Red mud base-biogas residue composite material as well as preparation method and application thereof

By combining red mud with slag biochar to form a highly adsorption-active red mud-based-slag composite material, the problem of unsatisfactory adsorption performance of traditional red mud-based ceramic particles when treating organic matter and anionic pollutants is solved, and the problem of unsatisfactory adsorption performance of traditional red mud-based ceramic particles is achieved. Inexpensive and efficient water treatment materials, and the materials are easy to separate and recycle.

CN119056407APending Publication Date: 2024-12-03HUNAN RENHE ENVIRONMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411448874.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-17
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Traditional red mud-based ceramic particles have poor adsorption performance when dealing with organic matter and anionic contaminants, and activated carbon particles are small and difficult to separate and costly, making it a challenge to find cheap and efficient water treatment materials.

Method used

By combining red mud with slag biochar, the inorganic minerals in the red mud are coated and bonded to the surface and interior of the slag biochar, a highly adsorption-active magnetite is generated to form a red mud-based-slag composite Materials, which increase particle size and improve adsorption performance, are prepared into different shapes to meet the needs of different pollutants.

Benefits of technology

The adsorption effect of red mud-based sludge-slag composite materials on nitrogen and phosphorus is significantly improved, production costs are reduced, and the materials are easily separated and recycled, and high adsorption capacity and efficiency are shown in wastewater treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056407A_ABST
    Figure CN119056407A_ABST
Patent Text Reader

Abstract

The invention discloses a red mud-biogas residue biochar composite nitrogen and phosphorus adsorption material and a preparation method thereof.The method comprises the steps that raw materials containing red mud and biogas residues are compounded and mixed and shaped according to different needs, and then a red mud-biogas residue precursor material is obtained; and pyrolyzing the red mud-based biogas residue precursor material at 300-900 DEG C under an anaerobic condition to obtain the adsorbing material with abundant pores. In addition, the material can be applied to a treatment scene of nitrogen and phosphorus wastewater, and shows excellent adsorption performance compared with an original material. The nitrogen and phosphorus removal cost in the wastewater can be reduced, and nitrogen and phosphorus elements in the wastewater can be recycled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite adsorption material preparation, and relates to a red mud-based biogas residue composite material and a preparation method and application thereof. Background Art

[0002] In today's society, environmental issues have become the focus of global attention, especially water pollution, which has attracted great attention. With the accelerated development of industrialization and urbanization, a large amount of industrial wastewater and domestic sewage are discharged, which seriously threatens the safety of water resources and human health. Therefore, the development of efficient, economical and environmentally friendly water treatment technology has become an important issue that needs to be solved in the current environmental protection field.

[0003] Among the numerous water treatment technologies, adsorption has received extensive attention and application due to its advantages such as simple operation, low cost and good treatment effect. The adsorption method mainly relies on the physical adsorption and chemical adsorption between the adsorbent and the pollutant to achieve the removal of pollutants. Among them, the selection of adsorbent is a key factor affecting the adsorption effect. Traditional adsorbents, such as activated carbon, have good adsorption properties, but they are relatively expensive and are easily separated from the water body during the water treatment process, which brings certain difficulties to subsequent treatment and recovery.

[0004] In recent years, with the continuous exploration of environmentally friendly materials, a new type of adsorbent, red mud-based ceramsite, has gradually attracted people's attention. Red mud, as a solid waste generated in the production process of aluminum plants, has a huge emission volume and a low comprehensive utilization rate. The main structure of red mud is similar to that of clay. It contains rich metal elements such as iron, aluminum, silicon, etc. and has good adsorption properties. By calcining red mud with various solid wastes or materials with adsorption properties, ceramsite with a certain strength for water treatment can be prepared. This red mud-based ceramsite can not only effectively adsorb pollutants in water, but also has good physical and chemical stability, and can maintain good adsorption properties in a wide pH range. In addition, the preparation process of red mud-based ceramsite can also realize the resource utilization of solid waste, with high environmental and economic benefits.

