe-Mn-P alloy particles. These alloy particles can react with the scattered valuable metals (W, Mo, Co, Ta, Nb, Ni, Cu, Fe) in the tungsten-molybdenum acid slag to capture these scattered valuable metals and promote their enrichment; in addition, the steel slag oxides CaO, SiO2 and SiO2, Na2O and other oxides in the tungsten-molybdenum acid slag can jointly regulate the melting temperature of the slag phase. By matching the tungsten-molybdenum acid slag, a silicate slag phase CaO-Na2O-SiO2-Al2O3 with a lower melting temperature can be obtained, which provides a liquid phase with better fluidity for the mass transfer process of the alloy phase and synergistically promotes the enrichment effect of the alloy.

[0027] 4) The present invention utilizes silicon as a reducing agent to achieve efficient reduction of valuable metal oxides in converter slag and tungsto-molybdic acid slag, thereby reducing carbon emissions.

[0028] 5) The present invention utilizes the composition characteristics of converter steel slag and tungsto-molybdic acid slag to regulate the composition, does not require complicated pre-treatment steps and special equipment, simplifies the recycling process, and is conducive to large-scale industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 It is the liquid phase temperature of the mixed raw material of converter steel slag and tungsten-molybdic acid slag and the recovery rate of valuable metals in each embodiment; wherein, Figure (a) is the liquid phase temperature of the mixed raw material of converter steel slag and tungsten-molybdic acid slag in each embodiment, and Figure (b) is the recovery rate of valuable metals in each embodiment.

[0031] Figure 2 This is the EPMA element distribution analysis diagram of the slag-metal interface of the smelting sample in Example 4.

[0032] Figure 3 This is a physical picture of the smelting sample in Example 4.

[0033] Figure 4 This is the EPMA element distribution analysis diagram of the smelted sample alloy sample in Example 4. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0035] This embodiment provides a method for recovering valuable metals based on converter slag, comprising:

[0036] S1. Raw material ratio design: According to the composition of converter steel slag and tungsten-molybdenum acid slag, the mixing ratio of the two waste slags is designed so that the liquid phase temperature of the mixture is between 1100-1300℃, which specifically includes the following steps:

[0037] The mass fraction of each oxide in converter slag and tungsten-molybdic acid slag is determined by X-ray fluorescence spectrometry (XRF); according to the mass fractions of CaO, SiO2, Na2O and Al2O3 in the mixture formed by converter slag and tungsten-molybdic acid slag, the corresponding component point is found in the CaO-Na2O-SiO2-Al2O3 multivariate phase diagram, and the temperature of the liquid phase region where it is located (i.e. the liquid phase temperature of the mixed raw materials) is determined; the mass ratio of converter slag and tungsten-molybdic acid slag is adjusted so that the liquid phase temperature of the mixture is between 1100-1300°C.

[0038] Specifically, the main components of converter slag in this embodiment are: SiO2 (10-20%), CaO (30-40%), FeO / Fe2O3 (30-40%), Al2O3 (<5%), MgO (2-10%), MnO2 (1-8%), P2O5 (<5%), etc.

[0039] The main components of tungsten-molybdic acid slag are: MoS2 (3-8%), WO3 (0-6%), CoO (2-10%), Ta2O5 (0-3%), Nb2O5 (0-3%), NiO (0-5%), CuO (0-10%), SiO2 (10-30%), Na2O (0-10%), etc.

[0040] The liquidus temperature of converter slag and tungsten-molybdenum acid slag at different ratios is as follows:

[0041] 100g converter slag: CaO: 35-40g, SiO2: 10-15g, Al2O3: 0-5g, the corresponding liquidus temperature is 2200-2300℃.

[0042] 100g tungsten-molybdic acid slag: SiO2: 30-35%, Al2O3: 0-5g, Na2O: 10-15g, the corresponding liquidus temperature is 1650-1700℃.

[0043] 100g converter slag + 100g tungsten-molybdic acid slag: CaO: 40-45g, SiO2: 70-75g, Na2O: 10-15g, Al2O3: 0-5g, the corresponding liquidus temperature is 1270-1300℃.

[0044] 50g converter slag + 100g tungsten-molybdic acid slag: CaO: 20-25g, SiO2: 55-60g, Na2O: 15-20g, Al2O3: 0-5g, the corresponding liquidus temperature is 1200-1230℃.

