Irreversible bond-linked auto-polymerization covalent organic framework material, composite electrocatalyst, and preparation method and application of irreversible bond-linked auto-polymerization covalent organic framework material and composite electrocatalyst
A self-polymerizing covalent organic framework material connected by irreversible bonds addresses the scalability and performance issues of COFs, enabling efficient large-scale production and high-performance electrocatalysts.
Patent Information
- Application Number
- CN202411338972.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-25
AI Technical Summary
The synthesis of irreversibly bonded covalent organic frameworks (COFs) is difficult to scale up due to unevenness and long reaction times, and precious metal-based electrocatalysts face issues like metal nanoparticle agglomeration and low catalytic performance when used with reversible COFs.
A self-polymerizing covalent organic framework material connected by irreversible bonds is synthesized using Suzuki coupling and melt polymerization, simplifying the process and enabling high crystallinity and stability, with a 'two-in-one' strategy for large-scale production and high catalytic performance.
The method accelerates reaction rates, shortens preparation time, and allows for industrial-scale synthesis of COFs with high crystallinity and stability, while the electrocatalyst maintains long-cycle stability and high catalytic performance.
Smart Images

Figure CN119060276A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of covalent organic framework materials, and in particular to an irreversible bond-connected self-polymerizing covalent organic framework material, a composite electrocatalyst, and a preparation method and application thereof. Background Art
[0002] Covalent organic frameworks (COFs) are a class of crystalline organic porous polymers connected by covalent bonds of organic monomers. Due to their adjustable structure, high specific surface area, low density, and stable chemical properties, COFs are widely used in catalysis, gas adsorption and separation, sensing, energy storage, and optical devices. After years of development, COFs have developed a variety of connection methods such as borate, imine, ethylene, amide, imide, and ester. Among them, COFs materials connected by irreversible bonds have high crystallinity and high stability.
[0003] It has broad application prospects and advantages. However, the synthesis of COFs with irreversible bond connection is very difficult, and the commonly used solvothermal method is basically unable to be prepared on a large scale, which affects its further application.
[0004] The preparation of irreversibly bonded COFs by melt polymerization is considered to be a necessary method for large-scale industrial mass production, and kilogram-level synthesis has been achieved. However, during the synthesis process, the melt is prone to unevenness during large-scale synthesis, which inevitably leads to a decrease in crystallinity. In addition, the existing synthesis method takes a long time (5-7 days) and the reaction environment must be strictly deoxygenated. The synthesis process is complicated and difficult to mass produce.
[0005] Existing electrocatalysts are usually metal-based catalysts, especially precious metal-based catalysts, such as platinum, palladium, ruthenium, rhodium, etc. Common precious metal single-substance electrodes are usually too expensive and have extremely low atomic utilization, making them difficult to use in industrial environments. Therefore, dispersing metals onto COFs carriers is considered to be an effective strategy. However, the precious metal-based catalysts supported by reversibly bonded COFs currently have problems such as metal nanoparticle agglomeration and deactivation, and the carrier is difficult to withstand a long-term current working environment, resulting in low catalytic performance of the electrocatalyst using it as a carrier and high catalyst cost, which limits its application.
[0006] Based on this, it is of great significance to develop a self-polymerizing covalent organic framework material with irreversible bond connection and a high-performance electrocatalyst using it as a carrier. Summary of the invention
[0007] The present application provides a self-polymerizing covalent organic framework material connected by irreversible bonds, a composite electrocatalyst, and a preparation method and application thereof, aiming to solve the problems that the existing irreversibly bonded COFs preparation process is complex and difficult to produce on a large scale, and the existing electrocatalysts have low catalytic performance.
[0008] In order to achieve the above objectives, the present application adopts the following technical solutions.
[0009] In a first aspect of the present application, there is provided a self-polymerizing covalent organic framework material connected by irreversible bonds, which is prepared by synthesizing monomers having equal amounts of reactive functional groups by Suzuki coupling and then self-polymerizing the monomers;
[0010] The monomer has an equal amount of aldehyde group and methyl group, or has an equal amount of phthalic acid group and amide group.
[0011] Another aspect of the present application provides a method for preparing the above-mentioned irreversibly bonded self-polymerizing covalent organic framework material, comprising:
[0012] S1, organic matter A, organic matter B, potassium carbonate and catalyst A are subjected to solvent reaction in a reactor under a nitrogen atmosphere to obtain a monomer;
[0013] S2, the monomer and the catalyst B are subjected to a melt condensation reaction in a reactor, and the product is cleaned and purified to obtain a self-polymerizing covalent organic framework material connected by irreversible bonds.