[0005] However, the adsorption performance of traditional red mud-based ceramsite is not ideal when dealing with certain specific pollutants, such as organic matter and anionic pollutants. In order to solve this problem, biochar prepared from biomass as raw materials has gradually become a research hotspot in recent years. Biochar, as a new type of activated carbon, has high porosity and specific surface area, and has good adsorption performance for organic and anionic pollutants. Activated carbon (biochar) made from biomass as raw materials has good adsorption performance for organic and anionic pollutants and is widely used in water treatment. However, the activated carbon particles are small, difficult to separate from water bodies and have a high price. Therefore, finding cheap, efficient and easy-to-separate water treatment materials remains a hot spot in the research and development of related industries. Summary of the invention

[0006] In order to solve the problems existing in the prior art, the first object of the present invention is to provide a red mud-based-sludge biochar composite material, which utilizes inorganic minerals in red mud to form mineral coatings and bonding layers in the porous structure on the surface and inside of the sludge biochar. At the same time, the metal oxides in the red mud undergo phase changes during the pyrolysis process to generate a new mineral phase (magnetite) with high adsorption activity, which also coats and penetrates the sludge biochar. On the one hand, the particle size of the red mud-sludge composite material is increased, making it easy to separate from the water body and recycle. On the other hand, the adsorption material can be prepared into different shapes according to the usage scenarios and the conditions of nitrogen and phosphorus pollutants, including but not limited to spherical, plate and honeycomb shapes. The two synergistically significantly improve the adsorption of nitrogen and phosphorus by the red mud-sludge composite material.

[0007] The second object of the present invention is to provide a method for preparing a red mud-based-sludge composite nitrogen and phosphorus adsorption material. The preparation method simultaneously realizes the carbonization of the sludge, the inorganic mineral coating of the red mud and the metal oxide phase change of the red mud by controlling the temperature during the pyrolysis process. This not only significantly reduces the production cost of the adsorbent, alleviates the problem of a large amount of solid waste having nowhere to go, and realizes resource utilization; the process flow is simple and the effect is significant.

[0008] The third object of the present invention is to provide an application of a red mud-based biogas residue composite material, which is used as an adsorption material for the adsorption of nitrogen and / or phosphorus in sewage, and has the advantages of large adsorption capacity and high adsorption efficiency through the combined action of physical adsorption and chemical adsorption. It is worth noting that the material of the present invention is rich in nitrogen and phosphorus after adsorption, and has the potential to be applied to the soil as a fertilizer to provide nutrition for crops, thus realizing the resource utilization of nitrogen and phosphorus.

[0009] In order to achieve the above technical objectives, the present invention provides a method for preparing a red mud-based-sludge biochar composite nitrogen and phosphorus adsorption material, which comprises mixing and shaping raw materials containing red mud and sludge to obtain a red mud-based-sludge precursor material; the red mud-based-sludge precursor material is pyrolyzed at 300 to 900°C under anaerobic conditions to obtain the material.

[0010] In the technical solution of the present invention, biogas residue contains a high content of organic matter and nutrients, while red mud contains rich inorganic minerals (such as Fe2O3, Al2O3, CaO, etc.). During the pyrolysis process, the organic matter in the biogas residue will decompose to form biogas residue biochar with a high specific surface area and a porous structure. At the same time, the red mud will also change during the pyrolysis process. The inorganic minerals in the red mud can form biochar by complexing, adsorption, electronic coordination and coprecipitation with the organic matter in the biogas residue. During the formation of biochar, the biochar is coated, filled and infiltrated synchronously, forming a firm mineral coating and bonding layer on the surface and inside of the biochar. At the same time, the metal oxides in the red mud undergo a phase change during the pyrolysis process, generating a new mineral phase (magnetite) with high adsorption activity, which is also coated and infiltrated in the biogas residue biochar, increasing the particle size of the red mud-biogas residue composite material, making it easy to separate from the water body and recycle. In addition, the surface of the biogas residue biochar after pyrolysis is rich in functional groups such as carbonyl, hydroxyl and carboxyl, which enhance the chemical affinity between the composite material and the nitrogen and phosphorus compounds.

[0011] The key to the technical solution of the present invention is to control the temperature of pyrolysis. The temperature range of pyrolysis of the present invention satisfies both the carbonization of organic matter in biogas residue and the phase change of metal oxides in red mud. In addition, the pyrolysis temperature range of the present invention is conducive to improving the stability of the composite material in water. If the pyrolysis temperature of the present invention is too low, not only the material cannot be formed but also the phase change cannot occur; if the pyrolysis temperature is too high, the preparation cost will increase, and the adsorption performance will not be significantly improved. It is further preferred that the pyrolysis temperature is 600-800°C.

