Method for strengthening chemical oxidation of arsenopyrite

By adding pyrite to the chemical oxidation system of arsenic pyrite, using its oxidative acid production and Fe/As molar ratio regulation and the generation of reactive oxygen radicals, the problem of reducing gold recovery caused by the formation of passivation layer is solved, and the problem of reducing gold recovery is achieved. High efficient leaching of arsenic and high gold recovery in arsenic pyrite.

CN119040660AActive Publication Date: 2024-11-29NORTHEASTERN UNIV CHINA
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411168297.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

During the chemical oxidation process of arsenic pyrite, due to the different dissolution rates of Fe, As, and S elements, a passivation layer will be formed, hindering further oxidation and dissolution, resulting in a decrease in the secondary wrapping and recovery of gold.

Method used

Add pyrite to the chemical oxidation system of arsenic pyrite, and use its oxidative acid production characteristics to reduce the pH of the system, so that the precipitation of iron hydroxide in the passivation layer is converted to iron arsenate, and reduce arsenic by increasing the Fe/As molar ratio The stability of iron acid is used to activate the small molecule environmental medium to generate reactive oxygen free radicals by using sulfur defect sites on the surface of pyrite to strengthen the oxidation of arsenic pyrite.

Benefits of technology

The leaching rate of arsenic in arsenic pyrite is significantly improved, and the recovery rate of gold is increased by nearly 3 times. The process is simple, the conditions are mild, the operation is simple, and the stability and surface morphology of the passivation layer are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005008454850000011
    Figure HDA0005008454850000011
  • Figure HDA0005008454850000012
    Figure HDA0005008454850000012
  • Figure HDA0005008454850000021
    Figure HDA0005008454850000021
Patent Text Reader

Abstract

The invention discloses a method for strengthening chemical oxidation of arsenopyrite, which specifically comprises the following steps of: adding a certain amount of pyrite into an arsenopyrite chemical oxidation system, and reducing the pH value of the system by utilizing the characteristic that the pyrite is oxidized to produce acid, so that ferric hydroxide precipitate in a passivation layer is converted into ferric arsenate; pyrite is used as a Fe source, and the Fe / As molar ratio in the system is increased, so that the stability of iron arsenate in the passivation layer is reduced; fe (III) and Fe (II) on sulfur defect sites on the surface of the pyrite can activate a micromolecular environmental medium, and the generated reactive oxygen species (ROS) have oxidation capacity on the arsenopyrite, so that the purpose of strengthening the oxidation of the arsenopyrite is achieved; by means of the method, the leaching rate of arsenic in an arsenopyrite chemical oxidation system is increased by nearly three times to the maximum degree, the strengthening effect on arsenopyrite oxidation is remarkable, and meanwhile the method is simple in process, mild in condition and easy and convenient to operate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sulfide ore metallurgy, and in particular to a method for chemical oxidation of arsenopyrite. Background Art

[0002] Gold is an important and scarce strategic mineral resource in my country. However, with the continuous exploitation of gold mines, easy-to-select gold resources are gradually exhausted, and the proportion of difficult-to-process gold resources in the raw materials of the gold industry is gradually increasing. Arsenic-containing gold ore is one of the most difficult gold ores to process. The gold in this type of ore is mainly encapsulated in gold-bearing minerals such as arsenopyrite and pyrite in the form of microscopic gold, submicroscopic gold or lattice gold. It is difficult to dissociate it into monomers through fine grinding and ultrafine grinding. At the same time, due to the encapsulation characteristics of such gold-bearing minerals on fine gold, the competition, inhibition or gold robbery of harmful elements in the gold extraction process, it is difficult to effectively recover gold during subsequent cyanidation. Therefore, in order to recover the gold in this type of gold ore, pre-treatment technology is usually used to pre-oxidize and remove arsenic, so that the encapsulated gold is dissociated and exposed, thereby improving the gold recovery rate.

