Cu0 / Cu < + > nano composite material as well as preparation method and application thereof

By wrapping the carbon layer on the surface of copper metal and cuprous oxide composite materials and dispersing nitrogen elements, controlling the ratio of monovalent copper to zero-valent copper, the iodine adsorption capacity of Cu0/Cu+ nanocomposites is improved, and the iodine adsorption in the existing technology is solved The problem of poor results has achieved the effect of efficiently removing iodine ions.

CN119056422APending Publication Date: 2024-12-03NANJING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411298676.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing adsorption materials have poor adsorption effect on iodine and cannot effectively solve the pollution problem of iodine ions in radioactive medical wastewater, resulting in environmental pollution and health risks.

Method used

Cu0/Cu+ nanocomposite material is used to wrap the carbon layer on the surface of the copper metal and cuprous oxide composite and disperse nitrogen elements uniformly, and the ratio of monovalent copper to zero-valent copper is controlled to be 0.45-0.8, and the adsorption capacity is improved through calcination treatment.

Benefits of technology

The adsorption ability of nanocomposites to iodine is significantly improved, structural defects and graphitization are enhanced, the contact between iodine and active sites is promoted, and the removal of iodine ions is achieved efficiently, and the thermal stability and irradiation stability are good.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056422A_ABST
    Figure CN119056422A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of iodine adsorbents, and discloses a Cu0 / Cu + nano composite material and a preparation method and application thereof, the composite material is a copper metal and cuprous oxide composite material, the surface of the composite material is provided with a carbon layer, and nitrogen elements are uniformly dispersed in the carbon layer and the composite material. The nano composite material obtained by the invention has good iodine adsorption capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of iodine adsorbents, and in particular to a Cu 0 / Cu + Nanocomposite materials and their preparation methods and applications. Background Art

[0002] radioactivity 131 I is commonly used in the field of nuclear medicine. 131 I has a half-life of 8.04 days and can release beta rays during decay, which is often used in the diagnosis and treatment of hyperthyroidism and thyroid cancer. 131 I has been used as the first choice for the treatment of hyperthyroidism. 131 I has strong radioactivity and is rich in 131 Medical wastewater containing radioactive iodine (I) will pollute the water and environment when it enters the environment. It may also cause thyroid cancer after being absorbed by the human body through the food chain. Therefore, medical wastewater generated by nuclear medicine departments needs to be effectively treated before being discharged into surface water. Conventional storage decay methods have long been unable to meet the growing scale of medical wastewater. Therefore, it is necessary to efficiently and cost-effectively remove radioactive iodine (I) from the water environment. - ) is of great significance to the sustainable development of nuclear medicine and human health.

[0003] In the prior art, methods such as adsorption, ion exchange, chemical precipitation and catalytic oxidation are often used to remove iodide ions. At present, the adsorption method is widely used in radioactive iodine adsorption research due to its economic effectiveness and environmental friendliness. Various porous adsorbents such as metal organic frameworks, covalent organic frameworks, carbon materials and aerogels have been developed to capture iodine ions. However, the current adsorption materials have poor adsorption effects on iodine. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a Cu 0 / Cu + A nano composite material and a preparation method and application thereof. The nano composite material obtained by the invention has good iodine adsorption capacity.

[0005] The present invention provides a Cu 0 / Cu + The nano composite material is a copper metal and cuprous oxide composite material. A carbon layer is provided on the surface of the composite material, and nitrogen elements are uniformly dispersed in the carbon layer and the composite material.

[0006] Furthermore, the ratio of monovalent copper to zero-valent copper in the copper metal and cuprous oxide composite material is 0.45-0.8.

[0007] Furthermore, the ratio of monovalent copper to zero-valent copper in the copper metal and cuprous oxide composite material is 0.6-0.68.

[0008] The present invention also provides the Cu 0 / Cu + A method for preparing a nanocomposite material, the method comprising: The copper metal frame is placed in an inert atmosphere for calcination to obtain a nanocomposite material. The calcination temperature is 300°C-500°C, the calcination time is 1.5h-2.5h, and the heating rate to reach the calcination temperature is 1.5°C / min-2.5°C / min.

[0009] Furthermore, the inert atmosphere includes one of nitrogen, argon, helium, and argon.

[0010] Furthermore, the preparation method of the copper metal frame includes: dissolving a copper source and polyvinyl pyrrolidone in a solvent to obtain a solution A; dissolving 1,3,5-benzenetricarboxylic acid (H3-BTC) in a solvent to obtain a solution B; mixing solution A and solution B, performing a hydrothermal reaction after mixing, cooling, washing, and drying to obtain a copper metal frame.

[0011] Furthermore, the copper source includes one or more of copper nitrate trihydrate, copper nitrate nonahydrate, and copper nitrate.

[0012] Furthermore, based on the mass of copper in the copper source, the mass ratio of the copper source to polyvinyl pyrrolidone is 0.41:0.665.

[0013] In the present invention, the mass ratio between the divalent copper in the copper source and polyvinyl pyrrolidone is determined to be 0.41:0.665, so that the added masses of the copper source and polyvinyl pyrrolidone can be further converted.

[0014] Furthermore, the solvent consists of N,N-dimethylformamide and anhydrous ethanol, and the volume ratio of N,N-dimethylformamide to anhydrous ethanol is 1:1.

[0015] Furthermore, the mass concentration of the polyvinyl pyrrolidone in the solvent is 0.665 g / 30 mL.

[0016] Furthermore, those skilled in the art should understand that in order to make solution A uniform, after the copper source and polyvinyl pyrrolidone are dissolved in the solvent, stirring is performed. As an example, stirring is performed at room temperature for 20 minutes.

[0017] Furthermore, the mass concentration of the 1,3,5-benzenetricarboxylic acid in the solvent is 0.735 g / 30 mL.

[0018] Furthermore, by volume, the ratio of solution A to solution B is 1:1.

[0019] Furthermore, those skilled in the art should understand that in order to make solution A and solution B uniform, solution A and solution B can be stirred after being mixed. As an example, stirring is performed at room temperature for 30 minutes.

[0020] Furthermore, the temperature of the hydrothermal reaction is 110° C.-130° C., and the time of the hydrothermal reaction is 3.5 h-4.5 h.

[0021] Furthermore, the cooling to room temperature is 26°C-28°C.

[0022] Furthermore, the specific method of washing includes: washing with N,N-dimethylformamide and anhydrous ethanol in sequence for 3-5 times.

[0023] Furthermore, the drying temperature is 50°C-70°C, and the drying time is 11h-13h.

[0024] The present invention also provides the Cu 0 / Cu + Application of nanocomposites in iodine adsorption.

[0025] The embodiments of the present invention have the following technical effects: 1. In the adsorbent obtained by the present invention, firstly, the monovalent copper in the copper metal and cuprous oxide composite material can improve the adsorption capacity of the nanocomposite material, and the carbon layer outside the copper metal and cuprous oxide composite material can improve the structural defects and graphitization degree of the nanocomposite material, thereby facilitating the contact between iodine and active sites, and further improving the adsorption capacity of the nanocomposite material. In addition, the nitrogen element uniformly dispersed in the adsorbent can improve the adsorption capacity of the carbon layer for iodine, thereby promoting the contact between iodine and active sites in the carbon layer.

