Preparation method and application of electrocatalyst for preparing oxygen from carbon dioxide
Through rapid high-temperature roasting and secondary carbonization, combined with high electronegativity regulation of oxygen elements, the problem of insufficient efficiency and number of sites of carbon dioxide oxygen-generating electrocatalysts is solved, and a high-performance iron-based electrocatalyst is prepared, suitable for Mars Electric reduction of carbon dioxide in special environments to generate oxygen.
Patent Information
- Application Number
- CN202411089408.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-29
AI Technical Summary
The existing electrocatalysts for carbon dioxide oxygen production face the problems of low Faraday efficiency, small number of active sites, and poor electron transfer efficiency, especially the loss of lattice oxygen in the carbon support during high-temperature roasting affects the formation of oxygen coordination.
The carbon support is prepared by rapid high-temperature calcination combined with secondary carbonization, and induces the iron-based precursor to form coordination bonds between the oxygen elements in the carbon support in an inert atmosphere, and uses the high electronegativity of the oxygen elements to regulate the electronic properties of the active center. , by selecting water-soluble organic and inorganic substances as carbon sources and template agents, the process parameters of calcination and secondary carbonization are controlled, and the degree of graphitization and lattice oxygen content of the carbon carrier are improved.
The Faraday efficiency, number of active sites and electron transfer efficiency of the electrocatalyst are improved, and a high-performance iron-based electrocatalyst for carbon dioxide oxygen production is prepared, which is suitable for electroreduction of carbon dioxide in environments such as Mars and other countries with abundant carbon dioxide but scarce resources to generate oxygen.
Smart Images

Figure CN119040937A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of catalytic conversion of carbon dioxide, and in particular, relates to a preparation method and application of an electrocatalyst for producing oxygen from carbon dioxide. Background Art
[0002] As a compound rich in carbon and oxygen, carbon dioxide has great application potential in the fields of chemical production and aerospace. Oxygen has high practical value and is widely used in medical rescue, aircraft propellants, etc. For special environments such as the surface of Mars where carbon dioxide is relatively abundant but other resources are relatively scarce, the electro-reduction reaction of carbon dioxide to generate oxygen has high research value and practical significance. However, due to the stable chemical properties of carbon dioxide, the electro-reduction reaction of carbon dioxide requires the assistance of high-performance catalysts. In addition, the electro-reduction process of carbon dioxide is also affected by the competitive hydrogen evolution reaction. Therefore, the development of high-performance catalysts is of great significance to the development of the field of carbon dioxide to oxygen.
[0003] At present, iron-based catalysts have gradually become a research hotspot for carbon dioxide to oxygen electrocatalysts due to their advantages of low cost, high activity and abundant raw material sources. In terms of iron-based active raw materials, iron porphyrin (Fe-Por) is widely used as an active metal precursor for carbon dioxide to oxygen electrocatalysts, but its planar four-coordinated Fe-N4 centrosymmetric electron configuration affects the carbon dioxide to oxygen process. Nitrogen coordination modification is a traditional strategy to improve the performance of Fe-N4 active sites. Compared with nitrogen, the more electronegative oxygen element provides a new idea for improving the performance of Fe-N4 active sites.
[0004] In order to improve the conductivity and electron transfer efficiency of the catalyst, the carbon material used as the electrocatalyst carrier needs to be carbonized at a relatively high temperature (>600°C). However, when the calcination temperature is too high (>500°C), the lattice oxygen in the carbon material will be lost with the adjacent carbon atoms in the form of carbon monoxide or carbon dioxide, thereby affecting the formation of oxygen coordination. This also leads to great difficulties in the specific implementation of the oxygen coordination modification strategy at this stage. In addition, the small number of active sites and low electron transfer efficiency of traditional catalysts also limit the overall performance of the catalyst. Therefore, how to solve the problems of low Faraday efficiency, small number of active sites, and poor electron transfer efficiency faced by traditional catalysts on the basis of solving the problem that the oxygen coordination modification strategy is difficult to implement is the key to preparing high-performance carbon dioxide to oxygen electrocatalysts.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide a method for preparing an electrocatalyst for producing oxygen from carbon dioxide and its application, which can improve the Faraday efficiency, the number of active sites and the electron transfer efficiency of the obtained electrocatalyst, and improve the performance of the electrocatalyst.
[0007] In order to solve the above technical problems, the basic concept of the technical solution adopted by the present invention is:
[0008] A method for preparing an electrocatalyst for producing oxygen from carbon dioxide comprises the following steps:
[0009] (1) using an oxygen-containing and water-soluble organic substance as a carbon source and an inorganic substance that is water-soluble as a template, grinding the carbon source and the template together to form a mixture, heating the mixture to a calcination temperature under an inert gas atmosphere and maintaining the temperature, and then cooling the mixture to room temperature to complete the calcination process;
[0010] (2) washing the calcined mixture, drying it, and then heating it to a secondary carbonization temperature under an inert gas atmosphere and maintaining the temperature, and then cooling it to room temperature to complete the secondary carbonization process to obtain a carbon carrier; wherein the secondary carbonization temperature is lower than the calcination temperature;
[0011] (3) dispersing the carbon support in a solvent to obtain a solution A;
[0012] (4) dispersing the iron-based precursor in a solvent to obtain a solution B;
[0013] (5) adding solution B dropwise to the continuously stirred solution A to form solution C. After solution C is stirred for a period of time, solid-liquid separation is performed to obtain a black mixture;
[0014] (6) After the black mixture is washed and dried, it is heated to an induction temperature and maintained under an inert gas atmosphere, and then cooled to room temperature to obtain an oxygen-coordinated modified electrocatalyst for converting carbon dioxide into oxygen.
[0015] In the above scheme, the term "easily soluble in water" means that under standard conditions (usually 20° C. and 1 standard atmospheric pressure), the mass of the substance that can be dissolved in 100 g of water is greater than 10 g.
[0016] The degree of graphitization of the carbon carrier affects the conductivity of the carbon carrier and the electron transfer efficiency of the electrocatalyst. High-temperature calcination in an inert atmosphere is beneficial to improving the degree of graphitization of the carbon carrier. However, long-term high-temperature calcination will cause the lattice oxygen in the carbon material and the adjacent carbon atoms to be lost in the form of carbon monoxide or carbon dioxide, thereby affecting the formation of oxygen coordination.
[0017] In the present invention, the carbon source is firstly rapidly calcined at a relatively high temperature, so that the carbon carrier has a higher degree of graphitization while avoiding the influence of high temperature calcination on the lattice oxygen content of the carbon carrier. Afterwards, a relatively low temperature is used for secondary carbonization treatment, and the degree of graphitization of the carbon carrier is further improved while avoiding the problem of lattice oxygen loss in the carbon carrier. By combining the method of rapid high temperature calcination with secondary carbonization, a carbon carrier with both a higher lattice oxygen content and a higher degree of graphitization is prepared.
[0018] Subsequently, under a high-temperature inert atmosphere, the iron species in the iron-based precursor are induced to form coordination bonds with the oxygen element in the carbon carrier, thereby preparing an oxygen-coordinated modified high-performance iron-based electrocatalyst for producing oxygen from carbon dioxide.
[0019] Oxygen element has a high electronegativity, and oxygen coordination modification can have a good regulatory effect on the electronic properties of the catalytic active center. The lattice oxygen content in the carbon carrier affects the formation of coordination bonds between oxygen elements and active species, and thus affects the regulatory effect of oxygen coordination modification on the electronic properties of the catalytic active center. In the present invention, the carbon source needs to be an organic matter containing oxygen element, preferably an organic matter rich in oxygen element, so that the lattice oxygen content in the prepared carbon carrier is relatively high, and it is suitable as an electrocatalyst carrier in the process of preparing high-performance electrocatalysts for producing oxygen from carbon dioxide using the oxygen coordination modification strategy.
[0020] The rapid calcination process easily causes uneven graphitization of the carbon source, thereby affecting the electron transfer efficiency of the carbon carrier and the electrocatalyst. In the present invention, the carbon source is selected from organic matter that is easily soluble in water, and the calcined product can be cleaned to remove substances with a low degree of carbonization and substances that have not been carbonized in time, so as to achieve the purpose of improving the overall graphitization uniformity of the carbon carrier. After cleaning, a secondary carbonization treatment is performed to obtain a carbon carrier with a further improved degree of graphitization.
[0021] The specific surface area of the carbon carrier and the electrocatalyst will affect the contact effect between the reaction gas and the active sites during the reaction, thereby affecting the performance of the electrocatalyst. The use of a template agent to assist in the preparation process is an effective means to increase the specific surface area of the material, but the participation of the template agent often leads to an increase in the impurity content in the material, thereby affecting the performance of the catalyst. In the present invention, the template agent uses an inorganic substance that is easily soluble in water, which is easy to remove by washing after calcination. At the same time, the use of a substance with good high-temperature thermal stability as a template agent can further reduce the introduction of impurities.
[0022] On the other hand, relative to precious metals, transition metals represented by Fe, Co, and Ni have the advantages of low cost, high earth content, and easy access. Among transition metal-based carbon dioxide electroreduction catalysts, iron-based catalysts have the highest intrinsic activity. Therefore, in the present invention, iron-based materials are selected as catalysts for carbon dioxide electroreduction reactions.
[0023] In a further embodiment, in step (1), the carbon source comprises at least one of L-alanine, lysine, tyrosine, tryptophan, phenylalanine, serine, leucine, proline, isoleucine, glutamic acid, aspartic acid, valine and arginine, preferably L-alanine.
[0024] In the above scheme, the listed various compounds all contain a large amount of oxygen elements, and are used as carbon sources, so that the prepared carbon carrier has a high lattice oxygen content. At the same time, the above various compounds are all soluble in water, and after the roasting process, it is easy to wash and remove the uncarbonized and low-carbonized components, thereby ensuring the uniformity of graphitization of the entire carbon carrier.
[0025] In order to increase the lattice oxygen content in the carbon carrier, in addition to using a rapid high-temperature calcination method to avoid lattice oxygen loss, the present invention also uses a rapid calcination method to test a variety of organic substances. After testing, it was found that the carbon carrier prepared by using L-alanine containing a large amount of oxygen as a carbon source has a higher lattice oxygen content, and is suitable for use as a carrier of the electrocatalyst in the preferred scheme of preparing high-performance electrocatalysts for producing oxygen from carbon dioxide using the oxygen coordination modification strategy.
[0026] In addition, during the carbonization process, the polymerization of carbon source molecules and the growth and extension of carbon materials are beneficial to the loading of iron-based precursors and the increase in the number of catalyst active sites. The atomic arrangement of L-alanine molecules theoretically has a structure that is beneficial to the molecular polymerization during the carbonization process, which can then promote the growth and extension of carbon materials. In the present invention, it was found through experiments that the use of L-alanine as a carbon source has better performance of the obtained electrocatalyst, achieving the purpose of carbon material growth and extension during the carbonization process of the carbon source.