[0045] 50g converter slag + 150g tungsten-molybdic acid slag: CaO: 20-25g, SiO2: 85-95g, Na2O: 20-25g, Al2O3: 5-10g, the corresponding liquidus temperature is 1150-1180℃.

[0046] 50g converter slag + 200g tungsto-molybdic acid slag: CaO: 20-25g, SiO2: 100-105g, Na2O: 30-35g, Al2O3: 5-10g, the corresponding liquidus temperature is 1100-1130℃.

[0047] From the above data, it can be seen that if tungsten-molybdenum acid slag or converter steel slag is smelted separately, it needs to be heated to 1650℃ and 2200℃ respectively to be completely melted, which increases the energy consumption in actual smelting and makes it difficult to achieve. By combining the two components, the melting temperature can be greatly reduced. In addition, it can be found that as the mass of tungsten-molybdenum acid slag increases, the liquid phase temperature of the mixed raw materials gradually decreases.

[0048] The main reaction equation involved in the present invention is: Fe2O3+Si=Fe+SiO2. When the reaction temperature is increased to above 1400°C, the reaction is changed from solid-solid reaction to solid-liquid reaction, which can greatly improve the reaction rate. If the oxides CaO, SiO2, Al2O3 and Na2O can form a low melting point silicate phase CaO-SiO2-Al2O3-Na2O at below 1400°C, more liquid phase can be provided for the reduction reaction, which is beneficial to the transfer of reactants and heat in the reaction process and improves the reaction rate.

[0049] The present invention adjusts the liquid phase temperature of the mixture (converter slag + tungsten-molybdic acid slag) to between 1100-1300°C, so that the mixture of converter slag and tungsten-molybdic acid slag can form an appropriate liquid phase, which helps to improve the silicon thermal reduction reaction rate and mixing uniformity. When the liquid phase temperature of the mixture is too high, the energy consumption cost will increase, and the high temperature will also accelerate the loss of equipment and refractory materials (the maximum experimental temperature of commonly used alumina materials is 1700°C, and magnesium oxide crucibles are prone to cracking at 1700°C), increasing the cost of maintenance and replacement. Therefore, in the present invention, it is preferred to adjust the liquid phase temperature of the mixture (converter slag + tungsten-molybdic acid slag) to between 1100-1300°C.

[0050] S2: After determining the mixing ratio of converter slag and tungsten-molybdic acid slag, determine the amount of silicon reducing agent added according to the total amount of oxygen in the highest oxide of the valuable metals in the mixture of converter slag and tungsten-molybdic acid slag. The valuable metals (including W, Mo, Co, Ta, Nb, Ni, Cu, Fe) in the mixture of converter slag and tungsten-molybdic acid slag mainly exist in the form of oxides. In this step, when calculating the proportion of silicon reducing agent addition, it is assumed that all valuable metals exist in the form of the highest oxide (i.e., WO3, MoO3, Co2O3, Ta2O5, Nb2O5, NiO, CuO, Fe2O3), and the total amount of oxygen in the highest oxide of the valuable metal is calculated. The theoretical maximum amount of silicon addition required is calculated through the silicon thermal reaction equation; MeOx+x / 2Si=Me+x / 2SiO2 (where MeOx=WO3, MoO3, Co2O3, Ta2O5, Nb2O5, NiO, CuO, Fe2O3); the molar ratio of the total amount of elemental silicon in the silicon reducing agent to the total amount of oxygen in the highest oxide of the valuable metal is 1:2. Among them, the silicon reducing agent can be selected from high-purity silicon powder, industrial silicon blocks, photovoltaic silicon cutting powder, etc.

[0051] S3: according to the determined addition ratio of converter slag, tungsto-molybdic acid slag and silicon reducing agent, the three are uniformly mixed to ensure that the mixture is evenly distributed to obtain a mixture I;

[0052] S4: Place the mixture I into a crucible (ceramic crucible such as corundum, magnesium oxide, etc.), and heat it to 1400-1500°C in an inert atmosphere to melt all the samples; during heating, the heating temperature is generally 100-200°C higher than the complete melting temperature of the mixture (i.e., the liquidus temperature of the mixture) to improve the reaction efficiency and the final recovery rate of valuable metals.