[0014] In some embodiments, the organic compound A is an aromatic compound having multiple bromine or iodine functional groups;
[0015] The organic compound B is an aromatic compound having a phenylethynyl group, a phenylboronic acid group or a phenylboronic acid pinacol ester group;
[0016] The catalyst A is an organic complex of palladium;
[0017] The solvent includes any one or a combination of water, tetrahydrofuran, 1,4-dioxane, N,N-dimethylformamide and toluene.
[0018] In some embodiments:
[0019] The organic matter A includes 4,8-dibromo-2,6-dimethyl[1,3]oxazacyclopenta[4',5':4,5]benzo[d][1,3]oxazacyclopenta, 1,3,5-tribromo-2,4,6-triiodobenzene, 6,7-dibromo-2,3-dimethylquinoxaline, 5,8-dibromo-2,3-dimethylquinoxaline, 1,2-dibromo-4,5-diiodobenzene, 1,3-dibromo-4,6-diiodobenzene, 1 , 4-dibromo-2,5-diiodobenzene, 4-bromo-2,6-dimethylpyridine, 4-bromo-6-methylpyridine-2-carboxaldehyde, 1,4-dibromobenzene, 1,3,5-tribromobenzene, 1,3,4,6-tetrabromo-2,5-dimethylbenzene, 2,7-dibromopyrene, 2,6-dibromonaphthalene, 2,6-dibromoanthracene, 3,6-dibromobenzene-1,2,4,5-tetracarboxylic acid or 3,6-diiodobenzene-1,2,4-5-tetracarboxylic acid;
[0020] and / or:
[0021] The organic matter B includes 4-formylphenylboronic acid, 3-fluoro-4-formylphenylboronic acid, 3,5-difluoro-4-formylphenylboronic acid, 4-formyl-3,5-dimethoxyphenylboronic acid, 2-methoxy-4-(4,4,5,5-tetramethylethyl-1,3,2-dioxaborolanol-2-yl)benzaldehyde, 4-boric acid pinacol ester-2-hydroxybenzaldehyde, 2-nitro-4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolanol-2-yl)benzaldehyde, 4'- Formylbiphenyl-4-boronic acid pinacol ester; 4-(4-formylphenyl)phenyl-2-boronic acid pinacol ester, 2-methyl-5-(4,4,5,5-tetramethyl-1,3,2-dioxaborol-2-yl)pyridine, 4-ethynylbenzene-1-carboxaldehyde, 5-(4,4,5,5-tetramethyl-1,3,2-dioxaborol-2-yl)benzene-1,3-dicarboxaldehyde, 1,4-phenyldiboronic acid pinacol ester, 4,4'-biphenyldiboronic acid pinacol ester, N-(4-( 4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenyl)benzamide, N-(2-fluoro-4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenyl)benzamide, N-(2,6-difluoro-4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenyl)benzamide, N-(2-hydroxy-4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenyl)benzamide any one of N-(4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenyl)benzamide, N-(4'-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)-[1,1'-biphenyl]-4-yl)benzamide or N-(4-(4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenyl)ethynyl)phenylbenzamide;
[0022] and / or:
[0023] The catalyst A includes any one of tetrakis(triphenylphosphine)palladium(0), bis(triphenylphosphine)palladium dichloride, 1,1-bis(diphenylphosphino)ferrocenepalladium dichloride or palladium acetate.
[0024] In some embodiments, the monomer has equal amounts of aldehyde groups and methyl groups, or has equal amounts of phthalic acid groups and amide groups;
[0025] The catalyst B is a compound containing anhydride functional groups, a compound containing acyl chloride functional groups or a compound containing carboxylic acid functional groups.
[0026] In some embodiments, the molar ratio of the organic matter A, organic matter B, potassium carbonate and catalyst A is 1:(3-4):(3-4):(0.1-0.2);
[0027] and / or:
[0028] The molar ratio of the catalyst B to the monomer is 1:1-10:1;
[0029] The temperature of the solvent reaction is 70-80°C;
[0030] The temperature of the melt condensation reaction is 160-250°C.
[0031] Another aspect of the present application provides the use of the irreversibly bonded self-polymerizing covalent organic framework material or the irreversibly bonded self-polymerizing covalent organic framework material prepared by the preparation method in an electrocatalyst.