[0003] At present, common pre-oxidation technologies mainly include roasting oxidation, hot pressing oxidation, chemical oxidation, biological oxidation, etc. Among them, compared with other oxidation processes, chemical oxidation has the advantages of easy operation, strong adaptability, fast reaction speed, and short processing cycle. However, in the process of chemical oxidation of arsenopyrite, due to the different dissolution rates of Fe, As, and S elements, a passivation layer composed of elemental sulfur, metal oxides, etc. will be formed on the surface of the mineral, hindering the further oxidation and dissolution of arsenopyrite, and causing secondary encapsulation of gold, thereby reducing the recovery rate of gold in the subsequent gold leaching process. Therefore, the method of strengthening the chemical oxidation of arsenopyrite by reducing the formation of the passivation layer during the chemical oxidation of arsenopyrite is the key to promoting the advancement of chemical pre-oxidation technology for difficult-to-leach gold ores. Summary of the invention

[0004] In view of this, the present disclosure provides a method for strengthening the chemical oxidation of arsenopyrite, which solves the problem that a passivation layer is formed on the surface of the mineral during the current chemical oxidation process of arsenopyrite, thereby reducing the gold recovery rate.

[0005] The core mechanism of the method for strengthening the chemical oxidation of arsenopyrite is as follows: a certain amount of pyrite is added to the arsenopyrite chemical oxidation system, one purpose is to utilize the characteristic of pyrite oxidation to generate acid, reduce the pH of the system, and transform the iron hydroxide precipitation in the passivation layer into ferric arsenate; the second purpose is to use pyrite as an Fe source to increase the Fe / As molar ratio in the system to reduce the stability of the ferric arsenate in the passivation layer; the third purpose is that due to the presence of sulfur defect sites on the surface of pyrite, Fe(III) and Fe(II) on the sulfur defect sites can activate small molecular environmental media such as H2O and O2, and the generated reactive oxygen free radicals (ROS, Reactive Oxygen Species) have a strong oxidizing ability to arsenopyrite; therefore, adding pyrite to the arsenopyrite chemical oxidation system plays a strengthening role in the oxidation of arsenopyrite.

[0006] To achieve the above-mentioned object of the invention, the method for strengthening chemical oxidation of arsenopyrite comprises:

[0007] An arsenopyrite oxidation system is prepared, wherein the oxidation system comprises an arsenopyrite leaching sample and a pyrite leaching sample, wherein the mass ratio of the arsenopyrite leaching sample to the pyrite leaching sample is not greater than 1:1.

[0008] In the present disclosure and possible embodiments, the method for preparing arsenopyrite oxidation system comprises:

[0009] The arsenopyrite leaching sample and the pyrite leaching sample are placed in a basic salt solution, and the initial pH of the system is adjusted to 2-9 to obtain the oxidation system.

[0010] In the present disclosure and possible embodiments, the slurry concentration of the arsenopyrite leaching sample in the basic salt solution is 1-2%;

[0011] The slurry concentration of the pyrite leaching sample in the basic salt solution is 1-4%.

[0012] In the present disclosure and possible embodiments, the basic salt solution comprises: (NH4)2SO4 is 2 to 4 g / L, KCl is 0.1 to 0.3 g / L, K2HPO4 is 0.3 to 0.7 g / L, MgSO4·7H2O is 0.3 to 0.7 g / L, Ca(NO3)2 is 0.01 to 0.03 g / L, and the rest is deionized water.

[0013] In the present disclosure and possible embodiments, dilute sulfuric acid and potassium hydroxide solution are used to adjust the initial pH of the system, and the concentration of the dilute sulfuric acid is 3 to 8 mol / L; the concentration of the potassium hydroxide solution is 3 to 8 mol / L.

[0014] In the present disclosure and possible embodiments, the method further includes:

[0015] The arsenopyrite oxidation system is chemically oxidized to enhance the oxidation of the arsenopyrite.

[0016] In the present disclosure and possible embodiments, the method of chemically oxidizing the arsenopyrite oxidation system comprises:

[0017] The oxidation system is placed in an air bath constant temperature oscillator for oscillation oxidation for 18 to 25 days at 20 to 50° C. and 100 to 180 r / min.

[0018] In the present disclosure and possible embodiments, the particle size of the arsenopyrite leaching sample and the pyrite leaching sample is -0.03 to 0.05 mm.