[0012] At the same time, the inventors found that the preparation process of the present invention needs to be carried out under anaerobic conditions. The anaerobic conditions are for the purpose of forming biochar, carbonizing organic matter, and forming a porous material. If it is not carried out under anaerobic conditions, the organic matter will volatilize at high temperature, and what remains will be ash, and biochar cannot be formed. In actual operation, a protective atmosphere such as nitrogen is introduced.

[0013] As a preferred solution, the organic matter content in the biogas residue is greater than 50wt%, wherein the organic matter is calculated as the C element content. The biogas residue used in the present invention has a high organic matter content and nutrient elements, which makes the biogas residue biochar formed after pyrolysis have better adsorption performance and soil improvement effect.

[0014] As a preferred solution, the content of Fe2O3 in the red mud is 42-45wt.%, the content of Al2O3 is 20-23wt.%, the content of CaO is 0.5-1wt.%, the content of SiO2 is 14-18wt.%, and the remainder is impurities. The high content of Fe2O3 in the red mud of the present invention ensures that the red mud undergoes phase change during the pyrolysis process to generate a sufficient amount of new mineral phase (magnetite) with high adsorption activity. As a preferred solution, the mass ratio of the red mud to the biogas residue is (2-3):1. The amount of red mud used in the present invention is greater than that of biogas residue. This is because red mud serves as a skeleton in the composite material, and a sufficient amount of red mud must be ensured to ensure material molding; when the red mud content is too low, the material morphology will be unstable, thereby causing the adsorption performance of the composite material to decrease.

[0015] As a preferred solution, the pyrolysis time is 1 to 3 hours. By controlling the pyrolysis time, the carbonization effect of the biogas residue and the coating and phase change degree of the red mud can be controlled, and within the time range of the present invention, the optimal effect is achieved.

[0016] As a preferred solution, the particle sizes of the red mud and biogas residue are both less than 100 meshes. By controlling the particle sizes of the red mud and biogas residue raw materials, sufficient reaction between the two substances can be ensured during the pyrolysis process.

[0017] The present invention provides a method for preparing a red mud-based biogas residue composite material, which specifically comprises the following steps:

[0018] 1) The obtained red mud is dried and then crushed in a crusher to obtain red mud powder (raw material 1). Raw material 1 is collected and placed in a drying dish for later use. The obtained biogas residue is dried to constant weight, crushed in a crusher, and then taken out to obtain biogas residue powder (raw material 2). Raw material 2 is collected and placed in a drying dish for later use.

[0019] 2) Mix the raw material 1 and raw material 2 obtained in step 1) in different proportions, add deionized water, put them into a blender and stir them for a certain period of time until they become viscous, then take them out and put them into a mold for shaping. After shaping, air dry them until they can be demolded and taken out.

[0020] 3) placing the air-dried composite material obtained in step 2) in an oven for drying, taking it out and placing it in a closed calcining furnace, pyrolyzing it in a tubular furnace under oxygen-free conditions for a certain period of time, and taking it out after cooling to obtain a composite adsorption material.

[0021] As a preferred solution, the shaped shape is a sphere, a pancake, etc.

[0022] The present invention also provides a red mud-based biogas residue composite material obtained by the above preparation method.

[0023] As a preferred solution, the red mud-based biogas residue composite material has a porous structure with a specific surface area of ​​15.27 to 28.94 m 2 / g, and the average pore size is 12.75-14.93nm. The composite material of the present invention has a porous structure, which is mainly composed of mesopores, and has a small amount of micropores and macropores. The pore size distribution of the present invention has a significant improvement in the adsorption performance of nitrogen and phosphorus.

[0024] As a preferred solution, the particle size of the red mud-based biogas residue composite material is in the millimeter range, more preferably 6 to 7 mm. The composite material obtained by the preparation method of the present invention has a relatively large particle size and is easy to separate from water and recycle.

[0025] Finally, the present invention also provides an application of a red mud-based-biogas residue composite material, which is used as an adsorption material for the adsorption of nitrogen and / or phosphorus, and has the advantages of large adsorption capacity and high adsorption efficiency.

