Perovskite crystalline silicon laminated solar cell preparation method based on interface modification

By using interface modification technology in the preparation of perovskite crystalline silicon stacked solar cells, including high-purity cleaning and advanced deposition methods, the problem of low photoelectric conversion efficiency of perovskite crystalline silicon stacked solar cells is solved, significantly improving the battery Performance and stability.

CN119053215AInactive Publication Date: 2024-11-29陈成
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410909536.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The preparation method of perovskite crystalline silicon stacked solar cells has not been fully optimized, resulting in low photoelectric conversion efficiency and limited application. In-depth research is required in terms of materials, processes and equipment to improve performance and stability.

Method used

Using an interface modification-based preparation method, including careful selection of single crystal silicon wafers and high-purity deionized water cleaning, combined with RF power sputtering and atomic layer deposition technology to form a high-quality crystalline silicon substrate, followed by rotating in a nitrogen glove box Coating and heat treatment, followed by evaporation and atomic layer deposition techniques to form a perovskite layer, and depositing tin oxide and indium zinc oxide layers thereon, and finally depositing the electrode and anti-reflection layer by DC sputtering and thermal evaporation.

Benefits of technology

It significantly improves the crystal structure integrity of single crystal silicon wafers and the uniformity of the film, reduces the charge recombination loss caused by crystal defects, improves the photoelectric conversion efficiency, provides high-quality material guarantee for high-performance solar cells, and is precisely controlled and Ultrasonic assisted cleaning ensures surface cleanliness and process stability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a perovskite crystalline silicon laminated solar cell preparation method based on interface modification, and relates to the technical field of cell preparation, and the method specifically comprises the following steps: firstly, preparing raw materials, cleaning a textured crystalline silicon wafer by using deionized water, acetone and ethanol in sequence, and carrying out surface modification on the textured crystalline silicon wafer at room temperature; and depositing niox on the n surface of the pre-cleaned crystal silicon wafer through sputtering of a radio-frequency power supply, and setting the pressure of a cavity to be 0.3-0.4 Pa and the radio-frequency power to be 100-200W. The method has the advantages that the high integrity and few defects of the crystal structure of the monocrystalline silicon wafer are ensured by careful selection of the monocrystalline silicon wafer, the high-quality monocrystalline silicon wafer has lower dislocation density and impurity content, and the quality of the monocrystalline silicon wafer is improved. Therefore, a solid foundation is laid for subsequent preparation of the solar cell, charge recombination loss caused by crystal defects can be remarkably reduced when the cell works, current conduction is smoother and more efficient, the photoelectric conversion efficiency is greatly improved, and a high-quality material guarantee is provided for realizing the high-performance solar cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery preparation, and in particular to a method for preparing a perovskite crystalline silicon stacked solar cell based on interface modification. Background Art

[0002] As the global demand for clean energy continues to grow, the development of solar cell technology has received widespread attention. As a new type of solar cell with great potential, the key to improving the efficiency of perovskite crystalline silicon tandem solar cells lies in the optimization of the preparation method. This article introduces the preparation process of perovskite crystalline silicon tandem solar cells in detail, including the preparation of crystalline silicon bottom cells, the preparation of perovskite top cells, and the processing of the intermediate connection layer. It also discusses the key technologies and challenges in each step and looks forward to future development trends.

[0003] Perovskite silicon tandem solar cells are a promising solar cell technology. Continuous optimization and innovation of their preparation methods will lay the foundation for achieving higher photoelectric conversion efficiency and practical applications. However, they still face many technical challenges. Scientific researchers need to continue to conduct in-depth research in materials, processes and equipment to promote the rapid development and widespread application of this technology. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a perovskite crystalline silicon tandem solar cell based on interface modification.