[0019] In the present disclosure and possible embodiments, the method for preparing the arsenopyrite leaching sample comprises:

[0020] Take the arsenopyrite lump ore with purity meeting the requirements, crush it to -1~3mm, select and remove the gangue impurities, grind it to -0.1~0.3mm for sorting, and the obtained concentrate is ground to -0.03~0.05mm as the leaching sample.

[0021] In the present disclosure and possible embodiments, the method for preparing the pyrite leaching sample comprises:

[0022] Take pyrite lumps with purity that meets the requirements, crush them to -1~3mm, then pick out the gangue impurities, grind them to -0.1~0.3mm for sorting, and the obtained concentrate is ground to -0.03~0.05mm as leaching sample.

[0023] The present invention has the following beneficial effects:

[0024] (1) The present invention utilizes pyrite as an Fe source and adds it to a chemical oxidation system of arsenopyrite, thereby increasing the Fe / As molar ratio of the system and thereby increasing the content of hydrated iron oxide in the system; utilizing the strong adsorption characteristics of hydrated iron oxide, the agglomeration of ferric arsenate in the passivation layer is enhanced, thereby reducing the crystallization rate of ferric arsenate, reducing the volume and specific surface area of ​​ferric arsenate crystals, deteriorating the surface morphology of the passivation layer, and reducing the stability of the passivation layer, thereby increasing the leaching rate of arsenic in arsenopyrite.

[0025] (2) The present invention utilizes the characteristic of pyrite oxidation to generate acid, and adds pyrite to the arsenopyrite chemical oxidation system to achieve the purpose of lowering the pH of the system. When the pH of the system is lowered, the iron hydroxide in the passivation layer is converted into iron arsenate. Under the influence of the increase in the Fe / As molar ratio of the system, the iron arsenate in the passivation layer is further dissolved, and the arsenic ions are converted into AsO4 3-The arsenic in the arsenopyrite is released into the solution in the form of , thereby increasing the leaching rate of arsenic in arsenopyrite. Compared with the chemical oxidation system without adding pyrite, the leaching rate of arsenic in arsenopyrite is increased by nearly 3 times at most, with significant effects. At the same time, the method has simple process, mild conditions and easy operation.

[0026] (3) Since the SS bond on the surface of pyrite will break and lose a S atom under the action of mechanical external force or other forces, the unsaturated S(-I) produced can oxidize the adjacent Fe(II), and the formed Fe(III) can oxidize H2O to produce adsorbed ·OH, and O2 can directly obtain 2 electrons from the Fe(II) site on the surface of pyrite to produce H2O2. At the same time, ROS such as ·OH and H2O2 can serve as oxidants for arsenopyrite. Therefore, the present invention strengthens the oxidation of arsenopyrite by adding pyrite, thereby improving the leaching rate of arsenic in arsenopyrite.

[0027] (4) The pyrite used in the present invention has the characteristic of being symbiotic with arsenopyrite, and has the advantages of being easy to obtain, high in abundance, and low in cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The above and other objects, features and advantages of the present disclosure will become more apparent through the following description of the embodiments of the present disclosure with reference to the accompanying drawings, in which:

[0029] Figure 1 Fourier transform infrared spectra of the leached residue after 18 days of leaching in the chemical oxidation system of Comparative Example 1, Example 1 and Implementation Example 2;

[0030] Figure 2 The Fourier transform infrared spectra of the leached residue after 18 days of leaching in the chemical oxidation system of Comparative Example 2 and Example 3;

[0031] Figure 3 It is a curve diagram showing the change of As concentration in the leaching solution of the chemical oxidation system of Comparative Example 1, Example 1 and Implementation Example 2 over time;

[0032] Figure 4 It is a curve diagram showing the change of As concentration in the leaching solution of the chemical oxidation system of Comparative Example 2 and Example 3 over time;

[0033] Figure 5 It is a curve diagram showing the change of As concentration in the leaching solution of the chemical oxidation system of Comparative Example 3 and Example 4 over time;

[0034] Figure 6 The curve diagram of pH change over time of the chemical oxidation system of Comparative Example 3 and Example 4;

[0035] Figure 7 It is a curve diagram showing the change of the cumulative amount of ·OH in the chemical oxidation system leachate of Comparative Example 1, Example 1 and Implementation Example 2 over time;

[0036] Figure 8 The graph is a graph showing the change of the cumulative amount of ·OH in the leaching solution of the chemical oxidation system of Comparative Example 3 and Example 4 over time. DETAILED DESCRIPTION

[0037] The present disclosure is described below based on embodiments, but it is worth noting that the present disclosure is not limited to these embodiments. In the detailed description of the present disclosure below, some specific details are described in detail. However, for the parts that are not described in detail, those skilled in the art can also fully understand the present disclosure.