[0026] The adsorption principle of the composite material of the present invention for nitrogen and / or phosphorus is:

[0027] First, the oxygen-containing functional groups in red mud have an impact on the electron-donor-acceptor interaction, and the increase of carbonyl groups on biochar from digestate improves the adsorption of compounds with electron-donating groups. The increase in the content of iron (Fe), aluminum (Al), calcium (Ca) and silicon (Si) on the surface of the composite material after pyrolysis provides more active sites for the adsorption of nitrogen and phosphorus. At the same time, the decomposition of organic matter in digestate and the recrystallization of red mud minerals promote the formation of carboxyl (-COOH) and phenolic hydroxyl (Ar-OH), enhancing the adsorption of nitrogen and phosphorus.

[0028] The Fe in the red mud can form a Fe-OP ternary complex through adsorption and coprecipitation, which is beneficial to the removal of phosphate. In addition, the metal oxides in the hematite in the red mud are transformed from an oxidized state (Fe2O3) to a reduced state (FeO, Fe3O4) through phase change, which enhances the electrostatic attraction of the material to phosphates and the like. After pyrolysis, a large number of metal hydroxyls and metal active sites can undergo ligand exchange with phosphates in the solution to generate substances such as R-H2PO4 and Fe-OP ternary complexes. After the complex is formed by adsorption and coprecipitation, the composite material of the present invention can also hydrolyze the iron ions and ferrous ions released by oxygen absorption corrosion into ferric hydroxide colloids, thereby promoting the flocculation of the complex on the composite material.

[0029] Fe 3+ +3H2O→Fe(OH)3+3H +

[0030] Fe(OH)3→Fe x O y +H2O

[0031] Fe x O y +C / CO→Fe 0 +CO2

[0032] Fe 0 +H2O+O2→Fe(OH)3

[0033] Fe 3+ +PO4 3- →FePO4

[0034] C m H n -COOH+NH4 + →C m H n -COONH4+H +

[0035] Formula I.

[0036] As a preferred scheme, the adsorption conditions are: pH 7-8, time 3-24 hours, and the addition amount of nitrogen and / or phosphorus to the red mud-based-biogas residue composite material is 10-50 g / L.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] 1) The composite material of the present invention uses organic solid waste as raw materials, crushes and mixes them into granules to prepare a shaped composite adsorption material, which solves the problems of difficult recycling and secondary utilization of traditional powder adsorbents, and is applied to the field of sewage treatment. The process is simple, low-cost, and easy to mass produce. At the same time, it can also alleviate the problem of a large amount of solid waste having nowhere to go and realize resource utilization.

[0039] 2) The composite material of the present invention utilizes inorganic minerals in red mud to form a mineral coating and bonding layer in the porous structure on the surface and inside of the sludge biochar. At the same time, the metal oxides in the red mud undergo a phase change during the pyrolysis process to generate a new mineral phase (magnetite) with high adsorption activity that also coats and penetrates the sludge biochar. On the one hand, the particle size of the red mud-based-sludge composite material is increased, making it easy to separate from water and recycle. On the other hand, the two work together to significantly improve the adsorption of nitrogen and phosphorus by the red mud-based-sludge composite material.

[0040] 3) When the composite material of the present invention is used as an adsorbent, effective adsorption of nitrogen and phosphorus is achieved through the combined effects of physical adsorption, chemical adsorption, pore filling, electrostatic attraction, ion exchange and coordination complexation, and the composite material containing nitrogen and phosphorus after adsorption can be applied to the soil as a fertilizer to supply nutrition to crops, thereby realizing the resource utilization of nitrogen and phosphorus. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is the SEM photo of the red mud / sludge biochar composite adsorption material prepared in Example 1.

[0042] Figure 2 These are the BET test results of the red mud / sludge biochar composite adsorption material prepared in Example 1.

[0043] Figure 3 This is the kinetic model of ammonia nitrogen adsorption by the red mud / sludge biochar composite adsorption material prepared in Example 1. DETAILED DESCRIPTION

[0044] In order to make the purpose, technical solution and advantages of the present invention more clear, the technical solution of the present invention is clearly and completely described in combination with specific embodiments below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0045] The components and contents of the biogas residue used in the examples and comparative examples of the present invention are shown in Table 1:

[0046] Table 1

[0047] element C H O S Content (wt%) 58.13 10.22 30.32 1.33

[0048] The red mud used in the embodiments of the present invention and the comparative examples has a Fe2O3 content of 44.7wt.%, an Al2O3 content of 22.6wt.%, a CaO content of 0.87wt.%, a SiO2 content of 15.35wt.%, and the remainder being impurities.