[0026] 2. In the present invention, the monovalent copper in the composite material can improve the adsorption capacity of the adsorbent for iodine, and copper has a strong adsorption capacity for monovalent copper, which can prevent the conversion of monovalent copper into divalent copper, thereby reducing the adsorption capacity of the adsorbent for iodine. Therefore, in order to improve the adsorption capacity of the nanomaterial for iodine, the ratio of monovalent copper to zero-valent copper in the nanocomposite material is designed to be 0.45-0.8. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1 is a microscopic diagram of the preparation method and product provided by the embodiment of the present invention, wherein Figure 1 a is the preparation process. Figure 1 Figure b is a microscopic picture of Example 1. Figure 1 Figure c is a microscopic image of Example 1. Figure 1 Figure d is a microscopic image of Example 1. Figure 1 Figure e is a microscopic image of Example 1. Figure 1 b1 is Figure 1 The enlarged image of b, Figure 1 Where c1 is Figure 1 The enlarged image of c in the middle, Figure 1 In d1 is Figure 1 The enlarged image of middle d, Figure 1 e1 is Figure 1 Enlarged view of middle e.

[0029] Figure 2 is a product test diagram of an embodiment of the present invention, wherein Figure 2 a is a microscopic image of Example 1, Figure 2 Where b is the element distribution of Example 1, Figure 2 Figure c is a microscopic image of Example 2. Figure 2 Where d is the element distribution of Example 2, Figure 2 Figure e is a microscopic image of Example 3. Figure 2 Where f is the element distribution of Example 3.

[0030] Figure 3 are the TEM characterization and HRTEM characterization results of Example 2, wherein Figure 3 Figure a is a microscopic image of Example 2. Figure 3 b is a microscopic image of Example 2, Figure 3 Figure c is a microscopic image of Example 2. Figure 3 a1 is the distribution diagram of N element in Example 2, Figure 3 a2 is the distribution diagram of Cu element in Example 2, Figure 3 a3 is the distribution diagram of the O element in Example 2, Figure 3 a4 is the distribution diagram of N element in Example 2, Figure 3 Figure d is the TEM characterization image of Example 2. Figure 3 Figure e is the TEM characterization image of Example 2, Figure 3(f) is the HRTEM image of Example 2.

[0031] Figure 4 is the test result of the embodiment and the comparative example, wherein Figure 4 a is the XRD pattern, Figure 4 b is the FTIR spectrum, Figure 4 The c in the middle is the Raman spectrum. Figure 4 The figure d in the middle is the full spectrum scanning result. Figure 4 e in the figure is the high-resolution XPS spectrum of Cu 2p. Figure 4 f is the Cu LMM Auger spectrum, Figure 4 g is the high-resolution XPS spectrum of C 1s. Figure 4 h in the figure is the high-resolution XPS spectrum of N 1s. Figure 4 Where i is the high-resolution XPS spectrum of O 1s.

[0032] Figure 5 This is the TGA curve of thermal stability analysis of Example 1.

[0033] Figure 6 is the N2 adsorption-desorption isotherm of the embodiment and the comparative example, wherein Figure 6 a is the relationship between relative pressure and adsorption amount. Figure 6 b is the relationship between pore size and adsorption amount.

[0034] Figure 7 Cu in the adsorbent of the embodiment + , Cu 0 and total copper content.

[0035] Figure 8 are the test results of the embodiments under different conditions, wherein Figure 8 a is the relationship between iodine ion concentration and adsorption amount. Figure 8 b is the change of adsorption amount with adsorption time. Figure 8 Where c is the relationship between temperature change and adsorption amount. Figure 8 Where d is the adsorption capacity of Example 2 at different pH values, Figure 8 Where e is the effect of anions on the adsorption capacity of Example 2, Figure 8 Where f is the removal rate of trace iodine at different initial concentrations in Example 2, Figure 8 g is below the limit after adsorption of iodine ions in Example 2. Figure 8 h in I - The adsorption capacity of Cu / Cu2O@NC-400 for iodine changes with contact time when the initial concentration is 0.3 mg / L. Figure 8 Where i is the iodine removal capacity before and after irradiation in the embodiment, Figure 8 In J, ultrasonic and immersion treatments were used to test the storage capacity of iodine in Example 2.

[0036] Fig. 9 This is the relationship between the initial iodine ion concentration and the adsorption amount in Comparative Example 1.

[0037] Fig.10 It is to clarify - Combination with Cu2O, Fig.10 In the figure a is a top view. Fig.10 Middle b is a side view.

[0038] Fig.11 is the adsorption configuration diagram, where Fig.11 a in the middle is the top view of the adsorption configuration of the Cu2O(111) crystal surface. Fig.11 Figure b is a top-down adsorption configuration diagram of the Cu2O (110) crystal surface. Fig.11 The c in the figure is the top view of the adsorption configuration of the Cu(111) crystal surface. Fig.11 Figure d in the figure is the side-view adsorption configuration of the Cu2O(111) crystal plane. Fig.11 e is the side-view adsorption configuration diagram of the Cu2O(110) crystal plane. Fig.11 Figure f is the side-view adsorption configuration of the Cu(111) crystal plane.

[0039] Fig.12 is the test result of Example 2, wherein Fig.12 a is the pH value after adsorption at different pH values. Fig.12 b in the figure is the Zeta potential at different pH values.

[0040] Fig.13 This is a microscopic image of Example 2 after iodine adsorption, wherein Fig.13 a in the middle is the octahedral morphology of the adsorbent after enrichment of iodine. Fig.13 Figure b is a microscopic picture of the adsorbent after enriching iodine. Fig.13 The image c in the middle is the lattice fringe diagram of the adsorbent after enriching iodine. Fig.13 b1 is the C element distribution diagram, Fig.13 b2 is the Cu element distribution diagram. Fig.13 b3 is the distribution diagram of I element. Fig.13 b4 is the distribution diagram of O element. Fig.13 b5 is the N element distribution diagram.

[0041] Fig.14 is the element distribution diagram after iodine adsorption in Example 2, wherein Fig.14 Figure a is a TEM image of Cu. Fig.14 Figure b is the EDS spectrum.

[0042] Fig.15 This is a comparison of Example 2 before and after iodine adsorption, where Fig.15 a is the XRD pattern, Fig.15 b is the XPS graph. Fig.15 c is the XPS spectrum of I 3d of Example 2 after adsorption, Fig.15 (d) is the high-resolution spectrum of Cu before and after adsorption.

[0043] Fig.16 It is a diagram of the mechanism of iodine adsorption in the example.