[0038] The inventors of the present application have found that adding paragenetic minerals to the arsenopyrite chemical oxidation system can achieve effective regulation of the passivation layer in the arsenopyrite chemical oxidation system. In particular, the addition of pyrite can reduce the pH of the system, induce the iron hydroxide precipitation in the passivation layer to transform into ferric arsenate precipitation, not only improve the Fe / As molar ratio of the system, enhance the agglomeration of ferric arsenate in the passivation layer, but also reduce its crystallization rate, reduce the volume and specific surface area of ​​ferric arsenate crystals, deteriorate the surface morphology of the passivation layer, and reduce the stability of the passivation layer. Further, studies have confirmed that Fe (II) and Fe (III) on the sulfur defect sites on the surface of pyrite can activate small molecule environmental media, and the generated ROS have strong oxidizing properties, can non-selectively oxidize variable valence metals, and affect the oxidation process of minerals. Therefore, the inventors of the present application achieve the enhancement of the chemical oxidation of arsenopyrite by adding pyrite to the arsenopyrite chemical oxidation system.

[0039] Based on the above inventors' discovery, the technical solution of the present invention is as follows:

[0040] The method for strengthening the chemical oxidation of arsenopyrite comprises the following steps: adding a certain amount of pyrite to the arsenopyrite chemical oxidation system, utilizing the characteristic of pyrite oxidation to generate acid, lowering the pH of the system, converting the iron hydroxide precipitate in the passivation layer into ferric arsenate, and using pyrite as an Fe source to increase the Fe / As molar ratio in the system and reduce the stability of the ferric arsenate in the passivation layer; since Fe(III) and Fe(II) on the sulfur defect sites on the surface of pyrite can activate small molecule environmental mediators, the generated ROS has an oxidizing ability to arsenopyrite, thereby strengthening the oxidation of arsenopyrite.

[0041] Preferably, the mass ratio of arsenopyrite sample to pyrite sample in the system should be greater than 1:1. Reducing the ore ratio can effectively enhance the leaching rate of arsenic in arsenopyrite. When the ore ratio is greater than 1:1, the content of ferric arsenate in the passivation layer increases, and the growth rate of ferric arsenate crystals is higher than the nucleation rate, the crystal size is large, the crystal quality is high, and the passivation layer structure is stable, which is not conducive to the oxidation of arsenopyrite.

[0042] Based on the above technical solution, the present invention discloses a method for strengthening chemical oxidation of arsenopyrite as in any embodiment of the present invention, comprising the following steps:

[0043] (1) The arsenopyrite block was crushed and ground as the leaching sample.

[0044] In a specific embodiment, the arsenopyrite block is taken from an iron mine in Chifeng, Inner Mongolia.

[0045] In a specific embodiment, step (1) specifically includes: taking a high-purity arsenopyrite lump ore, crushing it to -1 to 3 mm, then picking out gangue impurities, grinding it to -0.1 to 0.3 mm, and then entering a shaking table for sorting, and the resulting concentrate is ground to -0.03 to 0.05 mm as a leaching sample. The arsenopyrite ore sample is chemically analyzed, and the mass fraction of each element is: 43 to 47% As, 32 to 36% Fe, and 17 to 21% S.

[0046] (2) The pyrite blocks were crushed and ground as leaching samples.

[0047] In a specific embodiment, the pyrite block is taken from an iron mine in Guilin, Guangxi.

[0048] In a specific embodiment, step (2) specifically includes: taking high-purity pyrite lumps, crushing them to -1 to 3 mm, and then picking out gangue impurities, grinding them to -0.1 to 0.3 mm, and then entering the shaking table for sorting. The resulting concentrate is ground to -0.03 to 0.05 mm as a leaching sample.

