Method for improving structure uniformity of 2A12 aluminum alloy extruded bar

Through the steps of homogenization annealing, blind mold upsetting and solution quenching, the problem of poor structural uniformity of the 2A12 aluminum alloy extruded rod is solved, and the performance uniformity of large-sized rods is improved, ensuring the mechanical properties at different locations consistency.

CN119040779APending Publication Date: 2024-11-29SOUTHWEST ALUMINUM GRP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411244345.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The 2A12 aluminum alloy extruded rod has poor tissue uniformity when large specifications, resulting in large chromatic aberration after anodization of the processed product, affecting the uniformity of performance.

Method used

Through the steps of homogenization annealing, blind-molding, extrusion and solution quenching, the extrusion ratio and temperature are controlled, the precipitation and recrystallization of MnAl6 are promoted, the grain aggregation is prevented, and the structure uniformity is improved.

Benefits of technology

The structure and performance uniformity of the 2A12 aluminum alloy extruded rod is significantly improved, ensuring the consistency of mechanical properties at different locations, and improving the quality of the processed product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention provides a method for improving the structure uniformity of a 2A12 aluminum alloy extruded bar. The method comprises the following steps: S1) carrying out homogenizing annealing on a 2A12 aluminum alloy cast ingot; (S2) the aluminum alloy cast ingot obtained in the step (S1) is heated, and the heated aluminum alloy cast ingot is subjected to blind die upsetting; (S3) the aluminum alloy cast ingot obtained in the step (S2) is extruded; and (S4) the aluminum alloy bar obtained in the step (S3) is subjected to solid solution quenching, and finally natural aging is conducted. According to the method, the means of shortening the homogenizing annealing heat preservation time of the 2A12 aluminum alloy cast ingot, upsetting the cast ingot through the blind die and increasing the extrusion ratio of the 2A12 aluminum alloy cast ingot are shared, the structure uniformity of the large-specification 2A12 aluminum alloy extruded bar is improved, and therefore the mechanical property uniformity of the 2A12 aluminum alloy bar is improved, and the yield of the 2A12 aluminum alloy extruded bar is improved. And therefore, the anodic oxidation chromatic aberration of a product after the aluminum alloy bar is processed is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloy preparation, and in particular to a method for improving the uniformity of the structure of a 2A12 aluminum alloy extruded bar. Background Art

[0002] 2A12 aluminum alloy is a typical hard aluminum alloy in the Al-Cu-Mg series with good comprehensive properties. The alloy has the characteristics of high strength and heat resistance, and can be used as working parts below 150°C. It is widely used in aircraft structures, rivets, truck wheels, propeller components and other structural parts.

[0003] Extrusion is a process that applies pressure from one end to a metal ingot placed in an extrusion barrel, forcing it to flow out of a specific die hole to obtain a product with the required cross-sectional shape and size. During the extrusion process, the outer layer of the metal ingot is subjected to friction between the inner wall of the extrusion barrel and the die, resulting in uneven structure of the extruded product in both the cross-sectional and length directions. Generally, there will be problems such as large grains at the head, small grains at the tail, coarse grains in the center, and small grains in the outer layer (except for products with coarse grain rings after heat treatment). Similarly, the macrostructure of large-sized bars (diameter φ250~φ300mm) extruded from 2A12 aluminum alloy often has poor uniformity, resulting in large color differences in products processed from large-sized bars after anodizing.

[0004] The non-uniformity of the microstructure of large-size extruded 2A12 aluminum alloy bars is closely related to the extrusion ratio and the heat treatment of the ingot. Improper heat treatment has a great impact on the uniformity of the microstructure of the extruded bars. Therefore, it is of great significance to provide a method for improving the uniformity of the microstructure of 2A12 aluminum alloy bars. Summary of the invention

[0005] The technical problem solved by the present invention is to provide a method for improving the uniformity of the structure of 2A12 aluminum alloy extruded bars. The method provided in the present application can improve the uniformity of the structure of 2A12 aluminum alloy extruded bars, and then improve the performance uniformity of 2A12 aluminum alloy extruded bars.