[0044] Fig.17 : is the XPS spectrum of O 1s before and after adsorption in the example. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0046] In a first aspect, some embodiments of the present invention provide a Cu 0 / Cu + The nano composite material is a copper metal and cuprous oxide composite material. A carbon layer is provided on the surface of the composite material, and nitrogen elements are uniformly dispersed in the carbon layer and the composite material.

[0047] In the nanocomposite material obtained by the present invention, the copper metal and cuprous oxide composite material is conducive to improving the adsorption capacity of iodine, the carbon layer increases the area and active sites for adsorbing iodine, and the nitrogen element uniformly dispersed in the adsorbent can improve the adsorption capacity of the carbon layer for iodine, thereby promoting the contact between iodine and the active sites in the carbon layer.

[0048] In some embodiments, the ratio of monovalent copper to zero-valent copper in the copper metal and cuprous oxide composite material is 0.45-0.8.

[0049] When the ratio is higher, although the increase of monovalent copper is beneficial to improve the affinity of the adsorbent to iodine, it will cause less zero-valent copper, which will cause the adsorption capacity between monovalent copper to decrease, which is not conducive to the full reaction of zero-valent copper and divalent copper. Divalent copper will be generated in the adsorbent, resulting in a decrease in the active sites between iodine and the adsorbent, and the adsorption capacity of the adsorbent to iodine will decrease; and when the ratio is lower, although too much zero-valent copper can reduce the generation of divalent copper through the adsorption capacity of monovalent copper, it will also cause less monovalent copper content, poor synergy between zero-valent copper and monovalent copper, and the adsorbent's affinity for iodine will decrease. Therefore, in the present invention, it is determined that the ratio of monovalent copper to zero-valent copper in the nanocomposite material is 0.45-0.8, which is conducive to further improving the adsorption capacity of the nanocomposite material.

[0050] In a second aspect, some embodiments of the present invention further provide the Cu 0 / Cu + A method for preparing a nanocomposite material, the method comprising: The copper metal frame is placed in an inert atmosphere for calcination to obtain a nanocomposite material. The calcination temperature is 300°C-500°C, the calcination time is 1.5h-2.5h, and the heating rate to reach the calcination temperature is 1.5°C / min-2.5°C / min.

[0051] In the method of the present invention, the ratio of monovalent copper to zero-valent copper in the nanocomposite material is controlled by controlling the calcination temperature and time; in addition, the setting of the calcination temperature can also enrich the pore size distribution of the nanocomposite material, thereby increasing the specific surface area and pore structure of the nanocomposite material, which is beneficial to increasing the contact area for iodine adsorption; in the present invention, the morphology collapse of the metal organic framework can be avoided by controlling the calcination heating rate, thereby ensuring the structure of the adsorbent.

[0052] In some embodiments, the inert atmosphere includes one of nitrogen, argon, helium, and argon.

[0053] In some embodiments, the preparation method of the copper metal frame includes: dissolving a copper source and polyvinyl pyrrolidone in a solvent to obtain a solution A; dissolving 1,3,5-benzenetricarboxylic acid in a solvent to obtain a solution B; mixing solution A and solution B, performing a hydrothermal reaction after mixing, cooling, washing, and drying to obtain a copper metal frame.

[0054] In some embodiments, the copper source includes one or more of copper nitrate trihydrate, copper nitrate nonahydrate, and copper nitrate.

[0055] Furthermore, based on the mass of copper in the copper source, the mass ratio of the copper source to polyvinyl pyrrolidone is 0.41:0.665.

[0056] In some embodiments, the solvent consists of N,N-dimethylformamide and anhydrous ethanol, and the volume ratio of N,N-dimethylformamide to anhydrous ethanol is 1:1.

[0057] In some embodiments, the mass concentration of polyvinyl pyrrolidone in the solvent is 0.665 g / 30 mL.

[0058] In some embodiments, the mass concentration of 1,3,5-benzenetricarboxylic acid in the solvent is 0.735 g / 30 mL.

[0059] In some embodiments, the ratio of solution A to solution B is 1:1 by volume.

[0060] In some embodiments, the temperature of the hydrothermal reaction is 110° C.-130° C., and the time of the hydrothermal reaction is 3.5 h-4.5 h.

[0061] In some embodiments, the cooling to room temperature is 26°C-28°C.

[0062] In some embodiments, the specific method of washing includes: washing with N,N-dimethylformamide and anhydrous ethanol in sequence for 3-5 times.

[0063] In some embodiments, the drying temperature is 50° C.-70° C., and the drying time is 11 h-13 h.

[0064] In a third aspect, some embodiments of the present invention further provide the Cu 0 / Cu + Application of nanocomposites in iodine adsorption.

[0065] The following is further described in conjunction with some specific embodiments: Embodiment 1: 1.55 g of copper nitrate trihydrate and 0.665 g of polyvinylpyrrolidone (PVP) were weighed and dissolved in 30 mL of a mixed solution of N,N-dimethylformamide (DMF) and anhydrous ethanol (wherein the volume ratio of N,N-dimethylformamide to ethanol was 1:1). The solution was stirred at room temperature for 20 min and recorded as solution A. 0.735 g of 1,3,5-benzenetricarboxylic acid was dissolved in another 30 mL of a mixed solution of N,N-dimethylformamide and anhydrous ethanol (wherein the volume ratio of N,N-dimethylformamide to ethanol was 1:1), which was recorded as solution B. Solution A and solution B were combined and stirred for 30 min and recorded as solution C, where the volume ratio of solution A to solution B was 1:1. Next, solution C was transferred to a 100 mL polytetrafluoroethylene-lined autoclave for a hydrothermal reaction at 120°C for 4 hours. After cooling to room temperature, centrifugation was performed, and the mixture was washed with DMF and anhydrous ethanol for 3-5 times. After drying in a vacuum oven at 60°C for 12 hours, a light blue powder was obtained, which was recorded as Cu-BTC. 0.2 g of the prepared Cu-BTC was placed in the center of a tube furnace. The temperature was raised to 300 °C at a rate of 2 °C / min under a nitrogen atmosphere. The mixture was calcined at this temperature for 2 h, and then naturally cooled to room temperature (28 °C) and a reddish-brown powder was collected, which was recorded as Cu / Cu2O@NC-300.

[0066] Embodiment 2: The preparation method of Example 2 is the same as that of Example 1, but in Example 2, 0.2 g of the prepared Cu-BTC is placed in the center of a tube furnace. The temperature is raised to 400°C at a heating rate of 2°C / min under a nitrogen atmosphere. The mixture is calcined at this temperature for 2 h, and then naturally cooled to room temperature (28°C) and a reddish-brown powder is collected, which is recorded as Cu / Cu2O@NC-400.

[0067] Embodiment 3: The preparation method of Example 3 is the same as that of Example 1, but in Example 3, 0.2 g of the prepared Cu-BTC is placed in the center of a tube furnace. The temperature is raised to 500°C at a heating rate of 2°C / min under a nitrogen atmosphere. The mixture is calcined at this temperature for 2 h, and then naturally cooled to room temperature (28°C) and a reddish-brown powder is collected, which is recorded as Cu / Cu2O@NC-500.