[0049] (3) The arsenopyrite leaching sample and the pyrite leaching sample are placed in a basic salt solution, and the initial leaching pH is adjusted to 2-9 using dilute sulfuric acid and potassium hydroxide solution to obtain an oxidation system.

[0050] In a specific embodiment, the basic salt solution composition is: (NH4)2SO4 is 2-4 g / L, KCl is 0.1-0.3 g / L, K2HPO4 is 0.3-0.7 g / L, MgSO4·7H2O is 0.3-0.7 g / L, Ca(NO3)2 is 0.01-0.03 g / L, and the rest is deionized water.

[0051] In a specific embodiment, the slurry concentration of the arsenopyrite leaching sample in the solution is 1-2%.

[0052] In a specific embodiment, the slurry concentration of the pyrite leaching sample in the solution is 1-4%.

[0053] In a specific embodiment, the mass ratio of the arsenopyrite sample to the pyrite sample in the system is not greater than 1:1.

[0054] In a specific embodiment, the concentration of dilute sulfuric acid is 3-8 mol / L.

[0055] In a specific embodiment, the concentration of the potassium hydroxide solution is 3-8 mol / L.

[0056] (4) The oxidation system is placed in an air bath constant temperature oscillator for oscillation oxidation at 20-50° C. and 100-180 r / min for 18-25 days, thereby achieving enhanced oxidation of arsenopyrite.

[0057] The following are specific embodiments of the present disclosure:

[0058] Example 1

[0059] The method for strengthening chemical oxidation of arsenopyrite in this embodiment specifically comprises the following steps:

[0060] Step 1: Take high-purity arsenopyrite ore, crush it to -2mm, then select and remove gangue impurities, grind it to -0.25mm, and then put it into a shaking table for sorting. The resulting concentrate is ground to -0.045mm as a leaching sample.

[0061] Step 2: Take the pyrite ore with higher purity, crush it to -2mm, select and remove the gangue impurities, grind it to -0.25mm, and then put it into the shaking table for sorting. The obtained concentrate is ground to -0.045mm as the leaching sample.

[0062] Step 3: weigh 3.0 g of (NH4)2SO4, 0.1 g of KCl, 0.5 g of K2HPO4, 0.5 g of MgSO4·7H2O, and 0.01 g of Ca(NO3)2, add them to 1000 mL of deionized water, stir thoroughly to dissolve, and form a basic salt solution.

[0063] Step 4: Weigh 2 g of arsenopyrite leaching sample and 2 g of pyrite leaching sample and place them in a basic salt solution, and use 5 mol / L dilute sulfuric acid to adjust the initial leaching pH to 2 to obtain an arsenopyrite oxidation system.

[0064] Step five, placing the oxidation system in an air bath constant temperature oscillator for oscillation oxidation at 30° C. and 110 r / min for 18 days, thereby finally achieving enhanced oxidation of arsenopyrite.

[0065] Example 2

[0066] The difference between this embodiment and embodiment 1 is that the preparation parameters of step 4 are changed as follows:

[0067] Step 4: Weigh 2 g of arsenopyrite leaching sample and 4 g of pyrite leaching sample and place them in a basic salt solution, and use 5 mol / L dilute sulfuric acid to adjust the initial leaching pH to 2 to obtain an arsenopyrite oxidation system.

[0068] Example 3

[0069] The difference between this embodiment and embodiment 1 is that the preparation parameters of step 4 are changed as follows:

[0070] Step 4: Weigh 2 g of arsenopyrite leaching sample and 4 g of pyrite leaching sample and place them in a basic salt solution, and use 5 mol / L dilute sulfuric acid to adjust the initial leaching pH to 5 to obtain an arsenopyrite oxidation system.

[0071] Example 4

[0072] The difference between this embodiment and embodiment 1 is that the preparation parameters of step 4 are changed as follows:

[0073] Step 4: Weigh 2 g of arsenopyrite leaching sample and 4 g of pyrite leaching sample and place them in a basic salt solution, and use 5 mol / L potassium hydroxide solution to adjust the initial leaching pH to 9 to obtain an arsenopyrite oxidation system.