[0005] In order to solve the problems raised in the above background technology, the present invention provides the following technical solution: a method for preparing a perovskite crystalline silicon tandem solar cell based on interface modification, comprising the following steps:

[0006] First prepare the raw materials, and then follow the steps below:

[0007] S1, using deionized water, acetone and ethanol to clean the textured crystalline silicon wafer in sequence;

[0008] S2. At room temperature, niox is deposited onto the n-side of the pre-cleaned crystalline silicon wafer by sputtering with a radio frequency power supply, the chamber pressure is set to 0.3-0.4 Pa, the radio frequency power is set to 100-200 W, the argon gas flow rate is set to 10-30 sccm, and the duration is 10-15 min to form a shj crystalline silicon substrate;

[0009] S3, dissolving (2-(3,6-dimethoxy-9h-carbazole-9-yl)ethyl)phosphonic acid in anhydrous ethanol, stirring in a nitrogen glove box to form a mixed solution with a concentration of 0.5-1.5 mg / ml, spin coating the mixed solution on the surface of the SHJ crystalline silicon substrate at a rotation speed of 2000-4000 rpm for 30 seconds in the nitrogen glove box, and then heat treating at 100-200° C. for 10-30 minutes to form a pretreated SHJ crystalline silicon substrate;

[0010] S4, using an evaporation device, setting an appropriate evaporation rate, and evaporating to form a Pb I2 thin film on the pre-treated shj crystalline silicon substrate;

[0011] S5. Use atomic layer deposition technology to process the Pb I2 film: place the SHJ crystalline silicon substrate containing the Pb I2 film in the chamber of the atomic layer deposition equipment, control the temperature in the chamber to be lower than 70°C, use a water pulse purge time of 20ms, and perform nitrogen purification for 10s, and repeat for 50 cycles;

[0012] S6. Add formamidine hydroiodide, methylamine hydrobromide and methylamine hydrochloride to isopropanol, stir and mix to form a uniform solution, wherein the concentration of formamidine hydroiodide is 80-90 mg / ml, the concentration of methylamine hydrobromide is 10-15 mg / ml, and the concentration of methylamine hydrochloride is 5-10 mg / ml, and spin-coat the solution on the surface of the Pb I2 thin film layer treated by atomic layer deposition technology at a speed of 2000-30000 rpm in air with a humidity of 5% for 30 seconds, and anneal for 25-35 minutes at a humidity of 35-50% and a temperature of 100-200°C to form a perovskite layer;

[0013] S7, sequentially evaporating a lithium fluoride layer with a thickness of 1-3 nm and a fullerene layer with a thickness of 20-30 nm on the perovskite layer, and then depositing a tin oxide layer by atomic layer deposition technology: placing tetrakis(dimethylamino)tin in the chamber of the atomic layer deposition equipment, maintaining the temperature in the chamber below 100°C, with a pulse length of 100 ms, and then purging with nitrogen for 20 s, followed by injecting a 20 ms water pulse, and then purging with nitrogen for 25 s, and repeating for 160 cycles. During the cycle, nitrogen is used as a carrier gas, and the nitrogen flow rate is set to 20 sccm;

[0014] S8. At room temperature, by DC sputtering, an indium zinc oxide layer with a thickness of 80-100 nm is deposited on the surface of the tin oxide layer, and a silver grid with a thickness of 80-100 nm is thermally evaporated around the indium zinc oxide layer, and then a magnesium fluoride anti-reflection layer with a thickness of 80-100 nm is evaporated, and a silver grid with a thickness of 100 nm is evaporated on the p-side of the crystalline silicon wafer.

[0015] As a further solution of the present invention: the materials required for preparation in the present application include high-purity single crystal silicon wafers, organic lead halides, organic amine salts, halides, hole transport materials, electron transport materials, metal electrode materials, solvents, and passivation materials.

[0016] As a further embodiment of the present invention, the organic lead halide includes methyl lead iodide (MAPbI3) and formamidine lead iodide (FAPbI3), the organic amine salt includes methylamine (MA) and formamidine (FA), and the halide includes iodide (I - ), bromide (Br - ), the hole transport material includes 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (spiro-OMeTAD), the electron transport material includes a fullerene derivative (such as PCBM), the metal electrode material includes gold (Au), silver (Ag), aluminum (Al), the solvent is dimethyl sulfoxide (DMSO), and the passivation material includes silicon oxide (SiO2).

[0017] As a further scheme of the present invention: the organic lead halide is prepared by weighing a certain amount of lead powder and potassium iodide, dissolving them in deionized water according to a stoichiometric ratio (usually 1:2) to obtain two solutions, then adding an appropriate amount of surfactant to the potassium iodide solution and stirring evenly to improve the dispersibility and morphology control of the product in the subsequent reaction, slowly dropping the lead powder solution into the potassium iodide solution, and turning on a magnetic stirrer to fully mix the reaction system, and then placing the mixed solution in an ultrasonic generator, utilizing the cavitation effect and mechanical vibration of ultrasound to accelerate the reaction and promote the uniform growth and crystallization of the product, stopping ultrasound after a period of reaction, and allowing the solution to stand for a period of time to precipitate the product, and obtaining pure lead iodide powder through filtering, washing and drying.