[0068] Comparative Example 1: 1.55 g of copper nitrate trihydrate and 0.665 g of polyvinylpyrrolidone (PVP) were weighed and dissolved in 30 mL of a mixed solution of N,N-dimethylformamide (DMF) and anhydrous ethanol (wherein the volume ratio of N,N-dimethylformamide to ethanol was 1:1). The solution was stirred at room temperature for 20 min and recorded as solution A. 0.735 g of 1,3,5-benzenetricarboxylic acid was dissolved in another 30 mL of a mixed solution of N,N-dimethylformamide and anhydrous ethanol (wherein the volume ratio of N,N-dimethylformamide to ethanol was 1:1), which was recorded as solution B. Solution A and solution B were combined and stirred for 30 min and recorded as solution C, where the volume ratio of solution A to solution B was 1:1. Next, solution C was transferred to a 100 mL polytetrafluoroethylene-lined autoclave for a hydrothermal reaction at 120°C for 4 hours. After cooling to room temperature, the mixture was centrifuged, washed with DMF and anhydrous ethanol for 3-5 times, and dried in a vacuum oven at 60° C. for 12 hours to obtain a light blue powder, which was recorded as Cu-BTC.

[0069] The obtained embodiments and comparative examples were tested: (1) Adsorption test: In order to evaluate the nano-adsorbent material obtained in the present invention, - The adsorption performance of iodine was investigated by adsorption kinetics, adsorption isotherms, adsorption thermodynamics, pH and competitive anions, trace iodine adsorption, adsorption stability and irradiation stability experiments. Since iodine isotopes have similar chemical properties, a safe 127 I(KI) replaces highly toxic and radioactive 131 I performed batch adsorption experiments.

[0070] (2) DFT The density functional theory (DFT) was used to study the relationship between the nano-adsorbent material and I -The interaction between Cu2O (111) and Cu (111) was investigated by constructing and optimizing the models to study the adsorption energy of iodine on different sites of Cu2O and Cu. The adsorption energy (Eads) was calculated according to the formula:

[0071] Where Eads is the adsorption energy, E adsorbent+I represents the total energy of iodine adsorbed on the adsorbent surface, E adsorbent is the energy of the pure adsorbent surface, E I represents the energy of the adsorbate.

[0072] (3) Characterization The morphology and elemental composition were analyzed using a field emission scanning electron microscope (SEM, S-4800, HITACHI) equipped with an energy dispersive X-ray spectrometer (EDS). X-ray diffraction (XRD) patterns were recorded from 10° to 70° on a Bruker-AXS (D8-Advance) diffractometer using Cu Kα radiation at 40 kV and 30 mA. Fourier transform infrared spectra were collected by a Fourier transform infrared spectrometer (FTIR, iS5, Nicolet). Raman spectra were recorded by a Nicolet Almega dispersive Raman spectrometer. The binding energies of the elements before and after iodine capture were determined using an X-ray photoelectron spectrometer (XPS, Qantera II, PHI). The specific surface area and porosity were measured by a nitrogen adsorption and desorption analyzer (BELSORP-MAX) using the Barrett-Emmett-Teller (BET) and Barrett-Joyner-Hallendar (BJH) calculation methods, respectively. Thermogravimetric analysis (TGA, SDTA851E, Mettler-Toledo) was used to characterize the thermal stability. The copper content in the solution was detected using an inductively coupled plasma mass spectrometer (ICP-MS, Agilent 7800). The concentration of trace iodide ions in the solution was determined by ion chromatography (IC, Metrohm 940).

[0073] Results and analysis: Table 1 Physical properties of examples and comparative examples

[0074] Table 2 Elemental composition of the examples analyzed by XPS

[0075] Table 3 Fitting parameters of Langmuir model and Freundlich model adsorption isotherms

[0076] Table 4 Fitting parameters of the kinetic model

[0077] Table 5 Langmuir model and Freundlich model fitting parameters of Example 2

[0078] Table 6 Thermodynamic parameters of Example 2

[0079] Table 7 Comparison of Example 2 with the prior art

[0080] The adsorbent is prepared by the method of the present invention, such as Figure 1 As shown in (a), a copper metal and cuprous oxide composite material is obtained, a carbon layer is wrapped on the surface of the composite material, and nitrogen elements are evenly dispersed in the carbon layer and the composite material. The copper metal and cuprous oxide composite material is conducive to improving the adsorption capacity of iodine, the carbon layer increases the area and active sites for adsorbing iodine, and the nitrogen elements evenly dispersed in the adsorbent can improve the adsorption capacity of the carbon layer for iodine, thereby promoting the contact of iodine with the active sites in the carbon layer. It can be seen that the adsorbent obtained by the present invention has a good adsorption capacity for iodine.

[0081] The microstructure and changes of Cu-BTC materials and calcined nanocomposites were observed by SEM. Figure 1 (b) and Figure 1 (b1) shows that Cu-BTC has a smooth and uniform octahedral structure, and the average particle size is about 700nm. In the process of preparing Cu-BTC materials, the particle size can be effectively adjusted by PVP. Taking Example 1 as an example, the Cu-BTC material of Example 1 is calcined at 300℃. Figure 1 (c)- Figure 1 (e) and Figure 1 (c1)- Figure 1 As shown in (e1), the overall morphology of the Cu-BTC material is still octahedral, but the surface structure of the particles becomes rough and the particle size is reduced to about 450nm. Figure 2 It can be found that the size of Cu / Cu2O@NC-400 and Cu / Cu2O@NC-500 is further reduced and becomes rough and porous. It is speculated that this may be due to the fact that the calcination temperature is too high, resulting in partial collapse on the basis of retaining the carbon skeleton; the results of EDS characterization of the elemental composition of the nanocomposites obtained in Example 1 to Example 3 show that the nanocomposites obtained in the present invention are composed of C element, Cu element, O element and N element.

[0082] In order to further reveal the structure of the prepared material and the formation of nano Cu / Cu2O, taking Example 2 as an example, TEM and HRTEM characterization of Cu / Cu2O@NC-400 were performed. Figure 3 (a)- Figure 3 As shown in (c), the carbonized sample retains the original octahedral structure and a clear core-shell structure can be observed. Figure 3 (a1)- Figure 3 The element distribution diagram (a4) shows that the N element is also evenly dispersed in the carbon shell, and the particle size of the Cu / Cu2O core particles is as low as 60nm. This is because the porous carbon shell inhibits the aggregation of nanoparticles. Figure 3 (d)- Figure 3 In the TEM and HRTEM images shown in (f), stripes with lattice spacing of 0.208 nm and 0.246 nm were observed, corresponding to the (111) crystal plane of Cu and the (111) crystal plane of Cu2O, respectively, which also proves that a nano-Cu / Cu2O composite material is formed in the carbon layer.