[0074] Comparative Example 1

[0075] This comparative example adopts a single arsenopyrite oxidation system, and the specific preparation steps are as follows:

[0076] Step 1: Prepare arsenopyrite leaching sample:

[0077] Take high-purity arsenopyrite lumps, crush them to -2mm, pick out gangue impurities, grind them to -0.25mm, and put them into a shaking table for sorting. The resulting concentrate is ground to -0.045mm as a leaching sample.

[0078] Step 2: Prepare basic salt solution:

[0079] Weigh 3.0 g of (NH4)2SO4, 0.1 g of KCl, 0.5 g of K2HPO4, 0.5 g of MgSO4·7H2O, and 0.01 g of Ca(NO3)2, add them to 1000 mL of deionized water, stir thoroughly to dissolve, and form a basic salt solution.

[0080] Step 3: Prepare arsenopyrite oxidation system:

[0081] 2 g of arsenopyrite leaching sample was weighed and placed in a basic salt solution, and 5 mol / L dilute sulfuric acid was used to adjust the initial leaching pH to 2 to obtain an arsenopyrite oxidation system.

[0082] Step 4: Complete chemical oxidation of arsenopyrite:

[0083] The arsenopyrite oxidation system was placed in an air bath constant temperature oscillator for 18 days at 30°C and 110 r / min.

[0084] Comparative Example 2

[0085] Compared with Comparative Example 1, this comparative example differs in that the preparation parameters of step 3 are changed, as follows:

[0086] Step three, weigh 2 g of arsenopyrite leaching sample and place it in a basic salt solution, and use a 5 mol / L dilute sulfuric acid solution to adjust the initial leaching pH to 5 to obtain an arsenopyrite oxidation system.

[0087] Comparative Example 3

[0088] Compared with Comparative Example 1, this comparative example differs in that the preparation parameters of step 3 are changed, as follows:

[0089] Step three, weigh 2 g of arsenopyrite leaching sample and place it in a basic salt solution, and use a 5 mol / L potassium hydroxide solution to adjust the initial leaching pH to 9 to obtain an arsenopyrite oxidation system.

[0090] Test Case

[0091] 1. In the oxidation systems of Examples 1-3 and Comparative Examples 1-2, the Fourier transform infrared spectra of the leached residues are as follows: Figure 1 and Figure 2 As shown, at 823.16cm -1 The absorption peak observed at the wavelength is due to the stretching vibration of the As(V)-O bond of As(V)-O-Fe in the ferric arsenate compound. Figure 1 and Figure 2 As shown, the tensile vibration peak intensity of the ferric arsenate compound in the implementation examples is less than that in the comparative example, which proves that the addition of pyrite can reduce the content of the ferric arsenate compound in the passivation layer.

[0092] 2. The As concentration in the leaching solution of the oxidation system of Examples 1-4 and Comparative Examples 1-3 is as follows: Figure 3-Figure 5 As shown, it was found that under the same initial pH conditions, the As concentration in the leaching solution of the oxidation system of the implementation example was higher than that of the comparative example, proving that the addition of pyrite can enhance the oxidation of arsenopyrite.

[0093] 3. The pH changes over time in the oxidation system of Example 4 and Comparative Example 3 are as follows: Figure 6 As shown, it is found that the pH of the oxidation system of the embodiment example is lower than that of the comparative example, indicating that the addition of pyrite can reduce the pH of the arsenopyrite oxidation system.

[0094] 4. The variation trend of the cumulative amount of ·OH in the oxidation system of Example 1, Example 2, Example 4 and Comparative Example 1 and Comparative Example 3 over time is shown in the following figure: Figure 7 and Figure 8 As shown. This indicates that the addition of pyrite can increase the concentration of ·OH in the system, that is, the concentration of ROS.

[0095] In summary, the present invention adds the paragenetic mineral pyrite to the arsenopyrite chemical oxidation system, reduces the pH of the oxidation system, and realizes the regulation of the passivation layer in the arsenopyrite chemical oxidation system. At the same time, the ROS produced by activating the small molecule environmental medium by Fe (II) and Fe (III) on the sulfur defect sites on the surface of pyrite has the characteristics of oxidizing, so as to achieve the purpose of strengthening the oxidation of arsenopyrite. Therefore, using this method, at the initial pH of the oxidation system of 9, the arsenopyrite slurry concentration of 2%, the pyrite slurry concentration of 4%, after leaching for 18 days, the As concentration in the leachate is 777.9 mg / L, while the As concentration in the leachate in the arsenopyrite single system is only 196.5 mg / L, that is, the As leaching rate is increased by nearly 3 times.