[0018] As a further scheme of the present invention: the hole transport material is prepared by dissolving spirobifluorene and methoxyaniline in dry toluene under nitrogen protection, adding an appropriate amount of palladium catalyst, heating the reaction system to a certain temperature, and keeping stirring to allow the reaction to proceed for a period of time, slowly adding an oxidant ammonium persulfate to the reaction solution, while continuing to stir and heat to promote the oxidation reaction, then adding alkaline potassium carbonate to neutralize the acidic substances produced during the reaction, cooling to room temperature after the reaction is completed, filtering to remove insoluble impurities, distilling the filtrate under reduced pressure to remove most of the solvent to obtain a concentrated solution, freeze-drying the concentrated solution to obtain pure spiro-OMeTAD powder, and then making the hole transport material.

[0019] By adopting the above technical solution, compared with the prior art, the beneficial effects of the present invention are:

[0020] 1. The present invention carefully selects single crystal silicon wafers to ensure the high integrity and few defects of its crystal structure. High-quality single crystal silicon wafers have lower dislocation density and impurity content, which lays a solid foundation for the subsequent preparation of solar cells. When the battery is working, it can significantly reduce the charge recombination loss caused by crystal defects, making the current conduction smoother and more efficient, thereby greatly improving the photoelectric conversion efficiency and providing high-quality material guarantee for the realization of high-performance solar cells;

[0021] 2. The present invention uses high-purity deionized water in the cleaning step and combines it with advanced ultrasound or megasonic wave assisted technology, showing significant advantages. High-purity deionized water effectively avoids secondary contamination of the silicon wafer surface by residual ions and impurities in the water, while ultrasound or megasonic wave assisted technology can produce strong vibration and cavitation effects, penetrate into the tiny pores and grooves on the surface of the silicon wafer, and completely remove tiny particles and stubborn organic residues, creating an extremely pure and smooth surface environment for subsequent thin film deposition;

[0022] 3. The pickling process of the present invention exhibits excellent selective removal ability by precisely controlling the acid concentration, temperature and treatment time. This precise control enables the pickling to specifically remove metal impurities and natural oxide layers on the surface of the silicon wafer, while minimizing excessive corrosion to the silicon wafer body. This not only ensures the cleanliness of the silicon wafer surface, but also maintains the structural integrity of the silicon wafer, providing an ideal surface state for subsequent process steps, which helps to improve the performance and stability of solar cells. DETAILED DESCRIPTION

[0023] The specific embodiments of the present invention are further described. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention.

[0024] In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0025] The present invention provides a method for preparing a perovskite crystalline silicon tandem solar cell based on interface modification, which specifically comprises the following steps:

[0026] Step 1: Preparation and cleaning of crystalline silicon wafers. Prepare the textured crystalline silicon wafers and clean them thoroughly with deionized water, acetone and ethanol in sequence.

[0027] Step 2: Preparation and processing of crystalline silicon substrate

[0028] Niox is deposited on the n-side of the cleaned crystalline silicon wafer by sputtering with a radio frequency power supply to form a shj crystalline silicon substrate, and a specific material is dissolved in anhydrous ethanol to form a mixed liquid, which is spin-coated and heat-treated in a nitrogen glove box to pretreat the shj crystalline silicon substrate.

[0029] Step 3: Preparation of perovskite layer and related thin films, evaporation of PBI2 thin film, and treatment using atomic layer deposition technology, preparation of a specific solution, spin coating and annealing to form a perovskite layer, sequentially depositing a lithium fluoride layer and a fullerene layer on the perovskite layer, and then depositing a tin oxide layer using atomic layer deposition technology.

[0030] Step 4: Deposition of electrodes and anti-reflection layers

[0031] An indium zinc oxide layer and a silver grid are deposited at corresponding positions by direct current sputtering and thermal evaporation, a magnesium fluoride anti-reflection layer is evaporated, and a silver grid is evaporated on the p-side of the crystalline silicon wafer.