[0083] The phase composition and crystallinity of Cu-BTC materials and nanocomposites were analyzed by XRD. Figure 4 As shown in (a), the prepared Cu-BTC material has good crystallinity and has the same characteristic peaks as the prior art. After carbonization at different temperatures for 2h, the original diffraction peaks of Cu-MOF disappeared, and new characteristic peaks appeared at 2θ=36.64°, 42.61°, 61.34° and 2θ=43.47°, 50.67° for Cu / Cu2O@NC-T (T=300, 400 and 500), corresponding to the (111) crystal plane, (200) crystal plane, (220) crystal plane of Cu2O and the (111) crystal plane, (200) crystal plane of Cu, respectively. Moreover, with the increase of carbonization temperature, Cu 0 The peak of Cu2O is enhanced while that of Cu2O is weakened, which indicates that the appropriate low temperature is conducive to the + The formation of Cu + Will be reduced to Cu 0 It can be seen that different content ratios of Cu can be obtained by adjusting different carbonization temperatures. + / Cu 0 .

[0084] In order to determine the surface functional groups of the adsorbent, FTIR analysis was performed. In the FTIR spectrum of Cu-BTC, Figure 4 (b) 715cm -1 and 740cm -1 The peak at 1357 / 1425cm is attributed to the stretching vibration of the CH bond. -1 and 1610 / 1705cm-1 The strong adsorption peaks at 605 cm correspond to the symmetric and asymmetric contraction vibrations of COO-. All the curves of Cu / Cu2O@NC-T (T=300, 400 and 500) do not show the FTIR peaks of the original Cu-BTC, and vibration bands of different intensities are detected at the same position. -1 The peak at 1615 cm is related to the vibration of Cu-O bond of Cu2O, while the peak at 1615 cm -1 The broad peak at is associated with the bending vibration of the C=C bond. In the Raman spectra of Cu / Cu2O@NC-T (T=300, 400 and 500), Figure 4 (c) shows that at a wavelength of 1331 cm -1 and 1584cm -1 The D band and the G band were detected. Generally speaking, the D band is associated with defects and disorder in the graphene layer, while the G band corresponds to the in-plane vibration of sp2 carbon atoms. Therefore, the intensity ratio of these two peaks (I D / I G ) represents the disorder of the crystal structure. D / I G The larger the value, the greater the structural defects and graphitization degree of the material, which is conducive to the contact between iodine and the active sites. The above conclusions prove that Cu / Cu2O@NC-T (T=300, 400 and 500) is carbonized and the intermediate Cu2O is generated.

[0085] Figure 5 This is the TGA curve of the thermal stability analysis of Cu-BTC material under N2 atmosphere. The 7.2% mass loss of the sample between 20℃-100℃ is caused by the evaporation of residual water on the surface. When the temperature increases to 280℃, the mass loss of Cu-BTC is 30.4%, which is the result of the loss of free ligands and some solvent molecules in the crystal. At 280℃-320℃, Cu-BTC dropped sharply by 34.8%, which is due to the oxidation of organic matter and the collapse of the skeleton structure. As the temperature continues to rise, the N-doped carbon skeleton continues to collapse, which is similar to the results of SEM, indicating that the calcination process promotes the structural defects and graphitization of the material, which is conducive to the contact of iodine with the active sites.

[0086] The specific surface area and pore size distribution of Cu-BTC materials and Cu / Cu2O@NC-T (T = 300, 400 and 500) were determined by N2 adsorption-desorption isotherms. Figure 6 As shown. The Cu-BTC material shows a typical type I isotherm, which corresponds to a sharp increase in adsorption at low relative pressure and is dominated by micropores and mesopores. Cu / Cu2O@NC-T (T=300, 400 and 500) belongs to the type IV isotherm, accompanied by an H3 type hysteresis loop, indicating that it is dominated by mesopores, such as Figure 6 (b) As shown in Table 1, the specific surface area of ​​the material decreased and the pore size increased after calcination, which is due to the collapse of the Cu-BTC pore structure and the formation of Cu and its oxides, resulting in the blockage of some micropores and mesopores. As the calcination temperature increases, the specific surface area of ​​the nanocomposite increases and the pore size decreases, which may be due to the formation of a new pore structure by the gas released by the decomposition of organic matter at high temperature. The data results show that the MOF-derived nano Cu / Cu2O adsorbent has a large specific surface area and rich pore structure, which is conducive to increasing the iodine adsorption active sites and contact area.

[0087] XPS was used to investigate the chemical composition and elemental valence of Cu / Cu2O@NC-T (T = 300, 400 and 500). Figure 4 (d) is the full spectrum scan result of Cu / Cu2O@NC-T (T=300, 400 and 500), indicating that the prepared material contains C, Cu, O and N. The high-resolution XPS spectrum of Cu 2p is shown in Figure 4 As shown in (e), the satellite peaks at the binding energies of 935.1 eV and 954.2 eV may originate from trace amounts of Cu + / Cu 0 The two typical characteristic peaks at binding energies of 932.3 eV and 952.1 eV are attributed to Cu + (Cu2O) / Cu 0 . Due to Cu + (Cu2O) and Cu 0 The chemical shift of Cu is very small, so it is difficult to determine the presence of copper. + and Cu 0 , the Cu LMM Auger spectrum was analyzed, such as Figure 4 (f) as described above; the characteristic peaks with binding energies of 570.0eV and 572.5eV correspond to Cu 0 and Cu + Moreover, the Cu + , Cu 0 and total copper content as Figure 7 As shown in Table 2. The total copper content of Cu / Cu2O@NC-T (T=300, 400 and 500) composites obtained after Cu-BTC was calcined at different temperatures did not fluctuate significantly, but the Cu + and Cu 0 As the calcination temperature increases, the content of Cu2O decreases and the content of Cu 0 The content of Cu increases, + / Cu 0The ratios decreased accordingly, which were 0.79 (Cu / Cu2O@NC-300), 0.64 (Cu / Cu2O@NC-400) and 0.48 (Cu / Cu2O@NC-500). 0 Affects Cu + to I - The adsorption effect. Figure 4 (g)- Figure 4 (i) is the XPS measurement spectra of C 1s, N 1s and O 1s. The C 1s spectrum can be fitted with three peaks, located at 284.7 / 286.6eV and 289.4eV, corresponding to CC, CN and C=O bonds, respectively. In the N 1s spectrum, the peak at 398.3eV belongs to pyridinic nitrogen (PdN), the peak at 400.1eV belongs to pyrrolic nitrogen (PyN), and the peak at 401.5eV corresponds to graphitic nitrogen (GrN). Nitrogen-containing porous carbon materials are beneficial to increase the affinity for iodine. Figure 4 The three peaks in (i) can be attributed to Cu-O (530.3 eV), C=O (531.4 eV) bonds and OH (533.2 eV) on the adsorbent surface.