[0027] In a further embodiment, in step (1), the template comprises at least one of potassium carbonate, potassium carbonate, sodium chloride and potassium chloride, preferably potassium carbonate.
[0028] In the above scheme, potassium carbonate has a melting point of 891°C, has good high temperature thermal stability, is easily soluble in water, and is easily removed by washing after being fully mixed with the carbon source and undergoing a roasting process. In the preferred scheme of the present invention, potassium carbonate is used as a template agent, which can effectively increase the specific surface area of the carbon carrier while avoiding the introduction of impurities.
[0029] In a further embodiment, in step (1), the mass ratio of the template to the carbon source is 1:1 to 10:1, preferably 3:1 to 4:1, and more preferably 3:1.
[0030] In the above scheme, if the amount of template used is too high, it will affect the cross-linking process of the carbon source and the growth and extension of the carbon material during the carbonization process; if the amount of template used is too low, the specific surface area of the carrier and the catalyst will be reduced. In the present invention, after many experiments, it was found that the mass ratio of the template to the carbon source is controlled at 1:1 to 10:1, and the performance of the obtained electrocatalyst is better. The optimal mass ratio of the template to the carbon source is 3:1, and the electrocatalyst obtained at this time has the best performance.
[0031] As a specific implementation, in step (1), the carbon source and the template are fully ground in proportion to form a uniform mixture, and then a subsequent calcination treatment is performed.
[0032] In a further embodiment, in step (1), the calcination temperature is 900-1200° C., preferably 950-1000° C., and more preferably 1000° C.; the holding time at the calcination temperature is 1-10 min, and preferably 5 min;
[0033] Preferably, the temperature is increased to the calcination temperature at a heating rate of 30 to 70°C / min, and the heating rate is preferably 30 to 50°C / min, more preferably 50°C / min;
[0034] The temperature is lowered from the calcination temperature to room temperature at a cooling rate of 20 to 70° C. / min, and the cooling rate is preferably 50° C. / min.
[0035] In the present invention, firstly, a mixture of a carbon source and a template agent is rapidly calcined at a high temperature. During the calcination process, the calcination temperature, the holding time, and the control of the heating and cooling rates are beneficial to improving the performance of the obtained electrocatalyst. If the heating and cooling rates are too fast, or the holding time at the calcination temperature is too short, the graphitization degree of the carbon source and the yield of the carbon carrier will be affected; and if the heating and cooling rates are too slow, or the holding time at the calcination temperature is too long, the lattice oxygen content in the carbon carrier will be reduced.
[0036] After many experiments, it was found that the above-defined parameter range is conducive to obtaining electrocatalysts with better performance. Among them, the optimal process conditions during the calcination process are: heating rate of 50℃ / min, calcination temperature of 1000℃, holding time of 5min, and cooling rate of 50℃ / min.
[0037] In a further embodiment, in step (1), the inert gas used in the calcination process is at least one of argon, nitrogen, helium and neon, preferably argon.
[0038] High temperature calcination in an inert gas atmosphere can prevent the carbon carrier from introducing new impurities during the carbonization process. Among them, argon has the advantages of being stable in nature and preventing the carbon carrier from introducing new impurities during the carbonization process. Therefore, in the preferred embodiment of the present invention, argon is selected as the inert gas.
[0039] As a specific implementation method, in step (1), the obtained mixture is placed in a tubular furnace in an inert gas atmosphere, heated to 900-1200°C at a heating rate of 30-70°C / min, maintained for 1-10 minutes, and then cooled to room temperature at a cooling rate of 20-70°C / min, thereby completing the roasting process.
[0040] In a further embodiment, in step (2), the calcined mixture is washed with a mixed solution of ethanol and water;
[0041] Preferably, the volume ratio of water to ethanol is 1:1 to 5:1, preferably 2:1.
[0042] In the above scheme, the cleaning operation can remove the template and the carbon source with a lower degree of carbonization, thereby preventing the carbon source and the template from bringing impurities to the carbon carrier and the catalyst. Among them, the template can be removed by cleaning with pure water, but the polarity of pure water is relatively high. When cleaning the carbon material after high-temperature roasting and carbonization, the hydroxyl content on the surface of the material will be increased, thereby affecting the load of the iron source on the surface of the carbon carrier in the subsequent preparation process, and the performance of the obtained electrocatalyst. The present invention adds a certain proportion of ethanol to water to reduce the polarity of the solution and avoid the above problems. After multiple tests, it was found that the volume ratio of water to ethanol was controlled in the range of 1:1 to 5:1, with a good cleaning effect, wherein the optimal volume ratio of water to ethanol is 2:1.
[0043] In a further embodiment, in step (2), the washed mixture is dried at 90-200°C, preferably at 90-120°C, more preferably at 120°C; the drying time is 10-30h, preferably 20-30h, more preferably 20h.
[0044] As a specific implementation manner, the cleaned mixture is transferred to an oven for drying, and the drying temperature of the oven is controlled to be 90 to 200° C., and the drying time is 10 to 30 hours.
[0045] In the above scheme, if the drying temperature is too high, the volatilization rate of free water will be too fast, thereby affecting the stability of the carbon support and the electrocatalyst structure. If the drying temperature is too low, the removal effect of free water will be affected.
[0046] In a further embodiment, in step (2), the secondary carbonization temperature is 400-450° C., preferably 400° C.; the holding time at the secondary calcination temperature is 1-5 h, preferably 2-3 h, more preferably 2 h;
[0047] Preferably, the temperature is increased to the secondary carbonization temperature at a heating rate of 1 to 10°C / min, and the heating rate is preferably 5 to 10°C / min, more preferably 5°C / min;
[0048] Cooling from the secondary calcination temperature to room temperature at a cooling rate of 5 to 20°C / min, preferably 10°C / min;
[0049] Preferably, the inert gas used in the secondary carbonization process is at least one of argon, nitrogen, helium and neon, preferably argon.
[0050] In the above scheme, the secondary low-temperature carbonization method is adopted to further improve the graphitization degree of the carbon carrier while avoiding the loss of lattice oxygen in the carbon carrier. Multiple process parameters in the secondary carbonization process will have an important impact on the performance of the electrocatalyst. Specifically, if the heating and cooling rates are too fast, or the secondary carbonization temperature is too low or the holding time is too short, the carbonization degree of the carbon carrier will be affected, and then the performance of the electrocatalyst will be affected; and if the heating and cooling rates are too slow, or the secondary carbonization temperature is too high or the holding time is too long, the lattice oxygen content in the carbon carrier will be reduced.
[0051] In the present invention, after many experiments, it was found that controlling the various process parameters involved in the secondary carbonization process within the above-mentioned specified range is conducive to obtaining an electrocatalyst with better performance. Among them, the optimal process conditions in the secondary carbonization process are: a heating rate of 5°C / min, a secondary carbonization temperature of 400°C, a holding time of 2h, and a cooling rate of 10°C / min.
[0052] Carrying out the secondary carbonization reaction under an inert gas atmosphere can reduce the possibility of side reactions and avoid the introduction of new impurities. Among various inert gases, argon has the most stable properties.
[0053] As a specific implementation method, the material dried in the oven is transferred to a tubular furnace in an inert gas atmosphere, heated to 400-450°C at a heating rate of 1-10°C / min, maintained for 1-5 hours, and then cooled to room temperature at a cooling rate of 5-20°C / min, thereby completing the secondary carbonization process.
[0054] In a further embodiment, in step (3), the mass ratio of the carbon support to the solvent is 1:5 to 1:15, preferably 1:10 to 1:12, and more preferably 1:10;
[0055] Preferably, the carbon carrier is mixed with the solvent and then subjected to ultrasonic treatment to obtain solution A; the temperature of the ultrasonic treatment is 20 to 70° C., preferably 30° C.; the duration of the ultrasonic treatment is 1 to 10 h, preferably 5 h.
[0056] In the above scheme, if the mass ratio of the carbon carrier to the solvent is too high, or the temperature of the ultrasonic treatment is too low, or the treatment time is too short, the dispersion of the carbon carrier in the solvent will be affected, which is not conducive to subsequent reactions. If the mass ratio of the carbon carrier is too low, or the temperature of the ultrasonic treatment is too high, or the treatment time is too long, the stability of the carbon carrier structure will be affected. Both of the above situations are not conducive to obtaining electrocatalysts with better performance.
[0057] In a further embodiment, in step (3), the solvent used to disperse the carbon carrier includes at least one of N,N-dimethylformamide, ethanol, carbon tetrachloride, ether, n-hexane, and chloroform, preferably N,N-dimethylformamide.
[0058] In the above scheme, compared with other solvents, N,N-dimethylformamide has the least effect on the polarity and physicochemical properties of the carbon carrier, and is therefore the preferred solvent for dispersing the carbon carrier.
[0059] In a further embodiment, in step (4), the iron-based precursor is iron porphyrin, and the mass ratio of iron porphyrin to solvent is 1:15 to 1:25, preferably 1:15 to 1:20, and more preferably 1:20;
[0060] Preferably, the iron-based precursor is mixed with a solvent and then subjected to ultrasonic treatment to obtain a solution B; the temperature of the ultrasonic treatment is 20 to 70° C., preferably 30° C.; the duration of the ultrasonic treatment is 1 to 10 h, preferably 5 h.
[0061] The regulation of the electronic properties of the active site is an effective means to improve the performance of the catalyst. The planar Fe-N4 coordination structure in iron porphyrin (Fe-Por) provides additional coordination sites in the axial direction, which indicates that suitable axial coordination can adjust the symmetrical electronic arrangement of the active center, thereby improving the performance of the catalyst. Therefore, the scheme of the present invention uses iron porphyrin as an iron-based precursor.
[0062] If the mass ratio of iron porphyrin to solvent is too high, or the temperature of ultrasonic treatment is too low, or the treatment time is too short, the dispersion of iron porphyrin will be affected. If the mass ratio of iron porphyrin is too low, or the temperature of ultrasonic treatment is too high, or the treatment time is too long, the structural stability of iron porphyrin will be affected. Both of the above situations will affect the performance of the final electrocatalyst.
[0063] In a further embodiment, in step (4), the solvent used to disperse the iron-based precursor includes at least one of N,N-dimethylformamide, ethanol, carbon tetrachloride, ether, n-hexane, and chloroform, preferably N,N-dimethylformamide.
[0064] In the above scheme, compared with other solvents, the solubility of iron porphyrin in N,N-dimethylformamide solution is the highest, so N,N-dimethylformamide is used as the preferred solvent for dispersing iron porphyrin.
[0065] In a further embodiment, in step (5), the mass ratio of solution A to solution B is 1:1 to 5:1, preferably 3:1;
[0066] Solution C is continuously stirred at 20-70° C. for 5-20 h, preferably at 30° C., and preferably for 10 h.
[0067] As a specific implementation, solution B is added dropwise into solution A which is continuously stirred to form solution C, and then solution C is continuously stirred at 20 to 70° C. for 5 to 20 hours, and then filtered to obtain a black mixture.