[0032] In one embodiment of the present invention, the organic lead halide includes methyl lead iodide (MAPbI3) and formamidine lead iodide (FAPbI3), the organic amine salt includes methylamine (MA) and formamidine (FA), and the halide includes iodide (I - ), bromide (Br - ), the hole transport material includes 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (spiro-OMeTAD), the electron transport material includes a fullerene derivative (such as PCBM), the metal electrode material includes gold (Au), silver (Ag), aluminum (Al), the solvent is dimethyl sulfoxide (DMSO), and the passivation material includes silicon oxide (SiO2).

[0033] In one embodiment of the present invention, the organic lead halide is prepared by weighing a certain amount of lead powder and potassium iodide, dissolving them in deionized water according to a stoichiometric ratio (usually 1:2) to obtain two solutions, then adding an appropriate amount of surfactant to the potassium iodide solution and stirring evenly to improve the dispersibility and morphology control of the product in the subsequent reaction, slowly dropping the lead powder solution into the potassium iodide solution, and turning on a magnetic stirrer to fully mix the reaction system, and then placing the mixed solution in an ultrasonic generator to accelerate the reaction by utilizing the cavitation effect and mechanical vibration of ultrasound, and promote the uniform growth and crystallization of the product. After a period of reaction, stop the ultrasound, let the solution stand for a period of time to precipitate the product, and obtain pure lead iodide powder through filtering, washing and drying.

[0034] Example 1: Ultrasonic assisted cleaning mainly relies on the cavitation effect, mechanical vibration and micro-jet effect generated by ultrasonic waves in liquid media. When ultrasonic waves propagate in the cleaning liquid, tiny bubbles will be formed locally. These bubbles will undergo a process of generation, expansion and collapse in a very short period of time. At the moment of bubble collapse, high temperature, high pressure and strong impact force will be generated, forming tiny local hot spots. This cavitation effect can effectively remove tiny particles and stubborn pollutants on the surface of the crystalline silicon wafer. For those tiny particles tightly attached to the surface of the crystalline silicon wafer, traditional cleaning methods may be difficult to completely remove them, but the strong impact force generated by ultrasound can make them detach from the surface. The mechanical vibration caused by ultrasound can promote the rapid flow and penetration of the cleaning liquid on the surface of the crystalline silicon wafer, ensuring that the cleaning liquid is in full contact with the entire surface, thereby improving the uniformity and consistency of cleaning. The micro-jet effect further enhances the flushing effect of the cleaning liquid on the surface. , which helps to remove deep-seated impurities and dirt. Ultrasonic-assisted cleaning can also shorten the cleaning time and improve the cleaning efficiency. It can achieve the ideal cleaning effect more quickly without damaging the surface of the crystalline silicon wafer, and provide a highly clean and pollution-free surface condition for the subsequent process steps. In summary, adding an ultrasonic-assisted cleaning step in the crystalline silicon wafer cleaning process can significantly improve the cleaning effect, ensure the quality of the crystalline silicon wafer, and lay a solid foundation for the subsequent preparation process. When using deionized water, acetone and ethanol for cleaning in sequence, they are all carried out in an ultrasonic environment. Ultrasonic assistance can enhance the cleaning effect, more effectively remove tiny pollutants and impurities on the surface of the crystalline silicon wafer, improve the cleanliness of the cleaning, and provide a more ideal substrate for subsequent thin film deposition, which helps to improve the performance and stability of the battery.

[0035] Embodiment 2: First, the real-time monitoring system will continuously collect chamber pressure data. The stability of chamber pressure directly affects the mean free path and collision frequency of sputtered particles. Through high-precision pressure sensors, subtle changes in pressure can be obtained instantly. When the pressure fluctuates and deviates from the preset value, the feedback system responds quickly. It will automatically adjust the intake and exhaust rates according to the preset algorithm and control logic to quickly restore the chamber pressure and stabilize it within the ideal range. Monitoring and regulation of RF power is also extremely critical. RF power determines the energy and sputtering rate of sputtered particles. The real-time monitoring system will accurately measure the actual applied RF power and compare it with the set value. Once a deviation is found, the feedback system will immediately fine-tune the RF power supply to ensure the RF power. It is always in the best state to ensure that the sputtered particles have appropriate energy and achieve uniform and high-quality thin film deposition. The argon flow rate is also one of the important factors affecting the sputtering effect. As a sputtering gas, the flow rate of argon will affect the collision and migration process of the sputtered particles. The real-time monitoring system will accurately sense the changes in the argon flow rate. When the flow rate deviates from the set value, the feedback system will adjust the gas flow controller to adjust the argon supply in time to maintain a stable and appropriate argon flow rate, provide a stable gas environment for the sputtering process, and ensure the performance and quality of the film to achieve a more uniform and dense niox film deposition, which can better control the quality and performance of the film, reduce defects and non-uniformity in the film, and improve the electrical properties of the crystalline silicon substrate, thereby improving the conversion efficiency of the battery.