[0088] In order to determine the iodine adsorption effect of nano-Cu / Cu2O@NC-T (T=300, 400 and 500) composites derived from Cu-MOF and the different contents of Cu + / Cu 0 The results showed that the difference in iodine capture capacity was 0.0447 W·m-1·K-1 and the adsorption capacity was 0.034 W·m-1·K-1. Figure 8 (a) and Fig. 9 As shown in Figure 2, the adsorption capacity of all samples for iodide increases with the initial I - The saturated adsorption capacity of Cu / Cu2O@NC-T (T=300, 400 and 500) is much greater than that of Cu-BTC ( Fig. 9 ), which indicates that the nano Cu / Cu2O particles wrapped in porous carbon shells generated by Cu-BTC carbonization can effectively enrich iodine ions. Figure 8 (a) has the lowest Cu + / Cu 0 The adsorption capacity of Cu / Cu2O@NC-500 with a content ratio of 1:1 was the lowest; surprisingly, Cu / Cu2O@NC-400 showed a higher iodine adsorption capacity than Cu / Cu2O@NC-300, while the Cu in Cu / Cu2O@NC-400 +The content of Cu / Cu2O@NC-300 is lower than that of Cu / Cu2O@NC-300. This phenomenon is because although Cu2O has a high affinity for iodide ions, it is easily oxidized to CuO by dissolved oxygen in the aqueous solution during the adsorption process, and an appropriate amount of Cu can undergo a disproportionation reaction with CuO to generate Cu2O to make up for this defect. The Cu content in Cu / Cu2O@NC-300 is too low, thus reducing the adsorption capacity of Cu2O. The Cu in Cu / Cu2O@NC-400 is + / Cu 0 The synergistic effect was fully exerted to enhance the iodine capture efficiency of Cu2O, thus showing the highest adsorption capacity, which indicates that the content of Cu is an important factor affecting the Cu / Cu2O-based adsorbent. The adsorption process of Cu / Cu2O@NC-T (T=300, 400 and 500) was further analyzed by fitting the isothermal adsorption results with the Langmuir model and the Freundlich model. It can be inferred from the fitting results shown in Table 3 that the fitting curve of the Langmuir model is more consistent with the adsorption data. Therefore, the adsorption of iodine ions by Cu / Cu2O@NC-T (T=300, 400 and 500) belongs to monolayer adsorption and is evenly distributed on the surface of the adsorbent. The saturated adsorption capacities of Cu / Cu2O@NC-300, Cu / Cu2O@NC-400 and Cu / Cu2O@NC-500 calculated by the Langmuir model are 81.45 mg / g, 91.05 mg / g and 68.48 mg / g, respectively.

[0089] Adsorption kinetics were conducted to investigate the temporal trend of the iodide ion adsorption capacity of Cu / Cu2O@NC-T (T = 300, 400, and 500). Figure 8 As shown in (b), in the initial stage of the reaction, due to the sufficient adsorption sites on the adsorbent surface and the large I - The concentration difference makes the adsorption reaction proceed rapidly. As the available adsorption sites are consumed and I - The concentration dropped sharply, the adsorption rate gradually decreased, and finally reached equilibrium. All adsorbents can reach I in a short time. - The adsorption equilibrium is related to the rich pore structure, large specific surface area and high activity of nano Cu / Cu2O particles of the nanocomposite materials. In addition, the adsorption equilibrium time of Cu / Cu2O@NC-300, Cu / Cu2O@NC-400 and Cu / Cu2O@NC-500 is about 70min, 50min and 80min respectively, which proves that the optimal Cu + / Cu 0 Not only is it beneficial to -The adsorption capacity and faster kinetics are also achieved. The pseudo-first-order kinetic model and the pseudo-second-order kinetic model were used to fit the experimental data, and the kinetic parameters obtained are shown in Table 4. The pseudo-second-order kinetics has a higher correlation coefficient, so it can better describe the adsorption behavior of iodine ions, indicating that chemical adsorption is dominant in the process. Therefore, based on the experimental results and data, we can infer that in the process of iodine adsorption by Cu / Cu2O@NC-T (T=300, 400 and 500) composite materials, a chemical reaction occurs between cuprous oxide and iodine ions, similar to the common Cu / Cu2O-based adsorbents in the past. Further, when the total copper content is close, Cu / Cu2O@NC-400 with a medium content of Cu2O has a better adsorption effect. Compared with the adsorption capacity and equilibrium time of adsorbents for removing iodine ions reported in other literature, Cu / Cu2O@NC-400 has an advantage (Table 7). Considering the adsorption capacity and adsorption equilibrium time of iodine, it is further preferred that the ratio of monovalent copper to zero-valent copper is 0.6-0.68.

[0090] Taking Cu / Cu2O@NC-400 as an example, the intrinsic energy change in the adsorption process was investigated by observing the adsorption performance of Cu / Cu2O@NC-400 for iodine ions at different solution temperatures. The experimental data were fitted by the Langmuir model and the Freundlich model. The results are shown in Figure 8 (c) and Table 5. As the temperature increases from 298K to 308K and 318K, the Cu / Cu2O@NC-400 - The adsorption capacity of Cu / Cu2O@NC-400 decreased from 91.05 mg / g to 82.84 mg / g and 79.19 mg / g, indicating that the adsorption process is an exothermic reaction and low temperature is conducive to the removal of iodide ions. Table 6 shows the relevant thermodynamic parameters calculated according to the Hoff equation. The △G at all temperatures is negative, indicating that Cu / Cu2O@NC-400 has a strong adsorption capacity on I - The adsorption process can proceed spontaneously. △H<0, which proves that the adsorption reaction is an exothermic process. It can be inferred from △S<0 that the disorder of the solid-liquid interface in this system is reduced, which is attributed to the I in the solution. - Combined with nano-Cu / Cu2O to form a precipitate.

[0091] Taking Example 2 as an example, DFT theoretical calculation is used to illustrate I - Combination mode with Cu2O. Fig.10 , site 1 and site 2 represent two different adsorption sites on the Cu2O(111) crystal surface. Fig.11 For I - The stable configuration after adsorption by Cu2O and Cu, I -The bond length when adsorbed to site 1 of Cu2O (named I-Cu2O-1) is 2.304Å, and the adsorption energy is -1.42eV, indicating that a chemical bond is formed between the I atom and the Cu atom through chemical reaction. - The bond length and adsorption energy when adsorbed to Cu2O site 2 are 2.178 Å and -2.49 eV, respectively, which are much smaller than I - The bond length of the adsorbed Cu(111) site is much more negative than that of I - The adsorption energy on the Cu(111) crystal surface is shown in Table 1. This indicates that Cu2O plays a dominant role in the adsorption of iodine ions and I- is more likely to bind to Cu2O, which explains the adsorption of Cu + / Cu 0 Cu / Cu2O@NC-500 with the lowest content ratio has the lowest iodine adsorption capacity.