[0006] In view of this, the present application provides a method for improving the uniformity of the structure of a 2A12 aluminum alloy extruded bar, comprising the following steps: S1) homogenizing annealing the 2A12 aluminum alloy ingot, wherein the homogenizing annealing temperature is 480-495° C. and the holding time is 3-5 h; S2) heating the aluminum alloy ingot obtained in step S1), and performing blind die upsetting on the heated aluminum alloy ingot; S3) extruding the aluminum alloy ingot obtained in step S2), wherein the extrusion ratio is 7.1-10.3; S4) The aluminum alloy bar obtained in step S3) is subjected to solution quenching and finally natural aging.

[0007] Preferably, in step S1), the temperature of the homogenization annealing is 485-495° C., and the holding time is 4 hours.

[0008] Preferably, in step S2), the heating temperature is 440-460°C.

[0009] Preferably, in step S3), the extrusion speed is ≤0.6 m / min.

[0010] Preferably, in step S3), the extrusion ratio of the extrusion is 7.11-10.24.

[0011] Preferably, in step S4), the solutionizing temperature is 490-500°C, and the quenching water temperature is 20-40°C.

[0012] Preferably, in step S4), the natural time is greater than 96 hours.

[0013] Preferably, in step S1), the diameter of the 2A12 aluminum alloy ingot is φ550 mm, in step S2), the diameter of the extrusion barrel of the blind die upsetting is φ800 mm, and the upsetting ratio is 2.1.

[0014] Preferably, in step S3), the diameter of the extrusion cylinder is φ800 mm, and the diameter of the aluminum alloy bar after extrusion is φ250~φ300 mm.

[0015] Preferably, the Mn content in the 2A12 aluminum alloy ingot is 0.30-0.90wt%.

[0016] The present application provides a method for improving the uniformity of the structure of a 2A12 aluminum alloy extruded bar, which comprises firstly subjecting the 2A12 aluminum alloy ingot to homogenization annealing, then heating the aluminum alloy ingot, and then subjecting the aluminum alloy ingot to blind die upsetting, and then subjecting the extrusion treatment to solution quenching and natural aging to obtain a 2A12 aluminum alloy extruded bar; in the method provided by the present application, the present application adopts a specific homogenization annealing system, so that the MnAl6 dispersed particles in the alloy have no time to gather and grow, and in the subsequent extrusion, due to the geometric constraints of the die and the strong friction, the outer layer of metal flows lagging behind the central part, and the outer layer of metal presents a large stress gradient and The additional tensile stress state promotes the precipitation of Mn, reduces the recrystallization temperature of the solid solution, and produces primary recrystallization. However, since the second phase is precipitated from the crystal and distributed on the grain boundary in a dispersed particle state, the aggregation and growth of the grains are hindered, and large-sized bars with good uniformity and consistency of organization can be extruded; the subsequent blind die upsetting causes the aluminum alloy ingot to undergo a pre-deformation in the extrusion barrel, which is conducive to obtaining bars with uniform organization. Finally, a higher extrusion ratio is limited to further ensure the uniformity of the organization of the 2A12 aluminum alloy bar. In summary, the method provided in the present application improves the uniformity of the organization of the 2A12 aluminum alloy extruded bar and achieves the uniformity of performance at different positions. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The graph is a relationship between the excess volume percentage of the non-equilibrium phase dissolved and the homogenization time when the 2A12 aluminum alloy ingot of the present invention is homogenized at 490°C; Figure 2 The microstructure photos of different positions of the φ280mm2A12 aluminum alloy bar prepared in the embodiment of the present invention; Figure 3 These are microstructure photos of different positions of the φ280mm2A12 aluminum alloy bar prepared in the comparative example of the present invention. DETAILED DESCRIPTION