[0036] Example 3: Introducing new additives, such as organic amine stabilizers, to optimize the formula of the perovskite solution can help improve the crystallization quality and stability of the perovskite film, reduce defects in the film, extend the service life of the battery and improve efficiency.

[0037] Example 4: Using magnetron sputtering technology to deposit the indium zinc oxide layer and the silver grid, while optimizing the sputtering process parameters, magnetron sputtering can improve the deposition rate and uniformity of the film, reduce the resistance of the electrode, enhance the charge collection efficiency, and further improve the performance of the battery

[0038] Specifically, first select high-purity indium zinc oxide target and silver target, then fix the pre-processed samples (i.e., the surface of the tin oxide layer, the p-side of the silicon wafer, etc.) on the substrate holder to ensure that the substrate surface is clean and flat, and then use argon as the main sputtering gas, and accurately set the flow rate of argon through the gas flow controller, for example, it can be set to 20-30sccm. As needed, a small amount of oxygen (e.g., 1-3sccm) or nitrogen (e.g., 0.5-1.5sccm) can be mixed into the argon to optimize the film performance. For the deposition of the indium zinc oxide layer, the sputtering power can be set between 100-150W; for the deposition of the silver grid, the sputtering power can be set between 120-180W. However, in actual operation, fine-tuning is required according to the film growth conditions;

[0039] Adjust the distance between the substrate and the target material to 6-8 cm to obtain a suitable deposition effect, control the sputtering gas pressure within the range of 0.2-0.5 Pa, and start the magnetron sputtering equipment. During the sputtering process, monitor the film thickness through a real-time film thickness monitor. When it reaches 80-100 nm, stop sputtering of the corresponding target material.

[0040] Working principle:

[0041] The working principle of perovskite crystalline silicon stacked solar cells is based on the synergistic effect of crystalline silicon bottom cells and perovskite top cells. The crystalline silicon bottom cell is composed of P-type and N-type silicon materials to form a PN junction. When sunlight irradiates the crystalline silicon bottom cell, photons with energy greater than the silicon bandgap width are absorbed, generating electron-hole pairs. Under the action of the built-in electric field, electrons move to the N region and holes move to the P region, forming photocurrent and photovoltage. Since crystalline silicon has a good absorption capacity for long-wavelength light, it mainly absorbs the energy of this part of the spectrum. The perovskite top cell also produces a photoelectric effect under light. The perovskite material has a unique band structure and can absorb short-wavelength light. Photons of different wavelengths stimulate the generation of electron-hole pairs. The electron transport layer and hole transport layer set in the perovskite top cell collect and transmit electrons and holes respectively. The intermediate connecting layer plays a key bridge role. Through the tunneling recombination junction, the electrons generated by the crystalline silicon bottom cell and the holes generated by the perovskite top cell can efficiently recombine, and vice versa, thereby realizing the effective transmission of charges. At the same time, the optical matching layer optimizes the propagation and absorption of light in the entire cell structure, reducing reflection and loss. The synergy of the two enables the cell to absorb the sunlight spectrum more widely, greatly improving the utilization efficiency of solar energy, thereby achieving higher photoelectric conversion efficiency.

[0042] At the same time, the present application uses specific words to describe the embodiments of the present application. For example, "one embodiment", "an embodiment", and / or "some embodiments" refer to a certain feature, structure or characteristic related to at least one embodiment of the present application. Therefore, it should be emphasized and noted that "one embodiment" or "an embodiment" or "an alternative embodiment" mentioned twice or more in different positions in this specification does not necessarily refer to the same embodiment. In addition, certain features, structures or characteristics in one or more embodiments of the present application can be appropriately combined.