[0092] The pH value of the solution can affect the active sites on the surface of the adsorbent and thus affect the capture efficiency of iodine. Taking Example 2 as an example, the adsorption capacity of Cu / Cu2O@NC-400 under different acid-base environments was explored. Figure 8 The experimental data of (d) show that it exhibits excellent adsorption performance under acidic conditions. At solution pH = 3, the adsorption capacity of Cu / Cu2O@NC-400 reaches 123.72 mg / g, which is attributed to the higher H + The concentration can promote Cu + The release of more I - captured on the adsorbent surface. Fig.12 The Zeta potential of Cu / Cu2O@NC-400 at different pH values ​​and the pH value after adsorption. The Zeta potential is positive when the pH value is 3-7, and the zero charge point is around pH 7.8. The pH value at the zero charge point is conducive to the adsorption of iodine anions. Example 2 The increase in pH after adsorption is due to Cu 0 / Cu2O and I - During the reaction, H + .

[0093] A large number of anions are commonly found in wastewater, so , Adsorption of Cu / Cu2O@NC-400 - The impact of Figure 8 (e) and There is little effect on the iodine adsorption capacity, which is attributed to their strong acid properties. The minor inhibitory effect on iodine adsorption may be due to the formation of CuCl complexes that occupy the I -Adsorption sites. In general, under the interference of the above anions, Cu / Cu2O@NC-400 still has a good capture ability for iodine ions.

[0094] Although Cu / Cu2O@NC-T (T=300, 400 and 500) showed good adsorption performance in aqueous solution, the iodide ion concentration in actual medical wastewater is relatively low. Therefore, taking Example 2 as an example, the removal effect of Cu / Cu2O@NC-400 on trace iodine was tested by the IC method. Figure 8 (f)- Figure 8 (g) shows that the iodine ion removal efficiency at different initial concentrations (C1=0.1mg / L, C2=0.3mg / L and C3=0.5mg / L) can reach more than 92%, and the iodine concentration after adsorption is lower than the limit of 0.04mg / L specified in China's "Surface Water Environmental Quality Standard" (GB 3838-2002). Figure 8 (h) is 1 - The iodine adsorption capacity of Cu / Cu2O@NC-400 changes with contact time when the initial concentration is 0.3 mg / L. Within 10 minutes, the iodine adsorption capacity of Cu / Cu2O@NC-400 reaches about 0.27 mg / g, and the removal rate reaches 90%, which depends on the high affinity of cuprous oxide and zero-valent copper for iodine and the high dispersion of nano-Cu / Cu2O. The concentration of residual copper in the treated solution is obtained by ICP-MS, such as Figure 8 As shown in (e), the dissolved copper content in all solutions is far below the safety threshold (2 mg / L) specified by WHO. These data demonstrate the practicality and safety of Cu / Cu2O@NC-T (T=300, 400 and 500) composite materials.

[0095] When treating radioactive wastewater, the adsorbent needs to have strong radiation resistance. After irradiating Cu / Cu2O@NC-T (T=300, 400 and 500) with Coγ rays (100KGy), it was used to remove iodine-containing wastewater. Figure 8 (i) is shown. Figure 8 (i) It can be seen that the iodine adsorption capacity of Cu / Cu2O@NC-300, Cu / Cu2O@NC-400 and Cu / Cu2O@NC-500 has basically no change after irradiation, indicating that the prepared materials have good irradiation stability. In addition, in order to study the stable storage after adsorption of radioactive iodine, the adsorption products were immersed in water and ultrasonically treated, such as Figure 8 As shown in (j), after immersion for 24 h and ultrasonication for 30 min, - The release amounts were only 1.12% and 3.25%, which was due to the chemical adsorption of the adsorbent, verifying the adsorption stability of the sample.

[0096] The differences in adsorption behavior between the synthesized materials prompted further investigation of I - In order to further reveal the absorption mechanism of I by Cu / Cu2O@NC-T (T=300, 400 and 500) composite materials - The adsorption mechanism of Cu / Cu2O@NC-I was characterized and analyzed. Taking Example 2 as an example, the microscopic morphology of Cu / Cu2O@NC-400 after adsorption of iodine ions was observed by SEM. The results are as follows: Fig.13 As shown in (a), the octahedral morphology of the adsorbent breaks down after iodine enrichment, and a nanorod-like structure grows on the surface. This is due to the interaction between Cu / Cu2O and I - The chemical reaction occurred. The chemical structure changes of Cu / Cu2O@NC-I were further characterized by TEM and HRTEM. Fig.13 (b)- Fig.13 (c) shows that CuI lattice fringes were found on the adsorbent surface, indicating that the adsorption product was CuI precipitate. Fig.13 (b1)- Fig.13 (b5) and Fig.14 The element distribution and EDS spectrum showed that Cu, I, C, O, and N were uniformly distributed on the adsorbent surface, confirming the absorption of iodine.

[0097] XRD images of Cu / Cu2O@NC-400 before and after iodine adsorption Fig.15 (a) shows that the diffraction peaks belonging to cuprous oxide and metallic copper all disappear and weaken, proving that Cu + / Cu 0 Full synergy and Cu 2 High utilization rate of O. We found that the diffraction peaks of CuI appeared at 2θ=25.6°, 29.7°, 42.4°, 50.1°, 61.5° and 67.5° in the adsorbed material, corresponding to the (111) crystal plane, (200) crystal plane, (220) crystal plane, (311) crystal plane, (400) crystal plane and (331) crystal plane of CuI (JCPDS No.06-0246), respectively. XRD analysis shows that both Cu2O and Cu play a role in the iodine capture process, and further verifies that the final product is CuI.

[0098] In order to obtain the elemental valence and chemical state of Cu / Cu2O@NC-I, XPS analysis was performed, taking Example 2 as an example. Fig.15 The I 3d peak at the binding energy of 625.0 eV in (b) indicates that iodine is successfully adsorbed. Fig.15(d) Compared with Cu / Cu2O@NC-400, the peaks of Cu 2p3 / 2 and Cu 2p3 / 2 of the adsorbed sample shifted to the higher energy level by 0.2eV-0.3eV, which is attributed to the change of the local chemical environment of Cu. Fitting Cu 2p3 / 2 can convolute two peaks. The peak at 932.5eV belongs to Cu + (CuI). The peak at the binding energy of 935.1 eV proves that Cu 2+ The presence of (CuO) phase, which is formed by the oxidation of part of Cu2O in Cu / Cu2O@NC by dissolved oxygen in the reaction system. The peak intensity of CuO in Cu / Cu2O@NC-I is significantly weaker than that in Cu / Cu2O@NC, which indicates that CuO participates in the process of iodine adsorption. 0 Can undergo disproportionation reaction to generate I - Has high affinity for Cu + (Cu2O), no diffraction peak of CuO was found in the XRD spectrum, which is because the CuO content in the sample is too small. Fig.15 (c) is the XPS spectrum of I 3d of the sample after adsorption. The two peaks at binding energies of 619.5 eV and 631.3 eV indicate that CuI is the final product of the iodine adsorption process, which is attributed to the interaction between Cu2O and I - Combined with irreversible chemical reactions, the corresponding phenomenon can also be explained by Fig.17 This is confirmed by the shift of the Cu-O bond of Cu2O in the O 1s spectrum, which is consistent with the results of XRD and TEM.

