Laser cladding repairing method for spinning die

The spinning mold is repaired through laser cladding technology, which solves the damage problem of the mold in high-strength environment, realizes multiple repairs and wear resistance, and reduces cost and replacement frequency.

CN119040886APending Publication Date: 2024-11-29SHAANXI LEISHI ADDITIVE INTELLIGENT MANUFACTURING CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411479701.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Spinning dies are prone to structural damage in high-strength extrusion and wear environments, resulting in insufficient accuracy and high replacement cost. Traditional welding repair is difficult and cannot achieve secondary repair, and the utilization rate is low.

Method used

The spinning mold is repaired by laser cladding technology, and the damaged layer is removed by cutting, preheating and laser cladding form a cladding repair layer, and grinding is carried out after cooling and solidification to ensure the stability and wear resistance of the repair layer. .

Benefits of technology

Multiple cycle repairs of spinning molds are achieved, which extends service life, reduces high costs after secondary damage, avoids cracking, and maintains high wear resistance and strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040886A_ABST
    Figure CN119040886A_ABST
Patent Text Reader

Abstract

The invention discloses a spinning mold laser cladding repairing method which comprises the following steps: setting a cutting amount, cutting the surface of a spinning mold according to the cutting amount, and cutting off a damaged layer of the spinning mold to obtain a cutting surface; a preheating path and a to-be-cladded path are determined on the cutting face, and the preheating path comprises the to-be-cladded path; preheating the preheating path, and starting to perform laser cladding on the to-be-cladded path after part of the to-be-cladded path is preheated, so as to obtain a cladding repair layer; putting the spinning mold subjected to laser cladding into a heat preservation environment until the cladding repair layer is cooled and solidified; and the cooled and solidified cladding repairing layer is ground, so that repairing of the spinning mold is completed. The spinning mold is repaired through the method, so that the spinning mold cannot crack in the repairing process, the repaired spinning mold still has high abrasion resistance and strength and can be cyclically repaired for multiple times, and the service life of the spinning mold is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of spinning die repair technology, and in particular to a laser cladding repair method for spinning dies. Background Technology

[0002] In the spinning process of barrel-shaped parts, the spinning die, as a core tool, plays a crucial role in the machining accuracy and quality of the parts. However, spinning dies operate under continuous high-intensity extrusion and wear conditions, facing harsh usage conditions and prone to various structural damages, including but not limited to axial tensile damage, severe surface wear, and extrusion deformation. Once any of these types of structural damage occurs, the spinning die will suffer from insufficient accuracy or even become unusable, affecting production progress and resulting in high replacement costs and resource waste.

[0003] Most common spinning dies use cold work die steel as raw material, such as Cr12MoV and 70Cr3NiMo. Although these materials have excellent hardness and wear resistance, the forging and heat treatment processes are complex, the process control is difficult, and the weldability is poor. These characteristics bring problems such as high production cost, long manufacturing cycle and difficulty in reuse to spinning dies.

[0004] Traditional methods for repairing spinning dies involve welding to repair damaged areas on the die surface. However, due to the high carbon content of cold work die steel, its hardness reaches 57-60 HRC after overall quenching, making welding difficult. Furthermore, uneven heating and cooling during welding can lead to uneven hardness in the repaired area, making it prone to welding cracks. Additionally, the microstructure of cold work die steel changes after welding, making secondary welding impossible. This results in the inability to perform secondary repairs on the spinning die, leading to low utilization of the spinning die. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a laser cladding repair method for spinning dies.

[0006] To solve the above-mentioned technical problems, the present invention adopts the following technical solution: This invention provides a method for laser cladding repair of spinning dies, comprising: Set a cutting amount, and cut the surface of the spinning die according to the cutting amount to remove the damaged layer of the spinning die to obtain the cutting surface; A preheating path and a cladding path are defined on the cutting surface, wherein the preheating path includes the cladding path; The preheating path is preheated, and after a portion of the path to be clad is preheated, laser cladding is performed on the path to be clad to obtain a cladding repair layer. The spinning die after laser cladding is placed in a heat-insulating environment until the cladding repair layer cools and solidifies; The cooled and solidified cladding repair layer is ground to complete the repair of the spinning die.