[0096] The above-described embodiments are only embodiments of the present disclosure, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the present disclosure. It should be noted that, for a person of ordinary skill in the art, without departing from the concept of the present disclosure, several variations, equivalent substitutions, improvements, etc. may be made, all of which fall within the scope of protection of the present disclosure. Therefore, the scope of protection of the present disclosure shall be subject to the attached claims.

Claims

1. A method for strengthening the chemical oxidation of arsenopyrite, characterized in that: include: An arsenopyrite oxidation system is prepared, wherein the oxidation system comprises an arsenopyrite leaching sample and a pyrite leaching sample, wherein the mass ratio of the arsenopyrite leaching sample to the pyrite leaching sample is not greater than 1:

1.

2. The method for strengthening chemical oxidation of arsenopyrite according to claim 1, characterized in that: The method for preparing the arsenopyrite oxidation system comprises: The arsenopyrite leaching sample and the pyrite leaching sample are placed in a basic salt solution, and the initial pH of the system is adjusted to 2-9 to obtain the oxidation system.

3. The method for strengthening chemical oxidation of arsenopyrite according to claim 2, characterized in that: The slurry concentration of the arsenopyrite leaching sample in the basic salt solution is 1-2%; The slurry concentration of the pyrite leaching sample in the basic salt solution is 1-4%.

4. The method for strengthening chemical oxidation of arsenopyrite according to claim 3, characterized in that: The basic salt solution comprises: 2-4 g / L (NH4)2SO4, 0.1-0.3 g / L KCl, 0.3-0.7 g / L K2HPO4, 0.3-0.7 g / L MgSO4·7H2O, 0.3-0.7 g / L Ca(NO3)2, and the rest is deionized water.

5. The method for strengthening chemical oxidation of arsenopyrite according to claim 4, characterized in that: The initial pH of the system is adjusted by using dilute sulfuric acid and potassium hydroxide solution, wherein the concentration of the dilute sulfuric acid is 3-8 mol / L; and the concentration of the potassium hydroxide solution is 3-8 mol / L.

6. The method for strengthening chemical oxidation of arsenopyrite according to any one of claims 1 to 5, characterized in that: Also includes: The arsenopyrite oxidation system is chemically oxidized to enhance the oxidation of the arsenopyrite.

7. The method for strengthening chemical oxidation of arsenopyrite according to claim 6, characterized in that: The method for chemically oxidizing the arsenopyrite oxidation system comprises: The oxidation system is placed in an air bath constant temperature oscillator for oscillation oxidation for 18 to 25 days at 20 to 50° C. and 100 to 180 r / min.

8. The method for strengthening chemical oxidation of arsenopyrite according to any one of claims 1 to 5 or 7, characterized in that: The particle size of the arsenopyrite leaching sample and the pyrite leaching sample is -0.03 to 0.05 mm.

9. The method for strengthening chemical oxidation of arsenopyrite according to claim 8, characterized in that: The method for preparing the arsenopyrite leaching sample comprises: Take the arsenopyrite lump ore with purity meeting the requirements, crush it to -1~3mm, select and remove the gangue impurities, grind it to -0.1~0.3mm for sorting, and the obtained concentrate is ground to -0.03~0.05mm as the leaching sample.

10. The method for strengthening chemical oxidation of arsenopyrite according to claim 8, characterized in that: The method for preparing the pyrite leaching sample comprises: Take pyrite lumps with purity that meets the requirements, crush them to -1~3mm, then pick out the gangue impurities, grind them to -0.1~0.3mm for sorting, and the obtained concentrate is ground to -0.03~0.05mm as leaching sample.

Citation Information

Patent Citations

  • Gold extraction process with low pollution and high recovery for refractory gold concentrate

    CN101285126A

  • Method for removing arsenic and sulfur from high-arsenic and high-sulfur gold ores

    CN105219948A

  • Method for strengthening microbiological leaching of arsenopyrite

    CN112375903A

  • Recovering metals from sulfidic materials

    CN1732277A