[0099] Therefore, based on the above characterization analysis results and experimental phenomena, the potential Cu / Cu2O@NC-T (T = 300, 400 and 500) adsorption I - The mechanism, such as Fig.16 As shown. I in aqueous solution - Adsorbed onto the Cu / Cu2O surface, Cu2O can efficiently adsorb I - In addition, zero-valent Cu contacts CuO and reacts to form Cu2O, thereby participating in the I - .

[0100] In summary, a new type of nano-Cu / Cu2O composite material was successfully synthesized by carbonizing Cu-BTC material for the removal of iodide ions. Batch adsorption experiments showed that the prepared material (Cu / Cu2O@NC-400) has fast kinetic characteristics and excellent working performance. It can reach adsorption equilibrium in 40 minutes and the adsorption capacity under acidic conditions (pH=3) reaches 123.72 mg / g. Moreover, Cu / Cu2O@NC-T (T=300, 400 and 500) can effectively remove trace I in the solution. -, after adsorption - The removal rate was higher than 92% when the concentration was below 30 ppb, and only a very small amount of copper remained in the solution. Mechanism studies and DFT calculations showed that Cu2O played a major role in the capture of iodide ions. - Combined with CuI precipitation, it was fixed. More importantly, different content ratios of Cu / Cu2O led to differences in adsorption rate and adsorption capacity, and Cu / Cu2O@NC-400 obtained the best adsorption performance. This work lays a foundation for the design of Cu / Cu2O-based adsorption materials and the enhancement of the adsorption capacity of Cu2O for iodine, providing application prospects for the deep treatment of wastewater containing radioactive iodine.

[0101] It should be noted that the terms used in the present invention are only for describing specific embodiments, rather than limiting the scope of the present application. As shown in the present specification, unless the context clearly indicates an exception, the words "one", "a", "a kind of" and / or "the" do not specifically refer to the singular, but may also include the plural. The terms "include", "comprise" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method or device. In the absence of more restrictions, the elements defined by the sentence "include one..." do not exclude the presence of other identical elements in the process, method or device including the elements.

[0102] It should also be noted that the orientations or positional relationships indicated by the terms "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside", etc. are based on the orientations or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. Unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", etc. should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be a connection between the two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0103] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the technical solutions of the embodiments of the present invention.

[0104] References: [1]Chen J, Wang P, Gong C, et al (2024) Bimetal ZIFs-derivedCu 0 Embedded in nitrogen-doped carbon framework activation of molecular oxygen for efficient iodide elimination. J. Environ. 12: 112235. https: / / doi.org / https: / / doi.org / 10.1016 / j.jece.2024.112235. [2]Zhang T, Yue [3]Mao P, Liu Y, Jiao Y, et al (2016) Enhanced uptake of iodide onAg@Cu2O nanoparticles. Chemosphere 164: 396-403. https: / / doi.org / https: / / doi.org / 10.1016 / j.chemosphere.2016.08.116. [4]Chen J, Gao Q, Zhang X, et al (2019) Nanometer mixed-valencesilver oxide enhancing adsorption of ZIF-8 for removal of iodide in solution.Sci. Total Environ. 646: 634-644. https: / / doi.org / https: / / doi.org / 10.1016 / j.scitotenv.2018.07.298. [5]Chen J, Gu A, Djam Miensah E, et al (2021) Core-shell ZnO@Cu2Oencapsulated Ag NPs nanocomposites for photooxidation-adsorption of iodideanions under visible light. Sep. Purif. Technol. 262: 118328. https: / / doi.org / https: / / doi.org / 10.1016 / j.seppur.2021.118328. [6]Theiss F L, Ayoko G A, Frost R L (2016) Iodide removal using LDHtechnology. Chem. Eng. J. 296: 300-309. https: / / doi.org / https: / / doi.org / 10.1016 / j.cej.2016.02.039. [7]Chen J, Wang J, Gao Q, et al (2020) Enhanced removal of I− onhierarchically structured layered double hydroxides by in suit growth of Cu / Cu2O. J. Environ. Sci. 88: 338-348. https: / / doi.org / https: / / doi.org / 10.1016 / j.jes.2019.09.024. [8]Mao P, Liu Y, Liu X, et al (2017) Bimetallic AgCu / Cu2O hybrid forthe synergetic adsorption of iodide from solution. Chemosphere 180: 317-325.https: / / doi.org / https: / / doi.org / 10.1016 / j.chemosphere.2017.04.038.

Claims

1. A Cu 0 / Cu + A nanocomposite material, characterized in that The composite material is a composite material of copper metal and cuprous oxide, a carbon layer is provided on the surface of the composite material, and nitrogen elements are uniformly dispersed in the carbon layer and the composite material.

2. The nanocomposite material according to claim 1, characterized in that The ratio of monovalent copper to zero-valent copper in the copper metal and cuprous oxide composite material is 0.45-0.

8.

3. Cu according to any one of claims 1 to 2 0 / Cu + The method for preparing a nanocomposite material is characterized in that: The preparation method comprises: The copper metal frame is placed in an inert atmosphere for calcination to obtain a nanocomposite material. The calcination temperature is 300°C-500°C, the calcination time is 1.5h-2.5h, and the heating rate to reach the calcination temperature is 1.5°C / min-2.5°C / min.

4. The preparation method according to claim 3, characterized in that: The inert atmosphere includes one of nitrogen, argon, helium and argon.

5. The preparation method according to claim 3, characterized in that: The preparation method of the copper metal frame comprises: dissolving a copper source and polyvinyl pyrrolidone in a solvent to obtain a solution A; dissolving 1,3,5-benzenetricarboxylic acid in a solvent to obtain a solution B; mixing the solution A and the solution B, performing a hydrothermal reaction after the mixing, cooling, washing and drying to obtain the copper metal frame.

6. The preparation method according to claim 5, characterized in that: The copper source includes one or more of copper nitrate trihydrate, copper nitrate nonahydrate, and copper nitrate.

7. The preparation method according to claim 5, characterized in that: Calculated based on the mass of copper in the copper source, the mass ratio of the copper source to polyvinyl pyrrolidone is 0.41:0.665; The solvent consists of N,N-dimethylformamide and anhydrous ethanol, and the volume ratio of N,N-dimethylformamide to anhydrous ethanol is 1:1; The mass concentration of the polyvinyl pyrrolidone in the solvent is 0.665 g / 30 mL; The mass concentration of the 1,3,5-benzenetricarboxylic acid in the solvent is 0.735 g / 30 mL.

8. The preparation method according to claim 5, characterized in that: The volume ratio of solution A to solution B is 1:1; The temperature of the hydrothermal reaction is 110°C-130°C, and the time of the hydrothermal reaction is 3.5h-4.5h; The step of cooling to room temperature is 26°C-28°C.

9. The preparation method according to claim 5, characterized in that: The specific method of washing comprises: washing with N,N-dimethylformamide and anhydrous ethanol in sequence for 3-5 times; The drying temperature is 50° C.-70° C., and the drying time is 11 h-13 h.