[0049] Example 1

[0050] A method for preparing a red mud-based biogas residue biochar composite nitrogen and phosphorus adsorption material is achieved by the following steps:

[0051] (1) The obtained red mud is dried and crushed in a crusher, taken out and ground through a 100-mesh sieve to obtain red mud powder (raw material 1); the obtained biogas residue is dried to constant weight, crushed in a crusher, taken out and ground through a 100-mesh sieve to obtain biogas residue powder (raw material 2).

[0052] (2) Mix the raw material 1 and raw material 2 obtained in step (1) in a mass ratio of 3:1, add deionized water, place in a blender and stir for 30 minutes until it becomes viscous, take out and put into a mold to shape, and air-dry after shaping until it can be demolded and taken out.

[0053] (3) The air-dried composite material obtained in step (2) was placed in a 105°C oven for drying for 2 hours, taken out and placed in a closed calcining furnace, and in an oxygen-free condition, the temperature was increased at a rate of 10°C / min, the nitrogen flow rate was 0.5L / min, the calcination temperature was 600°C, the heat preservation time was 2 hours, and the composite material was obtained after cooling. The average particle size of the composite material prepared in this embodiment was 7mm.

[0054] Figure 1 This is a SEM photo of the red mud / biogas residue biochar composite material prepared in this example. Figure 1 It can be seen that the material skeleton and hierarchical structure are obvious, which is due to the partial phase transformation inside the material during the pyrolysis process. On the other hand, it may be because the increase in temperature can promote the gasification reaction of carbon and the aggregation of metallic iron, making the material structure more stable and not easy to dissolve in water.

[0055] Figure 2 The BET test results of the red mud / biogas residue biochar composite material prepared in this example show that the pore size distribution of the material is concentrated in the range of 2 to 32 nm, indicating that the pore size distribution of the material is mainly mesopores, with a small amount of micropores and macropores. The specific surface area of ​​the material after pyrolysis is 28.9365 m 2 / g, the average pore size is 14.9315nm. The specific surface area before pyrolysis is 15.2677m 2 / g average pore size is 12.7495nm, and the specific surface area of ​​the material after pyrolysis increases significantly. With the increase of pyrolysis temperature, the unstable water molecules of red mud in the material are released, and some phases are decomposed to form pores, which not only expands the specific surface area of ​​the material and makes the pore structure of red mud richer, but also provides more active sites. At the same time, the increase in temperature also increases the total pore volume and average pore size of the material, which can make the material better play its interception role and improve the material's adsorption capacity for nitrogen and phosphorus.

[0056] Example 2

[0057] The composite material was prepared according to the method of Example 1, except that the raw material ratio of raw material 1: raw material 2 in step (2) was changed to 2.5:1, 2:1, and 1:1, respectively, to obtain the composite material, and the effect of the mass ratio of red mud to biogas residue on the nitrogen and phosphorus adsorption performance of the composite material was investigated. At the same time, the composite material under each mass ratio was investigated at calcination temperatures of 300°C, 400°C, 500°C, 600°C, 700°C, and 800°C, respectively.

[0058] When the mass ratio is 1:1, the composite material cannot be formed due to the small amount of red mud used.

[0059] Comparative Example 1

[0060] The only difference between this comparative example and Example 1 is that no red mud is added, and the other conditions and steps are the same to obtain a biochar material.

[0061] Comparative Example 2

[0062] A composite material was prepared according to the method of Example 1, except that no biogas slag was added, and the effects of red mud materials calcined at 300°C, 400°C, 500°C, 600°C, 700°C and 800°C on the nitrogen and phosphorus adsorption properties of the composite material were investigated.

[0063] Application example 1: Application of composite materials to the adsorption of ammonia nitrogen in simulated biogas slurry

[0064] The ammonia nitrogen adsorption capacity of the composite material was investigated by preparing 100 mg / L ammonium chloride solution as a simulated ammonia nitrogen solution. 40 mL of ammonium chloride solution was added to a 50 mL centrifuge tube, and the pH was adjusted to 7 with sodium hydroxide and hydrochloric acid solution. After adding 0.4 g of the composite material prepared in Example 1, it was shaken at 100 r / min for 24 h in a constant temperature shaking incubator at room temperature. The sample was filtered through a 0.45 μm filter membrane to determine the ammonia nitrogen concentration at adsorption equilibrium. Figure 3 It can be seen that after 180 minutes, the adsorption of ammonia nitrogen by the material basically reached equilibrium, and the equilibrium adsorption amount was 0.78 mg / g. Pseudo-second-order kinetic fitting correlation coefficient R 2 =0.98, indicating that the adsorption of ammonia nitrogen by the material is the result of the combined action of physical adsorption and chemical adsorption.