[0007] In one embodiment, in the step of setting the cutting amount and cutting the surface of the spinning die according to the cutting amount to remove the damaged layer of the spinning die to obtain the cutting surface, the cutting amount is determined by the following formula: When A≤t, B=|f|+2t; When A > t, B = |f| + 2A; Where B is the cutting amount, f is the lower deviation value of the required diameter of the spinning die, t is the minimum required functional layer thickness of the spinning die, and A is the depth of the damaged layer of the spinning die.

[0008] In one embodiment, the preheating path includes a preheating start point s 起 and preheating termination point s 终 The path to be clad includes the cladding starting point a. 起 and cladding termination point a 终 ; where s 起 With a 起 The distance is 3-5mm, a 终 With s 终 The distance is 1 to 3 mm.

[0009] In one embodiment, the step of preheating the preheating path and, after a portion of the path to be clad has been preheated, starting laser cladding of the path to be clad to obtain a cladding repair layer includes: The heater is operated from the preheating starting point s 起 Start towards the preheating termination point s 终 Move to preheat; When the heater moves beyond the cladding initiation point a 起 When the distance is 1.5–3.5 mm, the laser operates from the cladding starting point a. 起 Start towards cladding termination point a 终 The heater moves at the same speed as the laser to perform laser cladding.

[0010] In one embodiment, before the step of preheating the preheating path and starting laser cladding on the path to be clad after partial preheating of the path to be clad to obtain the cladding repair layer, the method further includes: Before the heater is operated, the preheating temperature of the heater is set to 190-210°C.

[0011] In one embodiment, before the step of preheating the preheating path and starting laser cladding on the path to be clad after partial preheating of the path to be clad to obtain the cladding repair layer, the method further includes: Before the laser is operated, the cladding parameters of the laser are set, including cladding linear speed, overlap ratio, laser power, and cladding thickness; wherein, the cladding linear speed is 20-50 mm / s, the overlap ratio is 35-55%, the laser power is 3000-5000 W, and the cladding thickness δ= q is a constant, with a value ranging from 1.0 to 1.3 mm.

[0012] In one embodiment, the laser is used to laser clad the spinning die with low-carbon, high-chromium self-fluxing alloy powder, wherein the low-carbon, high-chromium self-fluxing alloy powder has a carbon content of 0.15-0.2% and a chromium content of 17.5-19%.

[0013] In one embodiment, the step of placing the laser-clad spinning die into a heat-insulating environment until the cladding repair layer cools and solidifies includes: The spinning mold that has undergone laser cladding is embedded in insulating perlite for heat preservation until the cladding repair layer cools and solidifies.

[0014] In one embodiment, the step of grinding the cooled and solidified cladding repair layer to complete the repair of the spinning die includes: The cladding repair layer is ground using a white corundum grinding wheel to complete the repair of the spinning die.

[0015] In one embodiment, after grinding the cooled and solidified cladding repair layer to complete the repair of the spinning die, the method further includes: The parameters of the spinning die are tested to confirm whether the repaired spinning die is qualified.

[0016] The advantages of the laser cladding repair method for spinning dies of the present invention compared with the prior art are as follows: By using laser cladding technology to repair the spinning die, and preheating the cutting surface of the spinning die before laser cladding, the temperature difference between the cutting surface and the cladding repair layer is reduced, thereby reducing thermal stress and lowering the cracking tendency of the cladding repair layer; at the same time, after the laser cladding is completed, the spinning die is placed in a heat-insulating environment for cooling, which effectively prevents the cladding repair layer from cracking due to rapid temperature drop. After the cladding repair layer cools and solidifies, it is then ground to obtain the repaired spinning die. Multiple cyclic repairs can be performed. In other words, by using the laser cladding repair method for spinning dies provided by the present invention, the spinning die will not crack during the repair process. The repaired spinning die still has high wear resistance and strength, and can be repaired multiple times, extending the service life of the spinning die and solving the high cost caused by direct scrapping after secondary damage to the spinning die.