[0068] In the above scheme, if the mass ratio of solution A to solution B is too high, that is, the amount of iron-based precursor added is too small compared to the carbon carrier, or the stirring temperature is too low, and the stirring time is too short, it will affect the loading effect of the iron-based active sites, thereby reducing the number of active sites of the electrocatalyst. If the mass ratio of solution A to solution B is too low, it is equivalent to increasing the concentration of the iron-based precursor in solution C, which will reduce the dispersion of the iron-based active sites. If the stirring temperature is too high or the stirring time is too long, it will affect the structural stability of the carbon carrier and iron porphyrin.
[0069] In a further embodiment, in step (6), the cleaning liquid used to clean the black mixture includes at least one of N,N-dimethylformamide, ethanol, carbon tetrachloride, ether, n-hexane, and chloroform, preferably N,N-dimethylformamide.
[0070] As a specific implementation, the solvents used in step (3) and step (4), and the cleaning solution used in step (6) are all composed of the same ingredients.
[0071] In a further embodiment, in step (6), the washed black mixture is vacuum dried at a temperature of 50 to 90° C., preferably 60° C., and a drying time of 10 to 30 hours, preferably 20 hours.
[0072] Compared with traditional atmospheric pressure drying, vacuum drying can reduce the aggregation and growth of iron-based active species on the surface of carbon carriers and improve the stability and dispersion of iron-based active species. If the vacuum drying temperature is too high or the drying time is too long, it will also cause the aggregation and growth of iron-based active species on the surface of carbon carriers, thereby affecting the stability and dispersion of iron-based active species. If the vacuum drying temperature is too low or the drying time is too short, it will affect the removal effect of the cleaning solution.
[0073] As a specific implementation method, the black mixture obtained in step (5) is washed with a washing liquid until the washing liquid becomes colorless, and the washing is completed; then the mixture is transferred to a vacuum drying oven at 50 to 90° C. and dried for 10 to 30 hours; then the mixture is transferred to a tubular furnace and calcined in an inert gas atmosphere.
[0074] In a further embodiment, in step (6), the induction temperature is 350-400° C., preferably 400° C.; the holding time at the induction temperature is 1-5 h, preferably 2 h;
[0075] Preferably, the temperature is increased to the induction temperature at a heating rate of 1 to 10°C / min, preferably 5°C / min; the temperature is decreased from the induction temperature to room temperature at a cooling rate of 5 to 20°C / min, preferably 10°C / min.
[0076] The formation of coordination bonds and changes in the microstructure of active sites require the assistance of external energy. In the present invention, the carbon carrier loaded with an iron-based precursor is calcined in a high-temperature inert atmosphere to induce the iron species in the iron-based precursor to form coordination bonds with the oxygen element in the carbon carrier, thereby preparing an oxygen-coordinated modified high-performance electrocatalyst for producing oxygen from carbon dioxide.
[0077] If the induction temperature of the calcination is too low, or the heating and cooling rates are too fast, the formation of coordination bonds between the iron species in the iron-based precursor and the oxygen elements in the carbon carrier will be affected. If the induction temperature is too high, or the heating and cooling rates are too slow, the lattice oxygen in the carbon carrier will be lost, and the stability of the carbon carrier structure will be affected, thereby affecting the performance of the electrocatalyst.
[0078] In the present invention, the carbon support loaded with the iron-based precursor is heated to 350-400°C at a heating rate of 1-10°C / min, maintained for 1-5h, and then cooled to room temperature at a cooling rate of 5-20°C / min, so as to obtain an electrocatalyst with better performance.
[0079] As a specific implementation method, the cleaned and dried black mixture is placed in a tubular furnace under an inert gas atmosphere, heated to 350-400°C at a heating rate of 1-10°C / min, maintained for 1-5 hours, and then cooled to room temperature at a cooling rate of 5-20°C / min to obtain an oxygen-coordinated modified carbon dioxide electrocatalyst for producing oxygen.
[0080] In a preferred embodiment, the inert gas used in step (6) is at least one of argon, nitrogen, helium and neon, preferably argon.
[0081] In the process of preparing electrocatalysts by calcining carbon carriers loaded with iron-based precursors, the calcination atmosphere, especially small molecules such as free oxygen molecules and water molecules in the calcination environment, will affect the directional changes in the microstructure of the active sites. The use of inert gas can prevent the redox properties in the calcination atmosphere from affecting the stability of the carbon carrier and catalyst structure. Compared with other gases, argon is more stable and more conducive to maintaining an inert atmosphere during the calcination process, thereby reducing the possibility of side reactions to a greater extent and ensuring that the prepared electrocatalyst has better performance.
[0082] In the present invention, a carbon carrier loaded with an iron-based precursor is calcined in an inert atmosphere filled with argon, and experiments are carried out at different induction temperatures. It is found that when the induction temperature is 400°C and under an argon atmosphere, the iron species in the iron-based precursor can be more effectively induced to form coordination bonds with the oxygen elements in the carbon carrier, thereby inducing the formation of axial oxygen coordination at the iron-based active sites.
[0083] The present invention also provides an application of an electrocatalyst prepared by the above-mentioned method for preparing an electrocatalyst for producing oxygen from carbon dioxide in catalyzing the production of oxygen from carbon dioxide.
[0084] After adopting the above technical scheme, the present invention has the following beneficial effects compared with the prior art.
[0085] 1. The scheme of the present invention solves the problems of low oxygen Faraday efficiency, small number of active sites, low electron transfer efficiency, etc. faced by traditional catalysts for converting carbon dioxide into oxygen by adopting the strategy of regulating active sites through oxygen coordination, and provides a new idea for preparing high-performance iron-based electrocatalysts for converting carbon dioxide into oxygen by using the oxygen coordination modification strategy; at the same time, it also plays a certain demonstration role in the preparation of new single-atom catalysts with adjustable local environment for application in other fields.
[0086] 2. Compared with traditional nitrogen coordination regulation, the scheme of the present invention, with the help of the relatively higher electronegativity of oxygen element, adopts the strategy of oxygen coordination regulation to solve the problem of low oxygen Faraday efficiency faced by electrocatalysts for converting carbon dioxide into oxygen; at the same time, by utilizing the relatively higher electronegativity of oxygen element, the oxygen coordination structure is easier to form, which improves the success rate of preparing iron-based catalysts with oxygen coordination structure and reduces the difficulty of catalyst preparation.
[0087] 3. A new type of carbon carrier is prepared by combining rapid high-temperature calcination with secondary carbonization, which solves the problem that the carbon carrier prepared by the traditional long-term high-temperature calcination method is difficult to have both a high lattice oxygen content and a high degree of graphitization; by using a carbon carrier with both a high lattice oxygen content and a high degree of graphitization, and calcining the carbon carrier loaded with an iron-based precursor in an inert atmosphere, the problem of low electron transfer efficiency faced by traditional catalysts for producing oxygen from carbon dioxide is solved.
[0088] 4. In the calcination and carbonization process of the carbon source, inorganic substances with high temperature stability and easy solubility in water are used as templates. Under the premise of avoiding the introduction of impurities, the problem of small specific surface area of carbon carriers and catalysts is solved; by using carbon carriers with larger specific surface area, the number of attachment points of active sites on the surface of the carbon carrier is increased, and the iron-based precursor is loaded on the surface of the carbon carrier by combining the excessive impregnation method, which solves the problem of small number of active sites of traditional catalysts.
[0089] 5. By calcining the carbon carrier loaded with iron-based precursors in an inert atmosphere, the iron species in the iron-based precursors are induced to form coordination bonds with the lattice oxygen in the carbon carrier. The higher electronegativity of oxygen is utilized to adjust the microstructure and electronic arrangement of the active center. By regulating the distance between the electronic center and the Fermi level, the problem of low Faraday efficiency of oxygen production by traditional catalysts is solved.
[0090] 6. The kingfisher jadeite Aji prepared by the scheme of the present invention can be applied to the reaction of carbon dioxide electroreduction to generate oxygen. For special environments such as the surface of Mars where carbon dioxide is relatively abundant but other resources are relatively scarce, the process of carbon dioxide electroreduction to generate oxygen can play a key role in the construction of propulsion systems, life support, medical rescue, etc., and thus has high research value and practical significance for the development of deep space exploration, in-situ utilization of extraterrestrial resources, and confined space carbon dioxide purification and life system maintenance.
[0091] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0092] The accompanying drawings are part of the present invention and are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention, but do not constitute an improper limitation of the present invention. Obviously, the drawings described below are only some embodiments. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. In the accompanying drawings:
[0093] Figure 1 The performance and stability test results of the electrocatalyst in Example 1 of the present invention;
[0094] Figure 2 is a scanning electron microscope (SEM) image of the carbon support in Examples 1 and 2 of the present invention;
[0095] Figure 3 is the O1s XPS graph of the carbon support in Example 1 of the present invention and Comparative Example 1;
[0096] Figure 4 is the spherical aberration electron microscopy characterization result of the electrocatalyst in Examples 1 and 2 of the present invention;
[0097] Figure 5 is a BET graph of the electrocatalysts in Examples 1 and 2 of the present invention;
[0098] Figure 6 are the O1s XPS characterization results of the electrocatalysts in Example 1 of the present invention and Comparative Example 1;
[0099] Figure 7 It is the Fe 2p XPS characterization result of the electrocatalyst in Example 1 of the present invention and Comparative Example 1;
[0100] Figure 8 These are the performance test results of the electrocatalysts in Examples 1 and 2 of the present invention and Comparative Example 1.
[0101] It should be noted that these drawings and textual descriptions are not intended to limit the conceptual scope of the present invention in any way, but are intended to illustrate the concept of the present invention for those skilled in the art by referring to specific embodiments. DETAILED DESCRIPTION
[0102] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. The following embodiments are used to illustrate the present invention but are not used to limit the scope of the present invention.
[0103] It should be noted that in the embodiments and comparative examples of the present invention, the test instruments and test methods used are specifically as follows:
[0104] The element contents were tested using an ICP-AES instrument (Shimadzu ICPS-7500);
[0105] Scanning electron microscopy (SEM) characterization A JEM-2010F instrument was used to analyze the catalyst surface morphology;
[0106] The specific surface area test (BET) was conducted using the Autosorb-iQ fully automatic specific surface area and pore size distribution analyzer from Quantachrome, USA. The N2 adsorption-desorption curve was measured in a liquid nitrogen atmosphere, the specific surface area was calculated according to the BET equation, and the pore structure data was estimated according to the BJH model.
[0107] X-ray diffraction (XRD) characterization was performed using a Gigaku XRD-6000 diffractometer with a scanning speed of 10° / min and a scanning range of 10° to 90°;
[0108] The H2-TPR test was performed using a Micromeritics ChemisSorb 2720 instrument with a thermal conductivity detector (TCD) in the test range of 25°C to 900°C.