[0043] Some aspects of the present application may be performed entirely by hardware, entirely by software (including firmware, resident software, microcode, etc.), or by a combination of hardware and software. The above hardware or software may be referred to as "data blocks", "modules", "engines", "units", "components" or "systems". The processor may be one or more application specific integrated circuits (ASICs), digital signal processors (DSPs), digital signal processing devices (DAPDs), programmable logic devices (PLDs), field programmable gate arrays (FPGAs), processors, controllers, microcontrollers, microprocessors, or combinations thereof. In addition, various aspects of the present application may be expressed as computer products located in one or more computer-readable media, which include computer-readable program codes. For example, computer-readable media may include, but are not limited to, magnetic storage devices (e.g., hard disks, floppy disks, tapes ...), optical disks (e.g., compact disks CDs, digital versatile disks DVDs ...), smart cards, and flash memory devices (e.g., cards, sticks, key drives ...).

[0044] A computer-readable medium may include a propagated data signal containing computer program code, such as in baseband or as part of a carrier wave. The propagated signal may have a variety of manifestations, including electromagnetic, optical, etc., or a suitable combination. A computer-readable medium may be any computer-readable medium other than a computer-readable storage medium, which may be connected to an instruction execution system, device or apparatus to communicate, propagate or transmit a program for use. The program code on the computer-readable medium may be propagated through any suitable medium, including radio, cable, fiber optic cable, radio frequency signal, or similar medium, or a combination of any of the above mediums.

[0045] Similarly, it should be noted that in order to simplify the description disclosed in this application, so as to help understand one or more embodiments of the invention, in the above description of the embodiments of the present application, multiple features are sometimes merged into one embodiment. However, this disclosure method does not mean that the features required by the object of the present application are more than the features mentioned in the claims. In fact, the features of the embodiment are less than all the features of the single embodiment disclosed above. In some embodiments, numbers describing the number of components and attributes are used. It should be understood that such numbers used in the description of the embodiments are modified by the modifiers "approximately", "approximately" or "substantially" in some examples. Unless otherwise specified, "approximately", "approximately" or "substantially" indicate that the number allows a change of ±20%. Accordingly, in some embodiments, the numerical parameters used in the specification and claims are approximate values, which may change according to the required features of individual embodiments. In some embodiments, the numerical parameters should take into account the specified significant digits and adopt the general method of retaining the digits. Although the numerical domains and parameters used to confirm the breadth of their range in some embodiments of the present application are approximate values, in specific embodiments, such numerical settings are as accurate as possible within the feasible range.

[0046] Although the present invention is disclosed as above in terms of preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art may make possible changes and modifications without departing from the spirit and scope of the present invention. Therefore, any modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention shall fall within the scope of protection defined by the claims of the present invention.

Claims

1. A method for preparing a perovskite crystalline silicon tandem solar cell based on interface modification, characterized in that: First prepare the raw materials, and then follow the steps below: S1, using deionized water, acetone and ethanol to clean the textured crystalline silicon wafer in sequence; S2. At room temperature, niox is deposited onto the n-side of the pre-cleaned crystalline silicon wafer by sputtering with a radio frequency power supply, the chamber pressure is set to 0.3-0.4 Pa, the radio frequency power is set to 100-200 W, the argon gas flow rate is set to 10-30 sccm, and the duration is 10-15 min to form a shj crystalline silicon substrate; S3, dissolving (2-(3,6-dimethoxy-9h-carbazole-9-yl)ethyl)phosphonic acid in anhydrous ethanol, stirring in a nitrogen glove box to form a mixed solution with a concentration of 0.5-1.5 mg / ml, spin coating the mixed solution on the surface of the SHJ crystalline silicon substrate at a rotation speed of 2000-4000 rpm for 30 seconds in the nitrogen glove box, and then heat treating at 100-200° C. for 10-30 minutes to form a pretreated SHJ crystalline silicon substrate; S4, using an evaporation device, setting an appropriate evaporation rate, and evaporating to form a PBI2 thin film on the pre-treated SHJ crystalline silicon substrate; S5. Use atomic layer deposition technology to process the PBI2 film: place the SHJ crystalline silicon substrate containing the PBI2 film in the chamber of the atomic layer deposition equipment, control the temperature in the chamber to be lower than 70°C, use a water pulse purge time of 20ms, and perform nitrogen purification for 10s, and repeat for 50 cycles; S6. Add formamidine hydroiodide, methylamine hydrobromide and methylamine hydrochloride to isopropanol, stir and mix to form a uniform solution, wherein the concentration of formamidine hydroiodide is 80-90 mg / ml, the concentration of methylamine hydrobromide is 10-15 mg / ml, and the concentration of methylamine hydrochloride is 5-10 mg / ml, and spin-coat it on the surface of the PBI2 thin film layer treated by atomic layer deposition technology at a speed of 2000-30000 rpm in air with a humidity of 5% for 30 seconds, and anneal it at a humidity of 35-50% and a temperature of 100-200°C for 25-35 minutes to form a perovskite layer; S7, sequentially evaporating a lithium fluoride layer with a thickness of 1-3 nm and a fullerene layer with a thickness of 20-30 nm on the perovskite layer, and then depositing a tin oxide layer by atomic layer deposition technology: placing tetrakis(dimethylamino)tin in the chamber of the atomic layer deposition equipment, maintaining the temperature in the chamber below 100°C, with a pulse length of 100 ms, and then purging with nitrogen for 20 s, followed by injecting a 20 ms water pulse, and then purging with nitrogen for 25 s, and repeating for 160 cycles. During the cycle, nitrogen is used as a carrier gas, and the nitrogen flow rate is set to 20 sccm; S8. At room temperature, by DC sputtering, an indium zinc oxide layer with a thickness of 80-100 nm is deposited on the surface of the tin oxide layer, and a silver grid with a thickness of 80-100 nm is thermally evaporated around the indium zinc oxide layer, and then a magnesium fluoride anti-reflection layer with a thickness of 80-100 nm is evaporated, and a silver grid with a thickness of 100 nm is evaporated on the p-side of the crystalline silicon wafer.