[0017] The present invention will be further described below with reference to the accompanying drawings and specific embodiments. Attached Figure Description

[0018] To more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0019] Figure 1 A flowchart of the laser cladding repair method for spinning dies provided by the present invention; Figure 2 This is a schematic diagram illustrating an application scenario of the laser cladding repair method for spinning dies provided by the present invention. Detailed Implementation

[0020] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and specific embodiments.

[0021] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0022] In the description of this invention, it should be understood that the terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," and "counterclockwise," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.

[0023] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this invention, "a plurality of" means two or more, unless otherwise explicitly specified.

[0024] In this invention, unless otherwise explicitly specified and limited, the terms "installation," "connection," "linking," and "fixing," etc., should be interpreted broadly. For example, they can refer to a connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components. Those skilled in the art can understand the specific meaning of the above terms in this invention according to the specific circumstances.

[0025] In this invention, unless otherwise explicitly specified and limited, "above" or "below" the second feature can include direct contact between the first and second features, or contact between the first and second features through another feature between them. Furthermore, "above," "over," and "on top" of the second feature includes the first feature directly above or diagonally above the second feature, or simply indicates that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature includes the first feature directly below or diagonally below the second feature, or simply indicates that the first feature is at a lower horizontal level than the second feature.

[0026] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. The illustrative expressions of the above terms in this specification should not be construed as necessarily referring to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. In addition, those skilled in the art can combine and integrate the different embodiments or examples described in this specification.

[0027] See Figures 1 to 2 As shown, this invention discloses a specific embodiment of a laser cladding repair method for spinning dies, including: S1, Set the cutting amount, and cut the surface of the spinning die according to the cutting amount to remove the damaged layer of the spinning die to obtain the cutting surface; S2, determine a preheating path and a cladding path on the cutting surface, wherein the preheating path includes the cladding path; S3, preheat the preheating path, and after a portion of the path to be clad is preheated, begin laser cladding of the path to be clad to obtain a cladding repair layer; S4, the spinning mold that has completed laser cladding is placed in a heat-preserving environment until the cladding repair layer cools and solidifies; S5, the cooled and solidified cladding repair layer is ground to complete the repair of the spinning die.

[0028] Specifically, laser cladding technology is used to repair spinning dies. Before laser cladding, the cutting surface of the spinning die is preheated. The preheating path includes the path to be clad. After part of the path to be clad is preheated, laser cladding begins. This reduces the temperature difference between the cladding repair layer and the cutting surface, thereby reducing thermal stress and lowering the tendency of the cladding repair layer to crack. After laser cladding is completed, the spinning die is placed in an insulated environment to cool, effectively preventing the cladding repair layer from cracking due to rapid temperature drop. After the cladding repair layer cools and solidifies, it is then ground to achieve the dimensional tolerances and surface finish required by the drawings, resulting in a repaired spinning die that can be repeatedly repaired. By adopting the laser cladding repair method for spinning dies provided by this invention, the spinning dies will not crack during the repair process. The repaired spinning dies have a stable structure, high wear resistance and strength, and can be repaired multiple times, thus extending the service life of the spinning dies and solving the problem of high costs caused by direct scrapping after secondary damage to the spinning dies.

[0029] In one embodiment, in the step of setting the cutting amount and cutting the surface of the spinning die according to the cutting amount to remove the damaged layer of the spinning die to obtain the cutting surface, the cutting amount is determined by the following formula: When A≤t, B=|f|+2t; When A > t, B = |f| + 2A; Where B is the cutting amount, f is the lower deviation value of the required diameter of the spinning die, t is the minimum required functional layer thickness of the spinning die, and A is the depth of the damaged layer of the spinning die.