[0032] In another aspect of the present application, a composite electrocatalyst is provided, comprising an electrocatalyst and a carrier supporting the electrocatalyst;
[0033] The carrier is the above-mentioned irreversibly bonded self-polymerizing covalent organic framework material or the irreversibly bonded self-polymerizing covalent organic framework material prepared by the above-mentioned preparation method.
[0034] Another aspect of the present application provides a method for preparing the composite electrocatalyst, comprising:
[0035] The self-polymerizing covalent organic framework material connected by irreversible bonds is dispersed in a solvent, a metal salt solution is added, and the reaction is carried out in a nitrogen atmosphere under the action of a reducing agent, and the solid product is collected, washed and dried to obtain the product;
[0036] The metal salt includes at least one of sodium chloropalladate, chloroauric acid, sodium chloroplatinate, ruthenium chloride, rhodium chloride, silver nitrate, and copper chloride;
[0037] The solvent is at least one of water, acetonitrile, ethylene glycol, ethanol, methanol or N-methylpyrrolidone;
[0038] The reducing agent includes any one of sodium citrate, sodium borohydride or potassium borohydride.
[0039] Another aspect of the present application provides use of the above composite electrocatalyst in electrocatalytic synthesis of ammonia.
[0040] Compared with the prior art, the beneficial effects of this application are:
[0041] The irreversibly bonded self-polymerizing covalent organic framework material provided in the present application utilizes a "two-in-one" strategy and melt polymerization, simplifies the synthesis process, accelerates the reaction rate, shortens the preparation time, and has the potential for further scale-up of the synthesis; the irreversibly bonded self-polymerizing covalent organic framework material of the present application has high crystallinity, good stability, and a large specific surface area, and the electrocatalyst prepared using it as a carrier has high catalytic performance.
[0042] The present application successfully loads and disperses a noble metal-based catalyst by using a self-polymerizing covalent organic framework material connected by irreversible bonds as a metal catalyst carrier, which achieves long-cycle stability under catalytic conditions; it has higher electrocatalytic selectivity and higher yield than existing covalent organic framework material-based catalysts. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments recorded in the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0044] Figure 1 XRD spectrum of self-polymerized covalent organic framework material connected by irreversible bonds;
[0045] Figure 2 This is the infrared test spectrum of the self-polymerized covalent organic framework material connected by irreversible bonds;
[0046] Figure 3 The isothermal nitrogen adsorption-desorption curve of the self-polymerized covalent organic framework material connected by irreversible bonds at 77K;
[0047] Figure 4 The ammonia yield and Faraday efficiency of the composite electrocatalyst at different voltages;
[0048] Figure 5 This is the catalytic activity diagram of the composite electrocatalyst after 15 cycles of operation. DETAILED DESCRIPTION
[0049] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0050] In the following description of this embodiment, the terms "include", "comprising", "having" and "containing" are all open terms, meaning including but not limited to.
[0051] In the following description of this embodiment, the term "and / or" is used to describe the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, B exists alone, and A and B exist at the same time. A and B can be singular or plural. The character " / " generally indicates that the associated objects before and after are in an "or" relationship.
[0052] In the following description of this embodiment, the term "at least one" refers to one or more, and "plurality" refers to two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0053] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0054] Those skilled in the art should understand that in the following description of the embodiments of the present application, the order of serial numbers does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0055] Those skilled in the art will appreciate that the numerical ranges in the embodiments of the present application are to be construed as specifically disclosing each intermediate value between the upper and lower limits of the scope. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present application. The upper and lower limits of these smaller ranges may be independently included or excluded in the scope.
[0056] Unless otherwise specified, the technical / scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which this application belongs. Although this application only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of this application. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0057] In a first aspect, the present application provides a self-polymerizing covalent organic framework material connected by irreversible bonds, which is prepared by synthesizing monomers having equal amounts of reactive functional groups by Suzuki coupling and then self-polymerizing the monomers;
[0058] The monomer has an equal amount of aldehyde group and methyl group, or has an equal amount of phthalic acid group and amide group.
[0059] The self-polymerizing covalent organic framework material connected by irreversible bonds provided in the present application utilizes a "two-in-one" strategy and melt polymerization, simplifies the synthesis process, accelerates the reaction rate, shortens the preparation time, has the potential for further scale-up of the synthesis, and is suitable for industrial production.
[0060] The irreversibly bonded self-polymerizing covalent organic framework material of the present application has high crystallinity, good stability, and a large specific surface area, and the electrocatalyst prepared using the material as a carrier has high catalytic performance.