[0053] When the sample is completely melted, it is kept warm for 2 hours to obtain a stable melt. At this time, the alloy of the reduced valuable metals is deposited at the bottom of the melt. After the smelting is completed and cooled to room temperature, the metal and slag phases are separated to obtain a metal phase containing valuable metals and a harmless slag phase. The mixture can be smelted using heating equipment such as a tubular furnace and an induction melting furnace.

[0054] Example 1

[0055] The method for recovering valuable metals from converter slag in this embodiment includes the following steps:

[0056] 1) 50 g of converter slag (SiO2 content: 10-20%, CaO content: 30-40%, FeO / Fe2O3 content: 30-40%, Al2O3 content: <5%, MgO content: 2-10%, MnO2 content: 1-8%, P2O5 content: <5%), 50 g of tungsto-molybdic acid slag (MoS2 content: 3-8%, WO3 content: 0-6%, CoO content: 2-10%, Ta2O5 content: 0-3%, Nb2O5 content: 0-3%, NiO content 0-5%, CuO content: 0-10%, SiO2 content: 10-30%, Na2O content: 0-10%) and 10 g of silicon powder were uniformly mixed to ensure that the mixture was evenly distributed to obtain a mixture I;

[0057] 2) Place the mixed material I into a crucible (a ceramic crucible such as corundum or magnesium oxide), introduce argon gas into the tubular furnace, and adjust the temperature control program to raise the temperature to 1500° C. to melt all the samples.

[0058] 3) When the sample is completely melted, keep it warm for 2 hours to obtain a stable melt. At this time, the alloy of the reduced valuable metals is deposited at the bottom of the melt. After the smelting is completed and cooled to room temperature, the metal and slag phases are separated to obtain a metal phase containing valuable metals such as Fe, Mn, W, Mo, Ni, Co, and Cu and a harmless slag phase.

[0059] Example 2

[0060] The method for recovering valuable metals based on converter steel slag provided in this embodiment is basically the same as that in Example 1, except that, in this embodiment, 50 g of converter steel slag, 100 g of tungsto-molybdic acid slag and 15 g of silicon powder are uniformly mixed to obtain a mixture I.

[0061] Example 3

[0062] The method for recovering valuable metals based on converter steel slag provided in this embodiment is basically the same as that in Example 1, except that, in this embodiment, 50 g of converter steel slag, 150 g of tungsto-molybdic acid slag and 20 g of silicon powder are uniformly mixed to obtain a mixture I.

[0063] Example 4

[0064] The method for recovering valuable metals based on converter steel slag provided in this embodiment is basically the same as that in Example 1, except that, in this embodiment, 50 g of converter steel slag, 200 g of tungsto-molybdic acid slag and 25 g of silicon powder are uniformly mixed to obtain a mixture I.

[0065] Effect test

[0066] like Figure 1 As shown in (a), adding tungsten-molybdic acid slag can reduce the melting temperature of converter slag, and as the amount of tungsten-molybdic acid slag added increases, the melting temperature gradually decreases. The recovery rate of valuable metals in the alloy sample finally obtained is shown in Figure 1 As shown in (b), with the increase of the addition ratio of tungsten-molybdate slag, the recovery rate of valuable metals such as Fe, W, Mo, and Cu in the alloy gradually increases. The main reasons are as follows:

[0067] 1) As the amount of tungsten-molybdic acid slag added increases, the overall melting temperature of the mixed raw materials gradually decreases. At 1500°C, the more tungsten-molybdic acid slag is added, the earlier the reaction system melts, the melt fluidity improves, and the recovery of valuable metals is promoted. 2) The Fe and Mn elements in the steel slag can capture W, Mo, Cu and other elements in the tungsten-molybdic acid slag. As the amount of tungsten-molybdic acid slag added increases, there are more W, Mo, and Cu elements in the system, so they eventually react with the Fe and Mn elements to alloy and capture, resulting in an increase in the recovery rate.

[0068] The steel slag in the present invention has an alloy capture effect: Fe element has a good binding force with valuable metals such as W, Mo, Ta, Nb, Co, Ni, etc. After being reduced, Fe in the steel slag can be used as an alloy capture agent, combining with other valuable metals and alloying, thereby improving the enrichment rate of various valuable metals in the smelting process. Figure 2As shown in FIG. 1 , the element distribution analysis of the sample obtained in Example 4 shows that the main components of the alloy droplets are Fe, Cu, and Mo, which confirms that during the smelting process, the Fe element reacts with the Mo and Cu elements to form Fe-Cu-Mo alloy droplets. During the smelting process, these small alloy droplets migrate from the slag phase to the alloy phase and form alloy ingots (such as the attached Figure 3 To achieve the recovery of valuable metals.