[0030] Specifically, the lower deviation value of the required diameter of the spinning die refers to the allowable range where the actual diameter of the spinning die is smaller than the standard diameter. The minimum functional layer thickness required for the spinning die refers to the minimum material thickness required on the spinning die to withstand the spinning pressure and maintain the shape and dimensional stability of the die during the spinning process. A is taken as the maximum value of the depth of the damaged layer that causes the spinning die to lose precision, including cracks, scratches, wear, etc. When A≤t, B is set to B=|f|+2t, that is, the amount of material to be cut off from the surface of the spinning die is set to |f|+2t; when A>t, B is set to B=|f|+2A, that is, the amount of material to be cut off from the surface of the spinning die is set to |f|+2A. By setting the cutting amount in this way, the damaged layer and the surrounding structure that may be affected are removed during the cutting process, which can effectively prevent the spread and aggravation of damage, thereby extending the service life of the spinning die. Moreover, the dimensional accuracy of the spinning die after cutting is high, and the cut surface is relatively smooth. At the same time, the spinning die also has sufficient machining allowance, which facilitates the smooth progress of subsequent repair processes.

[0031] In one embodiment, the preheating path includes a preheating start point s 起 and preheating termination point s 终 The path to be clad includes the cladding starting point a. 起 and cladding termination point a 终 ; where s 起 With a 起 The distance is 3-5mm, a 终 With s 终 The distance is 1 to 3 mm.

[0032] Specifically, the path to be clad needs to be determined according to the design drawings of the spinning die, while the preheating path is determined based on the determined path to be clad. This is achieved by including the path to be clad within the preheating path, where s 起 With a 起 The distance is 3-5mm, a 终 With s 终The distance is 1-3mm, which ensures that the cladding path and the surrounding cutting surface are heated, preventing uneven heating and cooling of the repair area during repair, which could lead to uneven hardness and cracking, thus improving the repair quality.

[0033] In one embodiment, the step of preheating the preheating path and, after a portion of the path to be clad has been preheated, starting laser cladding of the path to be clad to obtain a cladding repair layer includes: The heater is operated from the preheating starting point s 起 Start towards the preheating termination point s 终 Move to preheat; When the heater moves beyond the cladding initiation point a 起 When the distance is 1.5–3.5 mm, the laser operates from the cladding starting point a. 起 Start towards cladding termination point a 终 The heater moves at the same speed as the laser to perform laser cladding.

[0034] Specifically, during laser operation, the distance between the heater and the laser is consistently 1.5–3.5 mm, where 1.5–3.5 mm is the diameter of a laser spot formed by the laser beam emitted by the laser. By precisely controlling the moving speed and distance between the heater and the laser through the above steps, the preheating and laser cladding processes can be synergistically optimized. This ensures that the laser cladding area and its surrounding structure maintain a high temperature during laser cladding of the cutting surface, which helps improve repair efficiency, reduce energy consumption, and ensure that the quality and performance of the cladding repair layer reach the optimal level.

[0035] In one embodiment, the laser is used to laser clad the spinning die with low-carbon, high-chromium self-fluxing alloy powder, wherein the low-carbon, high-chromium self-fluxing alloy powder has a carbon content of 0.15-0.2% and a chromium content of 17.5-19%.

[0036] Specifically, by using low-carbon, high-chromium self-fluxing alloy powder as the laser cladding powder to repair spinning dies, the resulting cladding repair layer has a carbon content of 0.15–0.2% and a chromium content of 17.5–19%, exhibiting high hardness and wear resistance, with a hardness exceeding 60 HRC. It also forms a good metallurgical bond with the cutting surface of the spinning die, making it less prone to cracking. Furthermore, the low-carbon, high-chromium self-fluxing alloy powder contains elements such as boron and silicon, which, during the laser cladding process, form low-melting-point borosilicates that cover the molten pool surface, preventing excessive oxidation of the liquid metal and thus improving the corrosion resistance of the cladding repair layer. By using low-carbon, high-chromium self-fluxing alloy powder as the laser cladding powder for repairing spinning dies, the surface wear resistance and strength of the spinning die are improved, significantly extending its service life.