[0018] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0019] In view of the problem of poor uniformity of low-magnification microstructure of large-sized (diameter φ250~φ300mm) 2A12 aluminum alloy extruded bars in the prior art, the present application provides a method for improving the microstructure uniformity of 2A12 aluminum alloy extruded bars, which improves the microstructure uniformity of large-sized 2A12 aluminum alloy extruded bars by shortening the homogenization annealing and heat preservation time of 2A12 aluminum alloy ingots, using blind molds to upset the ingots, and increasing the extrusion ratio of 2A12 aluminum alloy ingots. The microstructure uniformity of 2A12 aluminum alloy extruded bars is improved, thereby improving the microstructure uniformity of 2A12 aluminum alloy bars. Specifically, an embodiment of the present invention discloses a method for improving the microstructure uniformity of 2A12 aluminum alloy extruded bars, comprising the following steps: S1) homogenizing annealing the 2A12 aluminum alloy ingot, wherein the homogenizing annealing temperature is 480-495° C. and the holding time is 3-5 h; S2) heating the aluminum alloy ingot obtained in step S1), and performing blind die upsetting on the heated aluminum alloy ingot; S3) extruding the aluminum alloy ingot obtained in step S2), wherein the extrusion ratio is 7.1-10.3; S4) subjecting the aluminum alloy ingot obtained in step S3) to solid solution quenching and finally to natural aging.

[0020] In the method provided in the present application, the present application first prepares a 2A12 aluminum alloy ingot, and the preparation method is carried out in a manner familiar to those skilled in the art, specifically: raw material acceptance → batching → smelting → furnace purification → online refinement → online degassing → online hydrogen measurement → online filtration → casting; the above stages are carried out in a manner familiar to those skilled in the art, and the present application does not impose any special restrictions on this. The diameter of the 2A12 aluminum alloy extruded bar of the present application is φ250~φ300mm. In order to prepare the above-mentioned large-size aluminum alloy extruded bar, in the present application, the diameter of the 2A12 aluminum alloy ingot is 550mm, so as to increase the deformation of the ingot during extrusion.

[0021] The present application then performs homogenization annealing on the 2A12 aluminum alloy ingot, wherein the homogenization annealing makes the unbalanced eutectic structure in the ingot tend to be evenly distributed therein, and the supersaturated solid solution elements precipitate from the solid solution to eliminate the ingot stress, improve the ingot plasticity, reduce the deformation resistance, and improve the structure and performance of the processed product.

[0022] 2A12 aluminum alloy contains 0.30wt%~0.90wt% Mn, and its homogenization annealing temperature is 480~495℃. Within this temperature range, MnAl6 in the alloy will be precipitated from the matrix in large quantities. This is because during the casting process, the cooling speed is fast, and the MnAl6 phase does not have enough time to fully precipitate from the matrix. Therefore, during homogenization annealing, the MnAl6 phase further precipitates from the matrix. Under the action of long-term high temperature, the MnAl6 dispersed particles gather and grow, thereby reducing the recrystallization temperature and the ability to prevent recrystallization of the alloy during deformation. Therefore, for 2A12 aluminum alloy ingots, the longer the homogenization annealing holding time, the better.

[0023] The holding time basically depends on the time required for the non-equilibrium phase to dissolve and the intracrystalline segregation to be removed. Since these two processes occur simultaneously, the holding time is not the algebraic sum of the time required for these two processes. Experiments have shown that the time for the aluminum alloy solid solution composition to be fully homogenized is only slightly longer than the time for the non-equilibrium phase to be completely dissolved; in most cases, the homogenization completion time can be estimated based on the time for the non-equilibrium phase to be completely dissolved.

[0024] As the homogenization annealing process proceeds, the concentration gradient within the crystal decreases continuously, and the amount of diffused material also decreases continuously, so that the homogenization process tends to slow down automatically. Figure 1 As shown in the figure, when the 2A12 aluminum alloy ingot is homogenized and annealed, the total amount of non-equilibrium phase reduction in the first 30 minutes is much greater than that in the last 7 hours; this shows that excessively extending the homogenization annealing time is not only ineffective, but will reduce the furnace production capacity and increase heat energy consumption. However, the ingot diameter is large (φ550mm), and the insulation time is too short, which cannot effectively eliminate the internal stress of the ingot, and it is easy to crack during subsequent processing. Therefore, through process practice, the homogenization annealing time of this specification ingot is selected as 4 hours, and the annealing temperature remains unchanged. Under this homogenization annealing process, the MnAl6 dispersed particles have no time to gather and grow. During extrusion, due to the geometric constraints of the die and the strong friction, the outer metal flow lags behind the central part, and the outer metal presents a large stress gradient and additional tensile stress state, which promotes the precipitation of Mn, reduces the recrystallization temperature of the solid solution, and produces primary recrystallization. However, because the second phase precipitates from the crystal and is distributed on the grain boundary in a dispersed particle state, it hinders the aggregation and growth of the grains, thereby extruding large-size bars with good uniformity and consistency of organization.