[0061] The irreversibly bonded self-polymerizing covalent organic framework material of the present application includes a self-polymerizing covalent organic framework material connected by a polyimide group, a polyether group, an azo group, an ether bond group, a triazine group, an imidazole group, an oxazolyl group, a thiazole group or a pyrazine group.
[0062] In a second aspect, the present application provides a method for preparing the above-mentioned irreversibly bonded self-polymerizing covalent organic framework material, comprising:
[0063] S1, organic matter A, organic matter B, potassium carbonate and catalyst A are subjected to solvent reaction in a reactor under a nitrogen atmosphere to obtain a monomer;
[0064] In the present application, organic matter A is an aromatic compound having multiple bromine or iodine functional groups; organic matter B is an aromatic compound having phenylethynyl, phenylboronic acid or phenylboronic acid pinacol ester. In the present application, the reaction raw materials are subjected to a solvent reaction at 70-80°C, and organic matter A and organic matter B undergo a suzuki coupling reaction to obtain a monomer having an equal amount of aldehyde group and methyl group, or having an equal amount of phthalic acid dicarboxyl group and amide.
[0065] Specifically, the organic substance A can be selected from 4,8-dibromo-2,6-dimethyl[1,3]oxazacyclopenta[4',5':4,5]benzo[d][1,3]oxazacyclopenta[1,3], 1,3,5-tribromo-2,4,6-triiodobenzene, 6,7-dibromo-2,3-dimethylquinoxaline, 5,8-dibromo-2,3-dimethylquinoxaline, 1,2-dibromo-4,5-diiodobenzene, 1,3-dibromo-4,6-diiodobenzene, Any one of 1,4-dibromo-2,5-diiodobenzene, 4-bromo-2,6-dimethylpyridine, 4-bromo-6-methylpyridine-2-carbaldehyde, 1,4-dibromobenzene, 1,3,5-tribromobenzene, 1,3,4,6-tetrabromo-2,5-dimethylbenzene, 2,7-dibromopyrene, 2,6-dibromonaphthalene, 2,6-dibromoanthracene, 3,6-dibromobenzene-1,2,4,5-tetracarboxylic acid or 3,6-diiodobenzene-1,2,4-5-tetracarboxylic acid.
[0066] Organic matter B can be selected from 4-formylphenylboronic acid, 3-fluoro-4-formylphenylboronic acid, 3,5-difluoro-4-formylphenylboronic acid, 4-formyl-3,5-dimethoxyphenylboronic acid, 2-methoxy-4-(4,4,5,5-tetramethylethyl-1,3,2-dioxaborol-2-yl)benzaldehyde, 4-boric acid pinacol ester-2-hydroxybenzaldehyde, 2-nitro-4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)benzaldehyde, 4'-formylphenylboronic acid, 4-(4,4,5,5-tetramethylethyl ... Acylbiphenyl-4-boronic acid pinacol ester; 4-(4-formylphenyl)phenyl-2-boronic acid pinacol ester, 2-methyl-5-(4,4,5,5-tetramethyl-1,3,2-dioxaborol-2-yl)pyridine, 4-ethynylbenzene-1-carboxaldehyde, 5-(4,4,5,5-tetramethyl-1,3,2-dioxaborol-2-yl)benzene-1,3-dicarboxaldehyde, 1,4-phenyldiboronic acid pinacol ester, 4,4'-biphenyldiboronic acid pinacol ester, N-(4-( 4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenyl)benzamide, N-(2-fluoro-4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenyl)benzamide, N-(2,6-difluoro-4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenyl)benzamide, N-(2-hydroxy-4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenyl)benzamide any one of N-(4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenyl)benzamide, N-(4'-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)-[1,1'-biphenyl]-4-yl)benzamide or N-(4-(4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenyl)ethynyl)phenylbenzamide
[0067] Catalyst A is used to catalyze the Suzuki coupling reaction of organic matter A and organic matter B. Catalyst A is an organic complex of palladium, including any one of tetrakis(triphenylphosphine)palladium(0), bis(triphenylphosphine)palladium dichloride, 1,1-bis(diphenylphosphino)ferrocenepalladium dichloride or palladium acetate.
[0068] The solvent includes any one or a combination of water, tetrahydrofuran, 1,4-dioxane, N,N-dimethylformamide and toluene.