[0037] In one embodiment, before the step of preheating the preheating path and starting laser cladding on the path to be clad after partial preheating of the path to be clad to obtain the cladding repair layer, the method further includes: Before the heater is operated, the preheating temperature of the heater is set to 190-210°C.

[0038] Specifically, the heater adopts industrial frequency induction heating and is equipped with a closed-loop automatic temperature control system, which keeps the preheating temperature fluctuation range within ±10℃, effectively solving the problem of cold cracks in the spinning die during laser cladding.

[0039] In one embodiment, before the step of preheating the preheating path and starting laser cladding on the path to be clad after partial preheating of the path to be clad to obtain the cladding repair layer, the method further includes: Before the laser is operated, the cladding parameters of the laser are set, including cladding linear speed, overlap ratio, laser power, and cladding thickness; wherein, the cladding linear speed is 20-50 mm / s, the overlap ratio is 35-55%, the laser power is 3000-5000 W, and the cladding thickness δ= q is a constant, with a value ranging from 1.0 to 1.3 mm.

[0040] Specifically, by setting the cladding linear speed to 20–50 mm / s and the laser power to 3000–5000 W, the laser cladding powder can be rapidly melted and form a good metallurgical bond with the cutting surface of the spinning die. This ensures that the cladding repair layer achieves an ideal dilution rate and microstructure, resulting in excellent wear resistance and structural strength, while also improving cladding efficiency. Setting the overlap rate to 35–55% ensures a more uniform thickness of the cladding repair layer, facilitating subsequent grinding. Furthermore, by setting the cladding thickness to δ= q is a constant, ranging from 1.0 to 1.3 mm, and B is the cutting amount, so that the diameter of the spinning die obtained after cladding is D+q, where D is the diameter required by the spinning die drawing. This ensures that the part of the spinning die that is cut off is completely repaired by the cladding repair layer, and leaves a margin for subsequent grinding, thereby improving the repair accuracy.

[0041] In one embodiment, the step of placing the laser-clad spinning die into a heat-insulating environment until the cladding repair layer cools and solidifies includes: The spinning mold that has undergone laser cladding is embedded in insulating perlite for heat preservation until the cladding repair layer cools and solidifies.

[0042] Specifically, the spinning mold after laser cladding is embedded at least 100mm deep in insulating perlite and kept at that temperature for 24 hours before being removed and cooled to room temperature. At this point, the cladding repair layer has essentially solidified. Using insulating perlite to keep the laser-clad spinning mold warm effectively slows down the cooling rate of the cladding repair layer, ensuring uniform cooling and preventing internal stress and cracks caused by rapid cooling. This reduces performance differences due to uneven cooling, promotes the formation of a dense and uniform microstructure within the cladding repair layer, and effectively reduces the risk of oxidation and corrosion, thus significantly improving repair quality. If the spinning mold has not yet cooled to room temperature, it can be allowed to continue cooling in the ambient air to prepare for the grinding process, allowing the cladding repair layer to fully solidify during this cooling process.

[0043] In one embodiment, the step of grinding the cooled and solidified cladding repair layer to complete the repair of the spinning die includes: The cladding repair layer is ground using a white corundum grinding wheel to complete the repair of the spinning die.

[0044] Specifically, the white fused alumina grinding wheel has a grit size of 60 mesh and a hardness of L grade. The grinding speed is controlled between 140 and 180 mm / s. Compared to grinding wheels made of other materials, white fused alumina grinding wheels have higher hardness and grinding capacity, allowing for precise grinding of the cladding repair layer to reduce the roughness and unevenness of the spinning die surface. This significantly improves the surface finish of the spinning die, enhancing its geometric accuracy and dimensional stability, thus contributing to improved quality and performance. Furthermore, white fused alumina grinding wheels generate less heat during grinding, helping to reduce deformation and cracks caused by thermal stress, extending the die's service life. Moreover, white fused alumina grinding wheels do not produce toxic or harmful substances during grinding, making them more environmentally friendly and operator-friendly, thus improving operational safety.