2. The method for preparing a perovskite crystalline silicon tandem solar cell based on interface modification according to claim 1, characterized in that: The materials required for preparation in the present application include high-purity single crystal silicon wafers, organic lead halides, organic amine salts, halides, hole transport materials, electron transport materials, metal electrode materials, solvents, and passivation materials.

3. The method for preparing a perovskite crystalline silicon tandem solar cell based on interface modification according to claim 2, characterized in that: The organic lead halide includes methyl lead iodide (MAPbI3) and formamidine lead iodide (FAPbI3), the organic amine salt includes methylamine (MA) and formamidine (FA), the halide includes iodide (I - ), bromide (Br - ), the hole transport material includes 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (spiro-OMeTAD), the electron transport material includes a fullerene derivative (such as PCBM), the metal electrode material includes gold (Au), silver (Ag), aluminum (Al), the solvent is dimethyl sulfoxide (DMSO), and the passivation material includes silicon oxide (SiO2).

4. The method for preparing a perovskite crystalline silicon tandem solar cell based on interface modification according to claim 3, characterized in that: The organic lead halide is prepared by weighing a certain amount of lead powder and potassium iodide, dissolving them in deionized water according to a stoichiometric ratio (usually 1:2) to obtain two solutions, then adding an appropriate amount of surfactant to the potassium iodide solution and stirring evenly to improve the dispersibility and morphology control of the product in the subsequent reaction, slowly dropping the lead powder solution into the potassium iodide solution, and turning on a magnetic stirrer to fully mix the reaction system, then placing the mixed solution in an ultrasonic generator, utilizing the cavitation effect and mechanical vibration of ultrasonic waves to accelerate the reaction and promote uniform growth and crystallization of the product, stopping the ultrasound after a period of reaction, allowing the solution to stand for a period of time to precipitate the product, and obtaining pure lead iodide powder through filtering, washing, drying and other steps.

5. The method for preparing a perovskite crystalline silicon tandem solar cell based on interface modification according to claim 3, characterized in that: The hole transport material is prepared by dissolving spirobifluorene and methoxyaniline in dry toluene under nitrogen protection, adding a proper amount of palladium catalyst, heating the reaction system to a certain temperature, and stirring to allow the reaction to proceed for a period of time, slowly adding an oxidant, ammonium persulfate, to the reaction solution, while continuing to stir and heat to promote the oxidation reaction, then adding alkaline potassium carbonate to neutralize the acidic substances generated during the reaction, cooling to room temperature after the reaction is completed, filtering to remove insoluble impurities, performing reduced pressure distillation on the filtrate to remove most of the solvent to obtain a concentrated solution, and performing freeze-drying on the concentrated solution to obtain pure spiro-OMeTAD powder, which is then prepared into a hole transport material.