[0025] According to the present invention, the aluminum alloy ingot after homogenization annealing is then heated, and the heating temperature is 440-460°C, specifically, the heating temperature is 445-455°C.

[0026] The present application then performs upsetting on the heated aluminum alloy ingot, and the upsetting is specifically as follows: replace the blind die on the extruder, and introduce the heated aluminum alloy ingot into the φ800mm extrusion barrel for upsetting. The ingot with a diameter of φ550mm is upset with a blind die in the φ800mm extrusion barrel, and the upsetting ratio is 2.1, so that the aluminum alloy ingot undergoes a pre-deformation in the extrusion barrel, which is conducive to obtaining a rod with uniform structure. The blind die is a solid die (similar to a plug).

[0027] The present application then directly extrude the aluminum alloy ingot after upsetting in a φ800mm extrusion cylinder to obtain extruded rods with a diameter of φ250~φ300mm, and the extrusion ratio can reach 10.24~7.11; specifically, the extrusion ratio is 9.5 for extruding to a rod with a diameter of 260mm, 8.2 for extruding to a rod with a diameter of 280mm, and 7.1 for extruding to a rod with a diameter of 299mm. The inhomogeneity of the structure of large-size 2A12 aluminum alloy extruded rods is greatly related to the extrusion ratio. When the extrusion ratio is below 8, the structural characteristics at the center and periphery are still uneven, and the smaller the extrusion ratio, the greater the inhomogeneity. When the extrusion ratio is between 8 and 16, the structure is basically uniform; while the current large-size bars (diameter φ250~φ300mm) extruded from 2A12 alloy are extruded in a φ650mm extrusion barrel, and the extrusion ratio is 6.76~4.69, the deformation degree is small, and the structure inhomogeneity is very obvious; the present application improves the uniformity of the obtained aluminum alloy bars by adjusting the diameter of the extrusion barrel and the extrusion ratio. The extrusion speed of the extrusion is ≤0.6m / min to prevent cracks.

[0028] The present application finally performs solid solution quenching on the obtained aluminum alloy bar, and then performs natural aging; the solid solution temperature of the solid solution quenching is 490-500°C, and the holding time is 10-12h; specifically, the holding time is 10.5h, 11h or 12h; the quenching water temperature is 20-40°C. The natural aging time is greater than 96h.

[0029] In order to further understand the present invention, the method for improving the uniformity of the structure of the 2A12 aluminum alloy extruded rod provided by the present invention is described in detail below in conjunction with the embodiments. The protection scope of the present invention is not limited by the following embodiments.

[0030] Example

[0031] The process of improving the uniformity of the structure of large-size (diameter φ250~φ300mm) 2A12 aluminum alloy extruded bars is as follows: optimize the specifications of 2A12 aluminum alloy ingots → ingot preparation → ingot homogenization annealing → ingot heating → upsetting → extrusion → solution quenching → natural aging → sampling and analysis; specifically includes the following steps: 1) Optimize the specifications of 2A12 aluminum alloy ingots A 2A12 aluminum alloy ingot with a diameter of φ250~φ300mm is extruded in a φ650mm extrusion cylinder to obtain a 2A12 aluminum alloy bar with a diameter of φ250~φ300mm; in the existing process, the diameter of the original aluminum alloy ingot is φ630mm, and the ingot diameter is now optimized to φ550mm, so as to increase the deformation of the ingot during extrusion; 2) After the specifications of the 2A12 aluminum alloy ingot are determined, an aluminum alloy ingot with a diameter of φ550 mm2A12 is prepared according to the original process, i.e., raw material acceptance → batching → smelting → furnace purification → online refinement → online degassing → online hydrogen measurement → online filtration → casting. After the above preparation process, a 2A12 aluminum alloy ingot is obtained; 3) homogenizing annealing of 2A12 aluminum alloy ingot with a diameter of φ550 mm according to the system of 480~495℃ / 4h; 4) heating the aluminum alloy ingot obtained in step 3) at 445-455° C.; 5) Replace the blind die on the extruder, introduce the heated aluminum alloy ingot into the φ800mm extrusion cylinder, and then perform blind die upsetting to obtain a 2A12 aluminum alloy ingot with a diameter of φ800mm; 6) After the upsetting is completed, the extrusion cylinder is replaced with a large-size rod die to be extruded and extrusion is started to obtain 2A12 aluminum alloy rods with a diameter of φ260mm, a diameter of φ280mm, and a diameter of φ299mm. The extrusion speed does not exceed 0.6m / min; 7) The 2A12 aluminum alloy extruded bar obtained in step 6) is solutionized at 495-500°C, and the holding time is 10.5h, 11.5h, and 12h respectively according to the relevant provisions of AMS 2772, and the quenching water temperature is 20-40°C; 8) Natural aging of the 2A12 aluminum alloy bar after solid solution for more than 96 hours; 9) Take samples of 2A12 aluminum alloy bars after natural aging and test low magnification, microstructure and other items. The results are as follows: Figure 2 As shown in Table 1; Table 1 Mechanical properties of 2A12 T4 large-size aluminum alloy bars