[0045] Preferably, in the processing steps of S1 to S5, the laser cladding repair method of the spinning die of the present invention uses the double-top processing method with the same reference to process the spinning die, so as to improve the repair accuracy of the spinning die.

[0046] In one embodiment, after the step of grinding the cooled and solidified cladding repair layer to complete the repair of the spinning die, it further includes: Performing parameter detection on the spinning die to confirm whether the repaired spinning die is qualified.

[0047] Specifically, the parameter detection includes but is not limited to hardness detection, dimensional tolerance detection, surface finish detection and non-destructive detection. Among them, the non-destructive detection can adopt fluorescence detection and ultrasonic detection. If all parameters meet the original drawing design requirements of the spinning die, the repaired spinning die is qualified, otherwise it is unqualified.

[0048] Next, the repair process of three M031-type spinning dies to be repaired will be used as a specific example to demonstrate the laser cladding repair method of the spinning die of the present invention.

[0049] The base material of the M031-type spinning die to be repaired is Cr12MoV, the outer diameter size is 406.55 mm, the length is 1880 mm, and there are three pieces in total. After heat treatment, the surface hardness is 57-60 HRC. There are multiple axial scratches and fatigue cracks on the surface, resulting in its failure and inability to be used. It is required that the surface hardness after repair is ≥60 HRC, the effective cladding repair layer thickness is ≥0.5 mm, the surface finish reaches below RA0.4, and there are no defects such as cracks, pores, and poor fusion in the cladding repair layer. Other dimensions and geometric tolerances meet the drawing requirements.

[0050] Using the laser cladding repair method of the spinning die provided by the present invention for the three M031-type spinning dies to be repaired: Set the cutting amount, and cut the surface of the spinning die according to the cutting amount to remove the damaged layer of the spinning die to obtain a cutting surface.

[0051] The cutting amount is determined by the following formula: when A≤t, B = |f| + 2t; when A>t, B = |f| + 2A; where B is the cutting amount, f is the lower deviation value required for the diameter of the spinning die, t is the minimum functional layer thickness required for the spinning die, and A is the depth of the damaged layer of the spinning die.

[0052] In this embodiment, t is taken as 0.6 mm. At the same time, by querying the tolerance table, it can be known that the lower deviation value of the M031-type spinning die with an outer diameter size of 406.55 mm is -0.03 mm. The cutting amount parameters of the three M031-type spinning dies to be repaired are statistically shown in the following table: Table 1. Cutting Parameter Table serial number Type of damage Depth of damaged layer Judgment basis Cutting amount B <![CDATA[M01]]> Wear and damage <![CDATA[A1=0.4mm]]> <![CDATA[A1<t]]> <![CDATA[B1=|f|+2t=1.23mm]]> <![CDATA[M02]]> Surface fatigue cracks <![CDATA[A2=0.6mm]]> <![CDATA[A2=t]]> <![CDATA[B2=|f|+2t=1.23mm]]> <![CDATA[M03]]> Axial strain <![CDATA[A3=0.7mm]]> <![CDATA[A3>t]]> <![CDATA[B3=|f|+2A3=1.43mm]]> Based on the above cutting amount, the three M031 type spinning dies to be repaired were cut and the cutting surfaces were obtained.

[0053] Determine the preheating path and the cladding path on the cutting surface, wherein the preheating path includes the cladding path.

[0054] The preheating path includes the preheating start point. and preheating termination point The path to be clad includes the cladding starting point. and cladding termination point ;in, and The distance is 3-5mm. and The distance is 1 to 3 mm.

[0055] The preheating path is preheated, and after part of the path to be clad is preheated, laser cladding is performed on the path to be clad to obtain a cladding repair layer.