[0109] Furthermore, the catalytic performance of the electrocatalyst was tested using the following method.
[0110] The CO2 electrochemical reduction reaction test was performed by linear sweep voltammetry (LSV) in a CO2-saturated 0.1M NaHCO3 solution using an H-type electrolyzer. During the test, the anode chamber and the cathode chamber were separated by a Nafion 117 membrane. CO2 gas was bubbled overnight in a NaHCO3 aqueous solution to obtain a CO2-saturated 0.1M NaHCO3 solution. To prepare a working electrode, 4 mg of sample (i.e., the electrocatalyst prepared in the examples and comparative examples) and 60 μl of Nafion solution were dispersed in 0.94 ml of ethanol solution to prepare 100 μl of catalyst ink. Then 12.5 μl of catalyst ink was applied to an area of 0.5 cm 2 on carbon paper. Pt wire and Ag / AgCl were used as counter electrode and reference electrode respectively. CO2 flow was controlled by mass flow meter and set to 27.4sccm. LSV test was performed on Princeton PMC-500 electrochemical workstation with a scan rate of 10mV / s. The potential value was corrected by reversible hydrogen electrode (RHE). According to previous literature, automatic compensation (85%) was used. A 15min chronoamperometric test was performed at each potential. The gas products were detected and analyzed by Shimadzu 2010 gas chromatograph and ST100 / 120 packed column gas chromatograph. High purity helium (99.999%) was used as chromatographic carrier gas. The relevant liquid products were analyzed by Bruker AvanceⅢHD 400NMR.
[0111] During the carbon dioxide electroreduction reaction, it is often affected by the competitive hydrogen evolution reaction. The specific reaction equations include:
[0112] Main reaction: CO2→CO+O2
[0113] Side reaction: H2O→H2+O2
[0114] It can be seen from the above reaction equations that the Faraday efficiency of producing oxygen from carbon dioxide can be expressed by the selectivity for carbon monoxide, and the Faraday efficiency of producing oxygen from water electrolysis can be expressed by the selectivity for hydrogen.
[0115] In an embodiment of the present invention, the process of preparing an electrocatalyst for producing oxygen from carbon dioxide comprises:
[0116] An organic substance rich in oxygen and easily soluble in water is used as a carbon source, and an inorganic substance with high temperature stability and easy solubility in water is used as a template. Through a rapid high-temperature roasting method, the organic substance as a carbon source is carbonized at high temperature while avoiding the problem of easy loss of lattice oxygen in the carbon material at high temperature, thereby preparing a carbon material with a high lattice oxygen content and a high degree of graphitization;
[0117] Taking advantage of the fact that carbon sources and templates are easily soluble in water, a mixed solvent of water and ethanol is used to clean the carbon sources and templates with a low degree of carbonization during the rapid calcination process, and a carbon carrier with a large specific surface area, a high lattice oxygen content and a high electrical conductivity is prepared by combining a secondary carbonization process.
[0118] The iron-based precursor dispersion solution is added dropwise to the carbon carrier dispersion solution, and after a long period of deposition, the iron-based precursor accumulated on the surface of the carbon carrier is washed away, so that the iron-based precursor is uniformly loaded on the surface of the carbon carrier;
[0119] By calcining the carbon carrier loaded with iron-based precursor in an inert atmosphere, the iron species in the iron-based precursor are induced to form coordination bonds with the oxygen element in the carbon carrier. The higher electronegativity of the oxygen element is utilized to regulate the electronic properties of the iron-based active center, and a high-performance iron-based electrocatalyst for producing oxygen from carbon dioxide modified by oxygen coordination is prepared.
[0120] The solution of the present invention is further described below in conjunction with specific embodiments.
[0121] Example 1
[0122] This embodiment adopts a preparation method comprising the following steps to prepare an electrocatalyst for producing oxygen from carbon dioxide:
[0123] (1) L-alanine is used as a carbon source and potassium carbonate is used as a template. L-alanine and potassium carbonate are fully ground to form a uniform mixture, wherein the mass ratio of the template to the carbon source is 3:1; the mixture is placed in a tube furnace in an argon atmosphere, and the temperature is increased to 1000°C at a heating rate of 50°C / min, maintained for 5 minutes, and then cooled to room temperature at a cooling rate of 50°C / min to complete a rapid calcination process;
[0124] (2) taking out the mixture that has been rapidly calcined, and washing the mixture that has been rapidly calcined with a mixed solution of ethanol and water to remove the template and the carbon source with a low degree of carbonization, wherein the volume ratio of water to ethanol is 2:1; after washing, transferring the black powder to an oven at 120°C, drying for 20 hours, placing it in a tubular furnace in an argon atmosphere, heating it to 400°C at a heating rate of 5°C / min, maintaining it for 2 hours, and then cooling it to room temperature at a cooling rate of 10°C / min to complete the secondary carbonization process, thereby obtaining a carbon carrier with both a high lattice oxygen content and a high degree of graphitization;
[0125] (3) dispersing the carbon support in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain solution A; wherein the mass ratio of the carbon support to N,N-dimethylformamide is 1:10;
[0126] (4) dispersing the iron porphyrin powder in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain a solution B, wherein the mass ratio of the carbon support to the N,N-dimethylformamide is 1:20;
[0127] (5) adding solution B dropwise into the continuously stirred solution A to form solution C, wherein the mass ratio of solution A to solution B is 3:1; stirring solution C for 10 h at 30° C., and then filtering to obtain a black precipitate;
[0128] (6) The black precipitate was washed with N,N-dimethylformamide until the washing solution was colorless; after washing, the precipitate was transferred to a vacuum drying oven at 60°C and dried for 20 hours; after drying, the black powder was placed in a tubular furnace in an argon atmosphere, and the temperature was increased to 400°C at a heating rate of 5°C / min, maintained for 2 hours, and then cooled to room temperature at a cooling rate of 10°C / min to obtain an oxygen-coordinated modified carbon dioxide electrocatalyst for producing oxygen.
[0129] Example 1 A carbon carrier is prepared by a method of rapid calcination combined with secondary carbonization. Figure 2 It can be seen that the carrier prepared in Example 1 presents a two-dimensional layered structure. Figure 3 It can be seen that the carrier prepared in Example 1 contains a large amount of CO in addition to conventional C=O, which indicates that the carbon carrier in Example 1 contains more lattice oxygen.
[0130] Subsequently, this embodiment adopts the method of excessive impregnation and controllable induction to prepare the iron-based electrocatalyst. Figure 4 It can be seen that the iron species on the surface of the catalyst prepared in Example 1 exists in the form of single atoms. Figure 5 It can be seen that the specific surface area of the catalyst prepared in Example 1 is as high as 997.3 m 2 / g. By Figure 6 It can be seen that the catalyst prepared in Example 1 forms an obvious Fe-O bond, indicating that the method in Example 1 can successfully induce the iron species in the iron-based precursor to form a coordination bond with the oxygen element in the carbon carrier under a high temperature inert atmosphere. Figure 7 It can be seen that the iron species of the catalyst prepared in Example 1 mainly presents a valence state of 3+.
[0131] Table 1 records the Faraday efficiency of CO2 to O2 produced by the electrocatalysts prepared in various embodiments of the present invention and comparative examples at different voltages. Figure 8As can be seen from Table 1, the Faraday efficiency of the electrocatalyst prepared in Example 1 for converting CO2 to O2 can be maintained at a high level of nearly 100% within a wide potential range of 400 mV (-0.55 V to -0.95 V). Figure 1 It can be seen that the electrocatalyst in Example 1 has no obvious performance deactivation in the 12-hour stability test. The above performance test results show that the strategy of rapid calcination combined with controllable induction in Example 1 can be used to prepare a high-performance electrocatalyst for CO2 to O2.
[0132] Example 2
[0133] This embodiment adopts a preparation method comprising the following steps to prepare an electrocatalyst for producing oxygen from carbon dioxide:
[0134] (1) L-alanine is used as a carbon source and potassium carbonate is used as a template. L-alanine and potassium carbonate are fully ground to form a uniform mixture, wherein the mass ratio of the template to the carbon source is 4:1; the mixture is placed in a tube furnace in an argon atmosphere, and the temperature is increased to 950°C at a heating rate of 30°C / min, maintained for 5 minutes, and then cooled to room temperature at a cooling rate of 50°C / min to complete a rapid calcination process;
[0135] (2) taking out the mixture that has been rapidly calcined, and washing the mixture that has been rapidly calcined with a mixed solution of ethanol and water to remove the template and the carbon source with a low degree of carbonization, wherein the volume ratio of water to ethanol is 2:1; after washing, transferring the black powder to a 90°C oven, drying for 30 hours, placing it in a tubular furnace in an argon atmosphere, heating it to 450°C at a heating rate of 10°C / min, maintaining it for 3 hours, and then cooling it to room temperature at a cooling rate of 10°C / min to complete the secondary carbonization process, thereby obtaining a carbon carrier with both a high lattice oxygen content and a high degree of graphitization;
[0136] (3) dispersing the carbon carrier in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain solution A; wherein the mass ratio of the carbon carrier to N,N-dimethylformamide is 1:12;
[0137] (4) dispersing the iron porphyrin powder in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain a solution B, wherein the mass ratio of the carbon support to the N,N-dimethylformamide is 1:15;
[0138] (5) adding solution B dropwise into the continuously stirred solution A to form solution C, wherein the mass ratio of solution A to solution B is 3:1; stirring solution C for 10 h at 30° C., and then filtering to obtain a black precipitate;
[0139] (6) The black precipitate was washed with N,N-dimethylformamide until the washing solution was colorless; after washing, the precipitate was transferred to a vacuum drying oven at 60°C and dried for 20 hours; after drying, the black powder was placed in a tubular furnace with an argon atmosphere, and the temperature was increased to 350°C at a heating rate of 5°C / min, maintained for 2 hours, and then cooled to room temperature at a cooling rate of 10°C / min to obtain an oxygen-coordinated modified carbon dioxide electrocatalyst for producing oxygen.
[0140] Example 2 uses a method similar to Example 1, which is a combination of rapid calcination and secondary carbonization, to prepare a carbon carrier. Compared with Example 1, some process parameters are changed. For example, the heating rate of step (1) in Example 2 is reduced to 30°C / min, and the secondary carbonization temperature of step (2) is increased to 450°C. Figure 2 It can be seen that the carbon carrier in Example 2 presents a two-dimensional layered structure.
[0141] Similar to Example 1, Example 2 adopts the method of excessive impregnation and controllable induction to prepare the iron-based electrocatalyst. Figure 4 It can be seen that the iron species on the surface of the electrocatalyst prepared in Example 2 exists in the form of single atoms. Figure 5 It can be seen that the specific surface area of the electrocatalyst prepared in Example 2 is as high as 986.2 m 2 / g. By Figure 8 As can be seen from Table 1, the Faraday efficiency of the electrocatalyst prepared in Example 2 for converting CO2 to O2 can be maintained at a high level of nearly 100% within a wide potential range of 400 mV (-0.55 V to -0.95 V). The above results show that the process parameters involved in the electrocatalyst preparation method provided by the present invention have a wide adjustable range.