[0069] See attached Figure 4 As shown, the elements of the alloy finally obtained in Example 4 were analyzed separately and it was found that the main phase components of the alloy ingot were valuable metals Fe, Cu, Mo and P, which confirmed that the method of the present invention can achieve the simultaneous enrichment and recovery of multiple valuable metals.

[0070] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for recovering valuable metals based on converter slag, characterized in that: The steps include: S1: Design the mixing ratio of the two waste slags according to the composition of converter steel slag and tungsten-molybdenum acid slag, so that the liquid phase temperature of the mixture is between 1100-1300℃; S2: After determining the mixing ratio of converter steel slag and tungsten-molybdic acid slag, determine the amount of silicon reducing agent to be added according to the total amount of oxygen element in the highest oxide of the valuable metal in the mixture of converter steel slag and tungsten-molybdic acid slag; S3: according to the determined addition ratio of converter steel slag, tungsto-molybdic acid slag and silicon reducing agent, the three are uniformly mixed to obtain a mixture I; S4: Mixture I is placed in a crucible, and heated in an inert atmosphere to melt the sample completely, followed by a constant temperature treatment to obtain a stable melt. After the smelting is completed and cooled to room temperature, the metal and slag phases are separated.

2. The method for recovering valuable metals from converter slag according to claim 1, characterized in that: The main components of the converter slag include SiO2, CaO, FeO / Fe2O3, Al2O3, MnO2, and P2O5; the main components of the tungstomolybdic acid slag include WO3, MoS2, CoO, Ta2O5, Nb2O5, NiO, CuO, SiO2, and Na2O.

3. The method for recovering valuable metals from converter slag according to claim 1, characterized in that: S1 specifically includes the following steps: The mass fraction of each oxide in converter slag and tungsto-molybdic acid slag was determined by X-ray fluorescence spectrometry. According to the mass fractions of CaO, SiO2, Na2O and Al2O3 in the mixture formed by converter slag and tungsto-molybdic acid slag, find the corresponding component point in the CaO-Na2O-SiO2-Al2O3 multi-element phase diagram, and determine the temperature of the liquid phase region where it is located, that is, the temperature at which the mixed raw materials are completely melted to form a liquid phase; The mass ratio of converter slag to tungsten-molybdate slag is adjusted so that the liquid phase temperature of the mixture is between 1100-1300℃.

4. The method for recovering valuable metals from converter slag according to claim 1, characterized in that: The valuable metals in the mixture of converter steel slag and tungstomolybdic acid slag described in S2 include W, Mo, Co, Ta, Nb, Ni, Cu, and Fe.

5. The method for recovering valuable metals from converter slag according to claim 4, characterized in that: The molar ratio of the total amount of elemental silicon in the silicon reducing agent in S2 to the total amount of oxygen in the highest oxide of the valuable metal is 1:

2.

6. The method for recovering valuable metals from converter slag according to claim 1, characterized in that: The silicon reducing agent is selected from any one or more combinations of high-purity silicon powder, industrial silicon blocks, and photovoltaic silicon cutting powder.

7. The method for recovering valuable metals from converter slag according to claim 1, characterized in that: The mixture I in S4 is heated to 1400-1500°C in an inert atmosphere to melt the entire sample.

8. The method for recovering valuable metals from converter slag according to claim 1, characterized in that: After the sample in S4 is completely melted, it is kept warm for 2 h to obtain a stable melt.

9. The method for recovering valuable metals based on converter slag according to claim 1, characterized in that: The crucible is a corundum or magnesium oxide ceramic crucible.

10. The method for recovering valuable metals from converter slag according to claim 1, characterized in that: The inert atmosphere in S4 is argon atmosphere.

Citation Information

Patent Citations

  • Method for determining content of lanthanum, cerium and barium in steel slag by X-ray fluorescent spectrometry

    CN108508050A

  • Method for cooperatively recycling tungsten slag and multi-element iron-rich slag

    CN111440953A

  • Method for recovering valuable metals in waste tungsten slag

    CN117778724A

  • Method of production of doped alloy containing refractory metals tungsten and molybdenum by technology of liquid-phase reduction

    RU2135611C1

  • Process and plant for SLAG treatment

    WO2024127339A1