[0056] Before operating the heater, the preheating temperature is set to 190–210℃. Before operating the laser, the laser cladding parameters are set, including cladding linear speed, overlap ratio, laser power, and cladding thickness; specifically, the cladding linear speed is 20–50 mm / s, the overlap ratio is 35–55%, the laser power is 3000–5000 W, and the cladding thickness δ= q is a constant, ranging from 1.0 to 1.3 mm; in this example, it is set to 1.2 mm. The specific cladding parameters set in this embodiment are shown in the table below: Table 2. Cladding Parameters serial number linear velocity power Overlap rate cladding thickness <![CDATA[M01]]> 35mm / s 3500W 50% <![CDATA[δ1=1.215 <!-- 7 -->]]> <![CDATA[M02]]> 35mm / s 3500W 50% <![CDATA[δ2=1.215]]> <![CDATA[M03]]> 30mm / s 3700W 45% <![CDATA[δ3=1.315]]> Run the heater from the preheating start point s 起 Start towards the preheating termination point s 终 Move to preheat; when the heater exceeds the cladding start point a 起 When the distance is 1.5–3.5 mm, the laser operates from the cladding starting point a. 起 Start towards cladding termination point a 终 The device moves to perform laser cladding, and the heater moves at the same speed as the laser. The laser uses laser cladding powder to perform laser cladding on three spinning dies. The laser cladding powder is a low-carbon, high-chromium self-fluxing alloy powder, wherein the carbon content of the low-carbon, high-chromium self-fluxing alloy powder is 0.15-0.2%, and the chromium content is 17.5-19%.

[0057] The above steps were used to perform laser cladding on three M031 type spinning dies.

[0058] Three spinning dies that have undergone laser cladding are placed in an insulated environment until the cladding repair layer cools and solidifies.

[0059] Among them, the three M031 type spinning molds that have completed laser cladding were buried in insulating perlite for more than 100mm and kept at that temperature for 24 hours before being taken out and cooled to room temperature.

[0060] The cooled and solidified cladding repair layer is ground to complete the repair of the spinning die.

[0061] The cladding repair layer on the three M031 spinning dies was ground using white fused alumina grinding wheels with a grit size of 60 mesh and a hardness of L. The grinding speed was 150 mm / s, the rough grinding depth of cut was no more than 0.03 mm, and the fine grinding depth of cut was no more than 0.01 mm. This was done to ensure that the three M031 spinning dies met the dimensional tolerances and surface finish required by the drawings, thus obtaining three repaired M031 spinning dies.

[0062] Finally, parameter tests were performed on the three repaired M031 spinning dies to confirm whether the repaired M031 spinning dies were qualified.

[0063] In this embodiment, hardness, dimensional tolerances, and surface finish were tested according to the drawings, and non-destructive testing was performed according to the technical requirements or GJB-2376A-2005, GB / T 42401-2023, and GB / T 5777-2019 U1 level. The parameter test results are shown in the table below: Table 3. Parameter Testing Table

[0064] According to the test results, the hardness, dimensional tolerances, surface finish, and non-destructive testing of the three repaired M031 spinning dies all meet the repair requirements. The surface and interior of the cladding repair layer are free of cracks, porosity, and incomplete fusion, which would affect the quality of the cladding repair layer. Therefore, all three repaired M031 spinning dies are qualified. Furthermore, through machine testing of the three qualified repaired M031 spinning dies, it was found that the service life of the repaired M031 spinning dies is 30%–35% longer than the original spinning dies. They can also be cyclically repaired, the repair process is stable and reliable, and the quality is controllable, greatly improving the recycling rate of spinning dies and reducing the scrap cost of spinning dies.

[0065] The above embodiments are preferred implementations of the present invention. In addition, the present invention can be implemented in other ways. Any obvious substitutions without departing from the concept of the present technical solution are within the protection scope of the present invention.

Claims

1. A laser cladding repair method for spinning molds, It is characterized in that The following steps are involved: Setting a cutting amount, cutting the surface of the spinning mold according to the cutting amount, and removing a damaged layer of the spinning mold to obtain a cutting surface; Determining a preheating path and a path to be clad on the cutting surface, wherein the preheating path includes the path to be clad; Preheating the preheating path, and starting laser cladding on the path to be clad after a portion of the path to be clad has completed preheating, so as to obtain a cladding repair layer; Placing the laser cladding-finished spinning mold in a heat preservation environment until the cladding repair layer is cooled and solidified; The cooled and solidified cladding repair layer is ground to complete the repair of the spinning mold.