[0142] Example 3
[0143] In this embodiment, based on the above embodiment 1, the carbon source is replaced by lysine from L-alanine to prepare the electrocatalyst. The specific preparation method includes the following steps:
[0144] (1) Lysine is used as a carbon source and potassium carbonate is used as a template. Lysine and potassium carbonate are fully ground to form a uniform mixture, wherein the mass ratio of the template to the carbon source is 3:1; the mixture is placed in a tube furnace in an argon atmosphere, heated to 1000°C at a heating rate of 50°C / min, maintained for 5 minutes, and then cooled to room temperature at a cooling rate of 50°C / min to complete a rapid calcination process;
[0145] (2) taking out the mixture that has been rapidly calcined, and washing the mixture that has been rapidly calcined with a mixed solution of ethanol and water to remove the template and the carbon source with a low degree of carbonization, wherein the volume ratio of water to ethanol is 2:1; after washing, transferring the black powder to an oven at 120°C, drying for 20 hours, placing it in a tubular furnace in an argon atmosphere, heating it to 400°C at a heating rate of 5°C / min, maintaining it for 2 hours, and then cooling it to room temperature at a cooling rate of 10°C / min to complete the secondary carbonization process, thereby obtaining a carbon carrier with both a high lattice oxygen content and a high degree of graphitization;
[0146] (3) dispersing the carbon support in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain solution A; wherein the mass ratio of the carbon support to N,N-dimethylformamide is 1:10;
[0147] (4) dispersing the iron porphyrin powder in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain a solution B, wherein the mass ratio of the carbon support to the N,N-dimethylformamide is 1:20;
[0148] (5) adding solution B dropwise into the continuously stirred solution A to form solution C, wherein the mass ratio of solution A to solution B is 3:1; stirring solution C for 10 h at 30° C., and then filtering to obtain a black precipitate;
[0149] (6) The black precipitate was washed with N,N-dimethylformamide until the washing solution was colorless; after washing, the precipitate was transferred to a vacuum drying oven at 60°C and dried for 20 hours; after drying, the black powder was placed in a tubular furnace in an argon atmosphere, and the temperature was increased to 400°C at a heating rate of 5°C / min, maintained for 2 hours, and then cooled to room temperature at a cooling rate of 10°C / min to obtain an oxygen-coordinated modified carbon dioxide electrocatalyst for producing oxygen.
[0150] It can be seen from the data in Table 1 that the electrocatalyst prepared in Example 3 has a Faraday efficiency of not less than 85% in a wide potential range of 400mV (-0.55V to -0.95V), and a Faraday efficiency of not less than 90% in a potential range of -0.65V to -0.85V, indicating that the electrocatalyst prepared by the preparation method provided by the present invention can improve the Faraday efficiency of CO2 to O2. However, compared with Example 1, the Faraday efficiency of CO2 to O2 of the electrocatalyst in this embodiment is as high as 93.81% at a voltage of -0.75V, and the Faraday efficiency is relatively low.
[0151] Due to the polymerization of carbon source molecules and the growth and extension of carbon materials during the carbonization process, it is beneficial to increase the loading of iron-based precursors and the number of catalyst active sites. The type of carbon source, especially the atomic arrangement in the carbon source molecules, will affect the polymerization of carbon source molecules and the growth and extension process of carbon carriers. From the above performance test results, it can be seen that compared with the electrocatalyst prepared with L-alanine as the carbon source, the performance of the electrocatalyst prepared with lysine as the carbon source is slightly worse. Further analysis shows that the atomic arrangement of L-alanine molecules is conducive to the polymerization of carbon sources and the growth and extension of carbon materials during the carbonization process, and it has unique advantages in using it as a carbon source to prepare electrocatalysts.
[0152] Example 4
[0153] In this embodiment, based on the embodiment 1, the template agent is replaced by sodium carbonate from potassium carbonate to prepare the electrocatalyst. The specific preparation method includes the following steps:
[0154] (1) L-alanine is used as a carbon source and sodium carbonate is used as a template. L-alanine and sodium carbonate are fully ground to form a uniform mixture, wherein the mass ratio of the template to the carbon source is 3:1; the mixture is placed in a tube furnace in an argon atmosphere, and the temperature is increased to 1000°C at a heating rate of 50°C / min, maintained for 5 minutes, and then cooled to room temperature at a cooling rate of 50°C / min to complete a rapid calcination process;
[0155] (2) taking out the mixture that has been rapidly calcined, and washing the mixture that has been rapidly calcined with a mixed solution of ethanol and water to remove the template and the carbon source with a low degree of carbonization, wherein the volume ratio of water to ethanol is 2:1; after washing, transferring the black powder to an oven at 120°C, drying for 20 hours, placing it in a tubular furnace in an argon atmosphere, heating it to 400°C at a heating rate of 5°C / min, maintaining it for 2 hours, and then cooling it to room temperature at a cooling rate of 10°C / min to complete the secondary carbonization process, thereby obtaining a carbon carrier with both a high lattice oxygen content and a high degree of graphitization;
[0156] (3) dispersing the carbon support in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain solution A; wherein the mass ratio of the carbon support to N,N-dimethylformamide is 1:10;
[0157] (4) dispersing the iron porphyrin powder in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain a solution B, wherein the mass ratio of the carbon support to the N,N-dimethylformamide is 1:20;
[0158] (5) adding solution B dropwise into the continuously stirred solution A to form solution C, wherein the mass ratio of solution A to solution B is 3:1; stirring solution C for 10 h at 30° C., and then filtering to obtain a black precipitate;
[0159] (6) The black precipitate was washed with N,N-dimethylformamide until the washing solution was colorless; after washing, the precipitate was transferred to a vacuum drying oven at 60°C and dried for 20 hours; after drying, the black powder was placed in a tubular furnace in an argon atmosphere, and the temperature was increased to 400°C at a heating rate of 5°C / min, maintained for 2 hours, and then cooled to room temperature at a cooling rate of 10°C / min to obtain an oxygen-coordinated modified carbon dioxide electrocatalyst for producing oxygen.
[0160] It can be seen from the data in Table 1 that the electrocatalyst prepared in Example 4 has a Faraday efficiency of not less than 87% in a wide potential range of 400mV (-0.55V to -0.95V), and a Faraday efficiency of not less than 90% in a potential range of -0.55V to -0.85V, indicating that the electrocatalyst prepared by the preparation method provided by the present invention can improve the Faraday efficiency of CO2 to O2. However, compared with Example 1, the Faraday efficiency of CO2 to O2 of the electrocatalyst in this embodiment at a voltage of -0.75V is as high as 94.18%, which is relatively low.
[0161] Adding a template is an effective means to increase the specific surface area of the catalyst. However, the presence of the template often leads to an increase in the impurity content in the material, which in turn affects the performance of the catalyst. The above performance test results show that the electrocatalyst prepared with potassium carbonate as a template has better performance. After analysis, it is known that the main reasons include: the melting point of sodium carbonate used in Example 4 is 851°C, while the melting point of potassium carbonate used in Example 1 is 891°C. In comparison, potassium carbonate has better high-temperature thermal stability, and potassium carbonate is easily soluble in water. After being fully mixed with the carbon source and subjected to high-temperature carbonization, it is easy to clean and remove, and the possibility of introducing impurities is lower.
[0162] Therefore, the use of potassium carbonate as a template in the preferred embodiment of the present invention has greater advantages in improving the performance of the electrocatalyst, such as increasing the Faraday efficiency.
[0163] Example 5
[0164] In this embodiment, based on the embodiment 1, the inert gas is replaced by nitrogen from argon to prepare the electrocatalyst. The specific preparation method includes the following steps:
[0165] (1) L-alanine is used as a carbon source and potassium carbonate is used as a template. L-alanine and potassium carbonate are fully ground to form a uniform mixture, wherein the mass ratio of the template to the carbon source is 3:1; the mixture is placed in a tubular furnace in a nitrogen atmosphere, and the temperature is increased to 1000°C at a heating rate of 50°C / min, maintained for 5 minutes, and then cooled to room temperature at a cooling rate of 50°C / min to complete a rapid calcination process;
[0166] (2) taking out the mixture that has been rapidly calcined, and washing the mixture that has been rapidly calcined with a mixed solution of ethanol and water to remove the template and the carbon source with a low degree of carbonization, wherein the volume ratio of water to ethanol is 2:1; after washing, transferring the black powder to an oven at 120° C., drying for 20 h, placing it in a tubular furnace in a nitrogen atmosphere, heating it to 400° C. at a heating rate of 5° C. / min, maintaining it for 2 h, and then cooling it to room temperature at a cooling rate of 10° C. / min to complete the secondary carbonization process, thereby obtaining a carbon carrier with both a high lattice oxygen content and a high degree of graphitization;
[0167] (3) dispersing the carbon support in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain solution A; wherein the mass ratio of the carbon support to N,N-dimethylformamide is 1:10;
[0168] (4) dispersing the iron porphyrin powder in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain a solution B, wherein the mass ratio of the carbon support to the N,N-dimethylformamide is 1:20;
[0169] (5) adding solution B dropwise into the continuously stirred solution A to form solution C, wherein the mass ratio of solution A to solution B is 3:1; stirring solution C for 10 h at 30° C., and then filtering to obtain a black precipitate;
[0170] (6) The black precipitate was washed with N,N-dimethylformamide until the washing solution was colorless; after washing, the precipitate was transferred to a vacuum drying oven at 60°C and dried for 20 hours; after drying, the black powder was placed in a tubular furnace in a nitrogen atmosphere, and the temperature was increased to 400°C at a heating rate of 5°C / min, maintained for 2 hours, and then cooled to room temperature at a cooling rate of 10°C / min to obtain an oxygen-coordinated modified carbon dioxide electrocatalyst for producing oxygen.
[0171] It can be seen from the data in Table 1 that the electrocatalyst prepared in Example 5 has a Faraday efficiency of not less than 86% in a wide potential range of 400mV (-0.55V to -0.95V), and the highest Faraday efficiency of CO2 to O2 (at a voltage of -0.75V) is 91.62%, indicating that the electrocatalyst prepared by the preparation method provided by the present invention can improve the Faraday efficiency of CO2 to O2 to a certain extent. However, compared with Example 1, the highest Faraday efficiency of the electrocatalyst in this embodiment at a voltage of -0.75V is 91.62%, which is relatively low.
[0172] The high-temperature carbonization process of the carbon source and the controllable high-temperature induction process of the Fe-O bond in the catalyst preparation need to be carried out in an inert atmosphere. Nitrogen and argon are two gases commonly used to maintain an inert atmosphere, but from the above performance test results, it can be seen that the electrocatalyst prepared using argon as an inert gas has relatively better catalytic performance. This is mainly because argon has more stable chemical properties and is a more suitable inert gas in the preferred embodiment of the present invention.