[0065] The composite materials prepared under various conditions in Example 2 and the biochar materials prepared in Comparative Example 1 were subjected to adsorption experiments on ammonium chloride and phosphorus (using 40 mL of 50 mg / L potassium dihydrogen phosphate) under the same adsorption conditions as in Example 1. The adsorption results are shown in Table 2.

[0066] Table 2 Adsorption rate of composite materials with different ratios at 600℃

[0067] Raw material quality ratio nitrogen phosphorus Red mud and biogas residue are mixed at a ratio of 3:1 47.79% 86.32% Red mud and biogas residue are mixed at a ratio of 2.5:1 46.45% 81.78% Red mud and biogas residue are mixed at a ratio of 2:1 47.24% 83.85% No red mud added Unable to form Unable to form

[0068] Comparative Example 2 The composite materials prepared under various conditions in Example 1 were subjected to adsorption experiments on ammonium chloride and phosphorus (using 40 mL of 50 mg / L potassium dihydrogen phosphate). The adsorption results are shown in Table 3.

[0069] Table 3 Adsorption rate of nitrogen and phosphorus by red mud at different temperatures

[0070] Temperature / ℃ nitrogen phosphorus 300 0.09% 0.8% 400 0.10% 1% 500 0.12% 1% 600 0.11% 0.5% 700 0.15% 0.8% 800 0.13% 0.6%

[0071] It can be seen from Table 3 that when no sludge is added, the adsorption rate of nitrogen and phosphorus by red mud is relatively low at different temperatures. This is because the adsorption effect of red mud itself is weak. It mainly serves as a supporting skeleton in the composite material. At the same time, the synergistic effect produced by the co-pyrolysis of sludge improves the adsorption capacity of the composite material.

[0072] In order to clarify the stability of the composite material in water, the composite materials prepared at different temperatures and proportions were quantitatively weighed, the mass was recorded as m1, placed in a sample bottle, 40 ml of deionized water was added, and the mixture was statically adsorbed at room temperature for 6 hours. The mixture was taken out and placed in an oven at 105°C to dry to constant weight. The mass was weighed and recorded as m2. The mass loss rate was calculated according to the formula.

[0073]

[0074] Table 4 Mass loss rate of materials at different temperatures and red mud proportions (%)

[0075]

[0076]

[0077] It can be seen from Table 4 that when the calcination temperature increases, it is beneficial to increase the stability of the composite material in water.

[0078] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a red mud-based biogas residue biochar composite nitrogen and phosphorus adsorption material, characterized in that: The red mud and biogas residue are compounded and mixed, and shaped into composite materials of different shapes according to the needs of the adsorption product, and then pyrolyzed at 300-900°C to obtain the composite material.

2. The method for preparing a red mud-based biogas residue biochar composite nitrogen and phosphorus adsorption material according to claim 1, characterized in that: The mass ratio of the red mud to the biogas residue is (2-3):

1.

3. The method for preparing a red mud-based biogas residue biochar composite nitrogen and phosphorus adsorption material according to claim 2, characterized in that: The red mud and biogas residue are compounded and mixed, and then pyrolyzed for 1 to 3 hours to carbonize the organic part thereof to form an adsorption material with abundant pores.

4. A red mud-based biogas residue biochar composite nitrogen and phosphorus adsorption material, characterized in that: The method is obtained by the preparation method according to any one of claims 1 to 3.

5. The red mud-based biogas residue biochar composite nitrogen and phosphorus adsorption material according to claim 4, characterized in that: It can be prepared into different shapes, including spherical, plate and honeycomb shapes, according to the usage scenarios and the conditions of nitrogen and phosphorus pollutants.

6. The use of a red mud-based biogas residue biochar composite nitrogen and phosphorus adsorption material according to claim 5, characterized in that: Used for adsorption and recovery of nitrogen and phosphorus in sewage.