2. The laser cladding repair method for a spinning die according to claim 1, It is characterized in that In the step of setting the cutting amount, cutting the surface of the spinning mold according to the cutting amount, and removing the damaged layer of the spinning mold to obtain the cutting surface, the cutting amount is determined by the following formula: When A≤t, B=|f|+2t; When A>t, B=|f|+2A; Among them, B is the cutting amount, f is the lower deviation value required for the spinning mold diameter, t is the minimum functional layer thickness required for the spinning mold, and A is the depth of the damaged layer of the spinning mold.

3. The laser cladding repair method for a spinning mold according to claim 2, It is characterized in that The preheating path includes a preheating starting point s 起 and preheating end point s 终 The path to be clad includes a cladding starting point a 起 and cladding end point a 终 ; Among them, s 起 with a 起 The distance is 3 to 5 mm, a 终 With s 终 The distance is 1 to 3 mm.

4. The laser cladding repair method for a spinning mold according to claim 3, It is characterized in that The step of preheating the preheating path and starting laser cladding on the path to be clad after a portion of the path to be clad has completed preheating to obtain a cladding repair layer includes: Run the heater from the preheat starting point 起 Start to warm up to the end point s 终 Move to warm up; When the heater moves beyond the cladding starting point a 起 When the distance is 1.5 to 3.5 mm, run the laser from the cladding starting point a 起 Start to the cladding end point a 终 The heater moves to perform laser cladding, and the moving speed of the heater is consistent with that of the laser.

5. The laser cladding repair method for a spinning die according to claim 4, It is characterized in that Before the step of preheating the preheating path and starting laser cladding the path to be clad after part of the path to be clad has completed preheating to obtain a cladding repair layer, the step further includes: Before the heater is operated, the preheating temperature of the heater is set to 190-210°C.

6. The laser cladding repair method for a spinning mold according to claim 4, It is characterized in that Before the step of preheating the preheating path and starting laser cladding the path to be clad after part of the path to be clad has completed preheating to obtain a cladding repair layer, the step further includes: Before the laser is operated, the cladding parameters of the laser are set, and the cladding parameters include cladding line speed, overlap rate, laser power and cladding thickness; wherein the cladding line speed is 20-50 mm / s, the overlap rate is 35-55%, the laser power is 3000-5000 W, and the cladding thickness δ= , q is a constant, ranging from 1.0 to 1.3 mm.

7. The laser cladding repair method for a spinning mold according to claim 4, Features The laser uses low-carbon high-chromium self-fluxing alloy powder to perform laser cladding on the spinning mold, wherein the carbon content of the low-carbon high-chromium self-fluxing alloy powder is 0.15-0.2% and the chromium content is 17.5-19%.

8. The laser cladding repair method for a spinning mold according to claim 1, It is characterized in that The step of placing the spinning mold after laser cladding into a heat preservation environment until the cladding repair layer is cooled and solidified comprises: The entire spinning mold that has completed laser cladding is buried in heat-insulating perlite for heat preservation until the cladding repair layer is cooled and solidified.

9. The laser cladding repair method for a spinning mold according to claim 1, It is characterized in that The step of grinding the cooled and solidified cladding repair layer to complete the repair of the spinning mold includes: The cladding repair layer is ground using a grinding wheel made of white corundum to complete the repair of the spinning mold.

10. The laser cladding repair method for a spinning mold according to claim 1, It is characterized in that After the step of grinding the cooled and solidified cladding repair layer to complete the repair of the spinning mold, the method further includes: The spinning mold is subjected to parameter detection to confirm whether the repaired spinning mold is qualified.

Citation Information

Cited By

  • Gradient metal ceramic coating repairing method based on laser directional energy deposition

    CN121514526A