[0173] Table 1 Faradaic efficiency of CO2 to O2 produced by electrocatalysts prepared in various embodiments at different voltages (%)
[0174]
[0175] Comparative Example 1
[0176] In this comparative example, on the basis of Example 1, the holding time at the calcination temperature in step (1) was extended from 5 min to 2 h to prepare the electrocatalyst. The specific preparation method includes the following steps:
[0177] (1) L-alanine is used as a carbon source and potassium carbonate is used as a template. L-alanine and potassium carbonate are fully ground to form a uniform mixture, wherein the mass ratio of the template to the carbon source is 3:1; the mixture is placed in a tube furnace in an argon atmosphere, and the temperature is increased to 1000°C at a heating rate of 50°C / min, maintained for 2 hours, and then cooled to room temperature at a cooling rate of 50°C / min to complete a rapid calcination process;
[0178] (2) taking out the mixture that has been rapidly calcined, and washing the mixture that has been rapidly calcined with a mixed solution of ethanol and water to remove the template and the carbon source with a low degree of carbonization, wherein the volume ratio of water to ethanol is 2:1; after washing, transferring the black powder to an oven at 120°C, drying for 20 hours, placing it in a tubular furnace in an argon atmosphere, heating it to 400°C at a heating rate of 5°C / min, maintaining it for 2 hours, and then cooling it to room temperature at a cooling rate of 10°C / min to complete the secondary carbonization process, thereby obtaining a carbon carrier with both a high lattice oxygen content and a high degree of graphitization;
[0179] (3) dispersing the carbon support in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain solution A; wherein the mass ratio of the carbon support to N,N-dimethylformamide is 1:10;
[0180] (4) dispersing the iron porphyrin powder in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain a solution B, wherein the mass ratio of the carbon support to the N,N-dimethylformamide is 1:20;
[0181] (5) adding solution B dropwise into the continuously stirred solution A to form solution C, wherein the mass ratio of solution A to solution B is 3:1; stirring solution C for 10 h at 30° C., and then filtering to obtain a black precipitate;
[0182] (6) The black precipitate was washed with N,N-dimethylformamide until the washing solution was colorless; after washing, the precipitate was transferred to a vacuum drying oven at 60°C and dried for 20 hours; after drying, the black powder was placed in a tubular furnace in an argon atmosphere, and the temperature was increased to 400°C at a heating rate of 5°C / min, maintained for 2 hours, and then cooled to room temperature at a cooling rate of 10°C / min to obtain an oxygen-coordinated modified carbon dioxide electrocatalyst for producing oxygen.
[0183] This comparative example investigates the differences between the electrocatalyst preparation method provided by the present invention and the conventional electrocatalyst preparation method, especially the advantages over the conventional high-temperature calcination method. This comparative example adopts the conventional high-temperature calcination method. Specifically, compared with Example 1, the high-temperature calcination time is changed from 5 minutes to 2 hours. Figure 3 It can be seen that the carbon carrier prepared in Comparative Example 1 contains conventional C=O, but the CO content is relatively low. It can be seen that the carbon carrier prepared in Comparative Example 1 contains less lattice oxygen, indicating that long-term high-temperature calcination will lead to the loss of lattice oxygen in the carbon carrier. The solution of the present invention adopts a rapid calcination method to solve the above problem.
[0184] pass Figure 6 It can be seen that the electrocatalyst prepared in Comparative Example 1 did not form obvious Fe-O bonds, indicating that the lattice oxygen content in the carbon support has an important influence on the formation of Fe-O bonds. Figure 7 It can be seen that the iron species of the electrocatalyst prepared in Comparative Example 1 mainly presents a valence state of 3+, but compared with Example 1, the valence state of the iron species is obviously shifted toward the direction of low binding energy, indicating that the absence of Fe-O bonds reduces the valence state of the iron species.
[0185] Table 2 records the Faraday efficiency of CO2 to O2 at different voltages for the electrocatalysts prepared in Example 1 of the present invention and various comparative examples. Figure 8 As shown in Table 2, the Faraday efficiency of the catalyst prepared in Comparative Example 1 at a voltage of -0.75 V for converting CO2 to O2 is only 82.29% at most, which is significantly lower than that in Example 1. The above performance test results illustrate the key role of Fe-O bonds in the structure and performance of the catalyst, and also illustrate the importance of the rapid calcination method adopted in the scheme of the present invention, especially the control of the rapid calcination time, to the formation of Fe-O bonds, thereby improving the performance of the obtained electrocatalyst.
[0186] Comparative Example 2
[0187] This comparative example eliminates the secondary carbonization process in step (2) on the basis of Example 1, and prepares the electrocatalyst. The specific preparation method includes the following steps:
[0188] (1) L-alanine is used as a carbon source and potassium carbonate is used as a template. L-alanine and potassium carbonate are fully ground to form a uniform mixture, wherein the mass ratio of the template to the carbon source is 3:1; the mixture is placed in a tube furnace in an argon atmosphere, and the temperature is increased to 1000°C at a heating rate of 50°C / min, maintained for 5 minutes, and then cooled to room temperature at a cooling rate of 50°C / min to complete a rapid calcination process;
[0189] (2) taking out the mixture after rapid calcination, and washing the mixture after rapid calcination with a mixed solution of ethanol and water to remove the template and the carbon source with a low degree of carbonization, wherein the volume ratio of water to ethanol is 2:1; after washing, transferring the black powder to an oven at 120° C. and drying for 20 hours to obtain a carbon carrier;
[0190] (3) dispersing the carbon support in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain solution A; wherein the mass ratio of the carbon support to N,N-dimethylformamide is 1:10;
[0191] (4) dispersing the iron porphyrin powder in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain a solution B, wherein the mass ratio of the carbon support to the N,N-dimethylformamide is 1:20;
[0192] (5) adding solution B dropwise into the continuously stirred solution A to form solution C, wherein the mass ratio of solution A to solution B is 3:1; stirring solution C for 10 h at 30° C., and then filtering to obtain a black precipitate;
[0193] (6) The black precipitate was washed with N,N-dimethylformamide until the washing solution was colorless; after washing, the precipitate was transferred to a vacuum drying oven at 60°C and dried for 20 hours; after drying, the black powder was placed in a tubular furnace in an argon atmosphere, and the temperature was increased to 400°C at a heating rate of 5°C / min, maintained for 2 hours, and then cooled to room temperature at a cooling rate of 10°C / min to obtain an oxygen-coordinated modified carbon dioxide electrocatalyst for producing oxygen.
[0194] Compared with Example 1, the secondary carbonization process is deleted in Comparative Example 2. It can be seen from the data in Table 2 that the Faraday efficiency of the electrocatalyst prepared in Comparative Example 2 at a voltage of -0.75V is as high as 72.39% for CO2 to O2, which is significantly lower than that in Example 1. It can be seen that the secondary carbonization process plays a key role in the preparation of electrocatalysts for CO2 to O2. Specifically, the secondary carbonization process can affect the graphitization degree of the carbon carrier, thereby affecting the electron transfer efficiency during the catalytic reaction of the electrocatalyst, and having an important impact on the performance of the electrocatalyst.
[0195] Comparative Example 3
[0196] In this comparative example, the secondary carbonization temperature is reduced from 400° C. to 300° C. on the basis of Example 1 to prepare the electrocatalyst. The specific preparation method includes the following steps:
[0197] (1) L-alanine is used as a carbon source and potassium carbonate is used as a template. L-alanine and potassium carbonate are fully ground to form a uniform mixture, wherein the mass ratio of the template to the carbon source is 3:1; the mixture is placed in a tube furnace in an argon atmosphere, and the temperature is increased to 1000°C at a heating rate of 50°C / min, maintained for 5 minutes, and then cooled to room temperature at a cooling rate of 50°C / min to complete a rapid calcination process;
[0198] (2) taking out the mixture that has been rapidly calcined, and washing the mixture that has been rapidly calcined with a mixed solution of ethanol and water to remove the template and the carbon source with a low degree of carbonization, wherein the volume ratio of water to ethanol is 2:1; after washing, transferring the black powder to an oven at 120°C, drying for 20 hours, placing it in a tubular furnace in an argon atmosphere, heating it to 300°C at a heating rate of 5°C / min, maintaining it for 2 hours, and then cooling it to room temperature at a cooling rate of 10°C / min to complete the secondary carbonization process, thereby obtaining a carbon carrier with both a high lattice oxygen content and a high degree of graphitization;
[0199] (3) dispersing the carbon support in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain solution A; wherein the mass ratio of the carbon support to N,N-dimethylformamide is 1:10;
[0200] (4) dispersing the iron porphyrin powder in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain a solution B, wherein the mass ratio of the carbon support to the N,N-dimethylformamide is 1:20;
[0201] (5) adding solution B dropwise into the continuously stirred solution A to form solution C, wherein the mass ratio of solution A to solution B is 3:1; stirring solution C for 10 h at 30° C., and then filtering to obtain a black precipitate;
[0202] (6) The black precipitate was washed with N,N-dimethylformamide until the washing solution was colorless; after washing, the precipitate was transferred to a vacuum drying oven at 60°C and dried for 20 hours; after drying, the black powder was placed in a tubular furnace in an argon atmosphere, and the temperature was increased to 400°C at a heating rate of 5°C / min, maintained for 2 hours, and then cooled to room temperature at a cooling rate of 10°C / min to obtain an oxygen-coordinated modified carbon dioxide electrocatalyst for producing oxygen.
[0203] Compared with Example 1, the secondary carbonization temperature is reduced from 400°C to 300°C in Comparative Example 3. It can be seen from the data in Table 2 that the Faraday efficiency of CO2 to O2 of the electrocatalyst prepared in Comparative Example 3 is as high as 89.37% at a voltage of -0.75V, which is significantly lower than that of Example 1. This shows that the secondary carbonization temperature will have an important influence on the performance of the electrocatalyst by affecting the degree of graphitization of the carbon carrier. Compared with the electrocatalyst prepared at a secondary carbonization temperature of 300°C, the electrocatalyst prepared when the secondary carbonization temperature is controlled at 400°C has a higher electron transfer efficiency and better performance.