[0032] It can be seen from Table 1 that the mechanical properties of aluminum alloy bars of the same specifications at the center, 1 / 2 radius and circumference are not much different; Figure 2 The microstructures of different positions of φ280mm aluminum alloy bars are shown in Figure 1. Figure 2 It can be seen that the metallographic structure of the aluminum alloy rod at different positions is relatively uniform.

[0033] Comparative Example 1 The preparation method of the 2A12 aluminum alloy bar is the same as that of the above embodiment, except that upsetting is not performed, that is, step 5 is not performed); the mechanical properties of the aluminum alloy bar prepared in this comparative example are shown in Table 2; Table 2 Mechanical properties of the φ280 mm rods prepared in this comparative example

[0034] It can be seen from Table 2 that the mechanical properties of the aluminum alloy bar obtained at the center, 1 / 2 radius and circumference are quite different when blind die upsetting is not performed during the preparation of the φ280mm large-size 2A12 aluminum alloy bar. Figure 3 The microstructures of different positions of φ280mm aluminum alloy bars are shown in Figure 1. Figure 3 It can be seen that the metallographic structures of aluminum alloy bars at different positions are quite different.

[0035] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

[0036] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for improving the uniformity of the microstructure of 2A12 aluminum alloy extruded bars. The following steps are involved: S1) homogenizing annealing the 2A12 aluminum alloy ingot, wherein the homogenizing annealing temperature is 480-495° C. and the holding time is 3-5 h; S2) heating the aluminum alloy ingot obtained in step S1), and performing blind die upsetting on the heated aluminum alloy ingot; S3) extruding the aluminum alloy ingot obtained in step S2), wherein the extrusion ratio is 7.1-10.3; S4) The aluminum alloy bar obtained in step S3) is subjected to solution quenching and finally natural aging.

2. The improvement method according to claim 1, It is characterized in that In step S1), the homogenization annealing temperature is 485-495° C., and the holding time is 4 hours.

3. The improving method according to claim 1, It is characterized in that In step S2), the heating temperature is 440-460°C.

4. The improving method according to claim 1, It is characterized in that In step S3), the extrusion speed is ≤0.6 m / min.

5. The improving method according to claim 1, It is characterized in that In step S3), the extrusion ratio of the extrusion is 7.11-10.

24.

6. The improving method according to claim 1, It is characterized in that In step S4), the solution temperature is 490-500°C, and the quenching water temperature is 20-40°C.

7. The improving method according to claim 1, It is characterized in that In step S4), the natural time is greater than 96 hours.

8. The improving method according to claim 1, It is characterized in that In step S1), the diameter of the 2A12 aluminum alloy ingot is φ550 mm, in step S2), the diameter of the extrusion barrel of the blind die upsetting is φ800 mm, and the upsetting ratio is 2.

1.

9. The improving method according to claim 8, It is characterized in that In step S3), the diameter of the extrusion cylinder is φ800 mm, and the diameter of the aluminum alloy bar after extrusion is φ250~φ300 mm.

10. The improving method according to any one of claims 1 to 9, It is characterized in that The Mn content in the 2A12 aluminum alloy ingot is 0.30-0.90wt%.