[0204] Comparative Example 4
[0205] In this comparative example, based on Example 1, the secondary carbonization temperature is increased from 400° C. to 500° C. to prepare the electrocatalyst. The specific preparation method includes the following steps:
[0206] (1) L-alanine is used as a carbon source and potassium carbonate is used as a template. L-alanine and potassium carbonate are fully ground to form a uniform mixture, wherein the mass ratio of the template to the carbon source is 3:1; the mixture is placed in a tube furnace in an argon atmosphere, and the temperature is increased to 1000°C at a heating rate of 50°C / min, maintained for 5 minutes, and then cooled to room temperature at a cooling rate of 50°C / min to complete a rapid calcination process;
[0207] (2) taking out the mixture that has been rapidly calcined, and washing the mixture that has been rapidly calcined with a mixed solution of ethanol and water to remove the template and the carbon source with a low degree of carbonization, wherein the volume ratio of water to ethanol is 2:1; after washing, transferring the black powder to an oven at 120°C, drying for 20 hours, placing it in a tubular furnace in an argon atmosphere, heating it to 500°C at a heating rate of 5°C / min, maintaining it for 2 hours, and then cooling it to room temperature at a cooling rate of 10°C / min to complete the secondary carbonization process, thereby obtaining a carbon carrier with both a high lattice oxygen content and a high degree of graphitization;
[0208] (3) dispersing the carbon support in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain solution A; wherein the mass ratio of the carbon support to N,N-dimethylformamide is 1:10;
[0209] (4) dispersing the iron porphyrin powder in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain a solution B, wherein the mass ratio of the carbon support to the N,N-dimethylformamide is 1:20;
[0210] (5) adding solution B dropwise into the continuously stirred solution A to form solution C, wherein the mass ratio of solution A to solution B is 3:1; stirring solution C for 10 h at 30° C., and then filtering to obtain a black precipitate;
[0211] (6) The black precipitate was washed with N,N-dimethylformamide until the washing solution was colorless; after washing, the precipitate was transferred to a vacuum drying oven at 60°C and dried for 20 hours; after drying, the black powder was placed in a tubular furnace in an argon atmosphere, and the temperature was increased to 400°C at a heating rate of 5°C / min, maintained for 2 hours, and then cooled to room temperature at a cooling rate of 10°C / min to obtain an oxygen-coordinated modified carbon dioxide electrocatalyst for producing oxygen.
[0212] Increasing the secondary carbonization temperature is beneficial to improving the graphitization degree of the carbon carrier and the electron transfer efficiency during the catalytic reaction of the electrocatalyst. However, compared with Example 1, Comparative Example 4 increases the secondary carbonization temperature to 500°C. From the data in Table 2, it can be seen that the Faraday efficiency of CO2 to O2 of the electrocatalyst prepared in Comparative Example 4 is as high as 84.91% at a voltage of -0.75V, which is significantly lower than that of Example 1. This shows that when the secondary carbonization temperature is too high, the performance of the electrocatalyst will be reduced. This is mainly because when the secondary carbonization temperature exceeds a certain level, the lattice oxygen in the carbon carrier will be lost in the form of CO or CO2, resulting in a decrease in the lattice oxygen content in the carbon carrier.
[0213] Comprehensively comparing the test results of Example 1 and Comparative Examples 2-4, it is found that the secondary carbonization process plays an important role in improving the performance of the electrocatalyst, and the secondary carbonization temperature is preferably controlled at about 400°C.
[0214] Comparative Example 5
[0215] In this comparative example, the template in step (1) is deleted on the basis of Example 1 to prepare the electrocatalyst. The specific preparation method includes the following steps:
[0216] (1) L-alanine was used as a carbon source, and the mixture was placed in a tube furnace in an argon atmosphere, heated to 1000°C at a heating rate of 50°C / min, maintained for 5 minutes, and then cooled to room temperature at a cooling rate of 50°C / min to complete a rapid calcination process;
[0217] (2) taking out the mixture that has been rapidly calcined, and washing the mixture that has been rapidly calcined with a mixed solution of ethanol and water to remove the template and the carbon source with a low degree of carbonization, wherein the volume ratio of water to ethanol is 2:1; after washing, transferring the black powder to an oven at 120°C, drying for 20 hours, placing it in a tubular furnace in an argon atmosphere, heating it to 400°C at a heating rate of 5°C / min, maintaining it for 2 hours, and then cooling it to room temperature at a cooling rate of 10°C / min to complete the secondary carbonization process, thereby obtaining a carbon carrier with both a high lattice oxygen content and a high degree of graphitization;
[0218] (3) dispersing the carbon support in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain solution A; wherein the mass ratio of the carbon support to N,N-dimethylformamide is 1:10;
[0219] (4) dispersing the iron porphyrin powder in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain a solution B, wherein the mass ratio of the carbon support to the N,N-dimethylformamide is 1:20;
[0220] (5) adding solution B dropwise into the continuously stirred solution A to form solution C, wherein the mass ratio of solution A to solution B is 3:1; stirring solution C for 10 h at 30° C., and then filtering to obtain a black precipitate;
[0221] (6) The black precipitate was washed with N,N-dimethylformamide until the washing solution was colorless; after washing, the precipitate was transferred to a vacuum drying oven at 60°C and dried for 20 hours; after drying, the black powder was placed in a tubular furnace in an argon atmosphere, and the temperature was increased to 400°C at a heating rate of 5°C / min, maintained for 2 hours, and then cooled to room temperature at a cooling rate of 10°C / min to obtain an oxygen-coordinated modified carbon dioxide electrocatalyst for producing oxygen.
[0222] The specific surface area of the carbon carrier and the electrocatalyst will affect the contact effect between the reaction gas and the active sites during the reaction, and thus affect the performance of the electrocatalyst. Template assistance is an effective means to increase the specific surface area of the material. This comparative example prepares the electrocatalyst without using a template, which is used to compare with Example 1 to examine the effect of the template. It can be seen from the data in Table 2 that the electrocatalyst prepared in Comparative Example 5 has a maximum Faraday efficiency of 87.03% for CO2 to O2 at a voltage of -0.75V, which is significantly lower than that of Example 1. The above performance test results show that the template plays a key role in the preparation of high-performance CO2 to O2 electrocatalysts.
[0223] Comparative Example 6
[0224] In this comparative example, the induction temperature is lowered from 400° C. to 300° C. on the basis of Example 1 to prepare the electrocatalyst. The specific preparation method includes the following steps:
[0225] (1) L-alanine is used as a carbon source and potassium carbonate is used as a template. L-alanine and potassium carbonate are fully ground to form a uniform mixture, wherein the mass ratio of the template to the carbon source is 3:1; the mixture is placed in a tube furnace in an argon atmosphere, and the temperature is increased to 1000°C at a heating rate of 50°C / min, maintained for 5 minutes, and then cooled to room temperature at a cooling rate of 50°C / min to complete a rapid calcination process;
[0226] (2) taking out the mixture that has been rapidly calcined, and washing the mixture that has been rapidly calcined with a mixed solution of ethanol and water to remove the template and the carbon source with a low degree of carbonization, wherein the volume ratio of water to ethanol is 2:1; after washing, transferring the black powder to an oven at 120°C, drying for 20 hours, placing it in a tubular furnace in an argon atmosphere, heating it to 400°C at a heating rate of 5°C / min, maintaining it for 2 hours, and then cooling it to room temperature at a cooling rate of 10°C / min to complete the secondary carbonization process, thereby obtaining a carbon carrier with both a high lattice oxygen content and a high degree of graphitization;
[0227] (3) dispersing the carbon support in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain solution A; wherein the mass ratio of the carbon support to N,N-dimethylformamide is 1:10;
[0228] (4) dispersing the iron porphyrin powder in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain a solution B, wherein the mass ratio of the carbon support to the N,N-dimethylformamide is 1:20;
[0229] (5) adding solution B dropwise into the continuously stirred solution A to form solution C, wherein the mass ratio of solution A to solution B is 3:1; stirring solution C for 10 h at 30° C., and then filtering to obtain a black precipitate;
[0230] (6) The black precipitate was washed with N,N-dimethylformamide until the washing solution was colorless; after washing, the precipitate was transferred to a vacuum drying oven at 60°C and dried for 20 hours; after drying, the black powder was placed in a tubular furnace with an argon atmosphere, and the temperature was increased to 300°C at a heating rate of 5°C / min, maintained for 2 hours, and then cooled to room temperature at a cooling rate of 10°C / min to obtain an oxygen-coordinated modified carbon dioxide electrocatalyst for producing oxygen.
[0231] During the catalyst preparation process, the formation of Fe-O bonds requires controllable induction in an inert atmosphere, and the induction temperature is an important factor affecting the formation of Fe-O bonds. This comparative example examines the effect of the induction temperature on the induction process. Compared with Example 1, Comparative Example 6 reduces the induction temperature from 400°C to 300°C. From the test data in Table 2, it can be seen that the electrocatalyst prepared in Comparative Example 6 has a maximum Faraday efficiency of 88.28% for CO2 to O2 at a voltage of -0.75V, which is significantly lower than that in Example 1, indicating that an electrocatalyst with excellent catalytic performance cannot be obtained when the induction temperature is too low.
[0232] Comparative Example 7
[0233] In this comparative example, the induction temperature is increased from 400° C. to 500° C. on the basis of Example 1, and the electrocatalyst is prepared. The specific preparation method includes the following steps:
[0234] (1) L-alanine is used as a carbon source and potassium carbonate is used as a template. L-alanine and potassium carbonate are fully ground to form a uniform mixture, wherein the mass ratio of the template to the carbon source is 3:1; the mixture is placed in a tube furnace in an argon atmosphere, and the temperature is increased to 1000°C at a heating rate of 50°C / min, maintained for 5 minutes, and then cooled to room temperature at a cooling rate of 50°C / min to complete a rapid calcination process;
[0235] (2) taking out the mixture that has been rapidly calcined, and washing the mixture that has been rapidly calcined with a mixed solution of ethanol and water to remove the template and the carbon source with a low degree of carbonization, wherein the volume ratio of water to ethanol is 2:1; after washing, transferring the black powder to an oven at 120°C, drying for 20 hours, placing it in a tubular furnace in an argon atmosphere, heating it to 400°C at a heating rate of 5°C / min, maintaining it for 2 hours, and then cooling it to room temperature at a cooling rate of 10°C / min to complete the secondary carbonization process, thereby obtaining a carbon carrier with both a high lattice oxygen content and a high degree of graphitization;
[0236] (3) dispersing the carbon support in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain solution A; wherein the mass ratio of the carbon support to N,N-dimethylformamide is 1:10;
[0237] (4) dispersing the iron porphyrin powder in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain a solution B, wherein the mass ratio of the carbon support to the N,N-dimethylformamide is 1:20;
[0238] (5) adding solution B dropwise into the continuously stirred solution A to form solution C, wherein the mass ratio of solution A to solution B is 3:1; stirring solution C for 10 h at 30° C., and then filtering to obtain a black precipitate;
[0239] (6) The black precipitate was washed with N,N-dimethylformamide until the washing solution was colorless; after washing, the precipitate was transferred to a vacuum drying oven at 60°C and dried for 20 hours; after drying, the black powder was placed in a tubular furnace in an argon atmosphere, and the temperature was increased to 500°C at a heating rate of 5°C / min, maintained for 2 hours, and then cooled to room temperature at a cooling rate of 10°C / min to obtain an oxygen-coordinated modified carbon dioxide electrocatalyst for producing oxygen.
[0240] It can be seen from the test data in Table 2 that the comparative example increases the induction temperature to 500°C, and the Faradaic efficiency of the obtained electrocatalyst to produce O2 at a voltage of -0.75V is as high as 86.34%, which is significantly lower than that of Example 1. The performance test results show that too high an induction temperature will lead to a decrease in the catalytic performance of the electrocatalyst.
[0241] By comparing the test results of Example 1 and Comparative Examples 6 and 7, it is found that in the scheme of the present invention, the induction temperature needs to be controlled within a certain range, and in the preferred scheme, the induction temperature is controlled at about 400°C, and the obtained electrocatalyst has better performance.
[0242] Comparative Example 8
[0243] In this comparative example, based on Example 1, the heating rate of the calcination process in step (1) was reduced from 50° C. / min to 20° C. / min to prepare the electrocatalyst. The specific preparation method includes the following steps:
[0244] (1) L-alanine is used as a carbon source and potassium carbonate is used as a template. L-alanine and potassium carbonate are fully ground to form a uniform mixture, wherein the mass ratio of the template to the carbon source is 3:1; the mixture is placed in a tube furnace in an argon atmosphere, and the temperature is increased to 1000°C at a heating rate of 20°C / min, maintained for 5 minutes, and then cooled to room temperature at a cooling rate of 50°C / min to complete a rapid calcination process;
[0245] (2) taking out the mixture that has been rapidly calcined, and washing the mixture that has been rapidly calcined with a mixed solution of ethanol and water to remove the template and the carbon source with a low degree of carbonization, wherein the volume ratio of water to ethanol is 2:1; after washing, transferring the black powder to an oven at 120°C, drying for 20 hours, placing it in a tubular furnace in an argon atmosphere, heating it to 400°C at a heating rate of 5°C / min, maintaining it for 2 hours, and then cooling it to room temperature at a cooling rate of 10°C / min to complete the secondary carbonization process, thereby obtaining a carbon carrier with both a high lattice oxygen content and a high degree of graphitization;
[0246] (3) dispersing the carbon support in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain solution A; wherein the mass ratio of the carbon support to N,N-dimethylformamide is 1:10;
[0247] (4) dispersing the iron porphyrin powder in N,N-dimethylformamide, and ultrasonicating for 5 h at a temperature of 30° C. to obtain a solution B, wherein the mass ratio of the carbon support to the N,N-dimethylformamide is 1:20;
[0248] (5) adding solution B dropwise into the continuously stirred solution A to form solution C, wherein the mass ratio of solution A to solution B is 3:1; stirring solution C for 10 h at 30° C., and then filtering to obtain a black precipitate;
[0249] (6) The black precipitate was washed with N,N-dimethylformamide until the washing solution was colorless; after washing, the precipitate was transferred to a vacuum drying oven at 60°C and dried for 20 hours; after drying, the black powder was placed in a tubular furnace in an argon atmosphere, and the temperature was increased to 400°C at a heating rate of 5°C / min, maintained for 2 hours, and then cooled to room temperature at a cooling rate of 10°C / min to obtain an oxygen-coordinated modified carbon dioxide electrocatalyst for producing oxygen.
[0250] It can be seen from the test data in Table 2 that the comparative example reduces the heating rate of the rapid calcination process to 20°C / min, and the Faraday efficiency of the obtained electrocatalyst to produce O2 at a voltage of -0.75V is as high as 87.92%, which is significantly lower than that in Example 1. The performance test results show that when the heating rate of the rapid calcination process is too slow, the catalytic performance of the electrocatalyst will decrease. This is because too slow a heating rate will cause the loss of lattice oxygen, which in turn leads to a decrease in the lattice oxygen content in the carbon carrier. The scheme of the present invention controls the heating rate of the rapid calcination process at 30 to 70°C / min, and optimally controls it at 50°C / min, so as to obtain an electrocatalyst with better catalytic performance.
[0251] Table 2 Faradaic efficiency of CO2 to O2 produced by electrocatalysts prepared in Example 1 and comparative examples at different voltages (%)
[0252]
[0253]
[0254] The above is only a preferred embodiment of the present invention, and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment, it is not used to limit the present invention. Any technician familiar with this patent can make some changes or modify the technical contents suggested above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the solution of the present invention.
Claims
1. A method for preparing an electrocatalyst for producing oxygen from carbon dioxide, characterized in that: The following steps are involved: (1) using an oxygen-containing and water-soluble organic substance as a carbon source and an inorganic substance that is water-soluble as a template, grinding the carbon source and the template together to form a mixture, heating the mixture to a calcination temperature under an inert gas atmosphere and maintaining the temperature, and then cooling the mixture to room temperature to complete the calcination process; (2) washing the calcined mixture, drying it, and then heating it to a secondary carbonization temperature under an inert gas atmosphere and maintaining the temperature, and then cooling it to room temperature to complete the secondary carbonization process to obtain a carbon carrier; wherein the secondary carbonization temperature is lower than the calcination temperature; (3) dispersing the carbon support in a solvent to obtain a solution A; (4) dispersing the iron-based precursor in a solvent to obtain a solution B; (5) adding solution B dropwise to the continuously stirred solution A to form solution C. After solution C is stirred for a period of time, solid-liquid separation is performed to obtain a black mixture; (6) After the black mixture is washed and dried, it is heated to an induction temperature and maintained under an inert gas atmosphere, and then cooled to room temperature to obtain an oxygen-coordinated modified carbon dioxide electrocatalyst for producing oxygen.
2. The method for preparing an electrocatalyst for producing oxygen from carbon dioxide according to claim 1, characterized in that: In step (1), the carbon source comprises at least one of L-alanine, lysine, tyrosine, tryptophan, phenylalanine, serine, leucine, proline, isoleucine, glutamic acid, aspartic acid, valine and arginine, preferably L-alanine; And / or, in step (1), the template comprises at least one of potassium carbonate, potassium carbonate, sodium chloride, and potassium chloride, preferably potassium carbonate; And / or, in step (1), the mass ratio of the template to the carbon source is 1:1 to 10:1, preferably 3:1 to 4:1, and more preferably 3:
1.
3. The method for preparing an electrocatalyst for producing oxygen from carbon dioxide according to claim 1 or 2, characterized in that: In step (1), the calcination temperature is 900-1200° C., preferably 950-1000° C., more preferably 1000° C.; the holding time at the calcination temperature is 1-10 min, preferably 5 min; Preferably, the temperature is increased to the calcination temperature at a heating rate of 30 to 70°C / min, and the heating rate is preferably 30 to 50°C / min, more preferably 50°C / min; Cooling from the calcination temperature to room temperature at a cooling rate of 20 to 70°C / min, preferably 50°C / min; Preferably, the inert gas used in the roasting process is at least one of argon, nitrogen, helium and neon, preferably argon.
4. The method for preparing an electrocatalyst for producing oxygen from carbon dioxide according to any one of claims 1 to 3, characterized in that: In step (2), the calcined mixture is washed with a mixed solution of ethanol and water; Preferably, the volume ratio of water to ethanol is 1:1 to 5:1, preferably 2:1; Preferably, the washed mixture is dried at 90-200° C., preferably 90-120° C., more preferably 120° C.; the drying time is 10-30 h, preferably 20-30 h, more preferably 20 h.
5. The method for preparing an electrocatalyst for producing oxygen from carbon dioxide according to any one of claims 1 to 4, characterized in that: In step (2), the secondary carbonization temperature is 400-450°C, preferably 400°C; the holding time at the secondary calcination temperature is 1-5h, preferably 2-3h, more preferably 2h; Preferably, the temperature is increased to the secondary carbonization temperature at a heating rate of 1 to 10°C / min, and the heating rate is preferably 5 to 10°C / min, more preferably 5°C / min; Cooling from the secondary calcination temperature to room temperature at a cooling rate of 5 to 20°C / min, preferably 10°C / min; Preferably, the inert gas used in the secondary carbonization process is at least one of argon, nitrogen, helium and neon, preferably argon.
6. The method for preparing an electrocatalyst for producing oxygen from carbon dioxide according to any one of claims 1 to 5, characterized in that: In step (3), the mass ratio of the carbon support to the solvent is 1:5 to 1:15, preferably 1:10 to 1:12, and more preferably 1:10; Preferably, the carbon carrier is mixed with the solvent and then subjected to ultrasonic treatment to obtain solution A; the temperature of the ultrasonic treatment is 20 to 70° C., preferably 30° C.; the duration of the ultrasonic treatment is 1 to 10 h, preferably 5 h; Preferably, the solvent used to disperse the carbon carrier includes at least one of N,N-dimethylformamide, ethanol, carbon tetrachloride, diethyl ether, n-hexane, and chloroform, preferably N,N-dimethylformamide.
7. The method for preparing an electrocatalyst for producing oxygen from carbon dioxide according to any one of claims 1 to 6, characterized in that: In step (4), the iron-based precursor is iron porphyrin, and the mass ratio of iron porphyrin to solvent is 1:15 to 1:25, preferably 1:15 to 1:20, and more preferably 1:20; Preferably, the iron-based precursor is mixed with a solvent and then subjected to ultrasonic treatment to obtain a solution B; the temperature of the ultrasonic treatment is 20 to 70° C., preferably 30° C.; the duration of the ultrasonic treatment is 1 to 10 h, preferably 5 h; Preferably, the solvent used to disperse the iron-based precursor includes at least one of N,N-dimethylformamide, ethanol, carbon tetrachloride, ether, n-hexane, and chloroform, preferably N,N-dimethylformamide.
8. The method for preparing an electrocatalyst for producing oxygen from carbon dioxide according to any one of claims 1 to 7, characterized in that: In step (5), the mass ratio of solution A to solution B is 1:1 to 5:1, preferably 3:1; Solution C is continuously stirred at 20-70° C. for 5-20 h, preferably at 30° C., and preferably for 10 h.
9. The method for preparing an electrocatalyst for producing oxygen from carbon dioxide according to any one of claims 1 to 8, characterized in that: In step (6), the induction temperature is 350-400° C., preferably 400° C.; the holding time at the induction temperature is 1-5 h, preferably 2 h; Preferably, the temperature is raised to the induction temperature at a heating rate of 1 to 10°C / min, and the heating rate is preferably 5°C / min; the temperature is lowered from the induction temperature to room temperature at a cooling rate of 5 to 20°C / min, and the cooling rate is preferably 10°C / min; Preferably, the inert gas used is at least one of argon, nitrogen, helium and neon, preferably argon; Preferably, the cleaning liquid used to clean the black mixture includes at least one of N,N-dimethylformamide, ethanol, carbon tetrachloride, ether, n-hexane, and chloroform, preferably N,N-dimethylformamide; Preferably, the cleaned black mixture is vacuum dried at a temperature of 50 to 90° C., preferably 60° C.; and the drying time is 10 to 30 hours, preferably 20 hours.
10. Use of an electrocatalyst prepared by the method for preparing an electrocatalyst for producing oxygen from carbon dioxide as claimed in any one of claims 1 to 9 in catalyzing the production of oxygen from carbon dioxide.