[0069] In the present application, in order to achieve better results, the molar ratio of organic matter A, organic matter B, potassium carbonate and catalyst A is preferably 1:(3-4):(3-4):(0.1-0.2); the preferred solvent reaction temperature is 70-80°C.
[0070] In the present application, the monomer has an equal amount of aldehyde group and methyl group, or has an equal amount of phthalic acid dicarboxyl group and amide. Among them, the monomer having an equal amount of aldehyde group and methyl group includes a compound having any of the following structures:
[0071]
[0072] Monomers having equal amounts of phthalic acid and amide, including compounds having any of the following structures:
[0073]
[0074] S2, the monomer and the catalyst B are subjected to a melt condensation reaction in a reactor, and the product is cleaned and purified to obtain a self-polymerizing covalent organic framework material connected by irreversible bonds.
[0075] In the present application, catalyst B is a compound containing anhydride functional groups, a compound containing acyl chloride functional groups or a compound containing carboxylic acid functional groups, such as one or more of benzoic anhydride, sodium benzoate, benzoyl chloride, 4-trifluoromethylbenzoic anhydride, 4-methoxybenzoic anhydride, acetic anhydride, trifluoroacetic anhydride, benzoic acid, 4-fluorobenzoic acid, acetic acid, formic acid and propionic acid.
[0076] In the present application, monomers and catalyst B are added to the reactor, the reactor is closed, and heated to 160-250° C. for melt condensation reaction. The reactor can be an oxygen-free environment or an aerobic environment; when an oxygen-free environment is selected, the reactor is evacuated to a pressure of ≤0.15 mmHg.
[0077] The molar ratio of catalyst B to monomer is preferably 1:1-10:1, more preferably 6:1-8:1.
[0078] The reactor can be a high temperature and high pressure resistant Pyrex tube, an ampoule bottle requiring flame sealing, or a polytetrafluoroethylene lined high pressure reactor.
[0079] In the present application, the product of the melt condensation reaction is immersed in DMF to remove unreacted monomers, then washed with methanol to remove excess catalyst, and then the product is dried at 60-150° C. to obtain a self-polymerizing covalent organic framework material connected by irreversible bonds.
[0080] The irreversibly bonded self-polymerizing covalent organic framework material prepared in the present application has a chemical structure including any one of the following general formulas:
[0081]
[0082] The hexagons and quadrilaterals represent the remaining aromatic rings and aromatic heterocyclic functional groups in the above monomers except the functional groups participating in the synthesis reaction.
[0083] The irreversibly bonded self-polymerizing covalent organic framework material prepared in the present application has high crystallinity and high stability. The electrocatalyst prepared with it as a carrier can withstand a long period of current working environment, has high electrocatalytic performance, and has broad application prospects.
[0084] The present application also provides a composite electrocatalyst, which uses the above-mentioned self-polymerized covalent organic framework material connected by irreversible bonds as a carrier to load a metal electrocatalyst. The composite electrocatalyst carrier has high stability and can withstand a long-term current working environment. The metal nanoparticles are not easy to agglomerate and deactivate, and have high electrocatalytic performance.
[0085] The present application also provides a method for preparing the composite electrocatalyst, comprising:
[0086] The self-polymerizing covalent organic framework material connected by irreversible bonds is dispersed in a solvent, a metal salt solution is added, and the reaction is carried out in a nitrogen atmosphere under the action of a reducing agent, and the solid product is collected, washed and dried to obtain the product.
[0087] Specifically, the irreversibly bonded self-polymerizing covalent organic framework material is ground into fine powder and dispersed in a solvent, and ultrasonically treated for 30 minutes; then a metal salt solution is dropped into it, stirred overnight, a reducing agent is added, the temperature is controlled at 50-120°C, and stirred for 1-8 hours in a nitrogen atmosphere, and the metal nanoparticles are loaded on the irreversibly bonded self-polymerizing covalent organic framework material through an in-situ solvothermal reaction.
[0088] Wherein, the metal salt includes at least one of sodium chloropalladate, chloroauric acid, sodium chloroplatinate, ruthenium chloride, rhodium chloride, silver nitrate, and copper chloride; the solvent is at least one of water, acetonitrile, ethylene glycol, ethanol, methanol, or N-methylpyrrolidone; and the reducing agent includes any one of sodium citrate, sodium borohydride, or potassium borohydride.
[0089] The above-mentioned composite electrocatalyst prepared in the present application can be used for catalytic oxygen reaction, hydrogen evolution reaction, nitrogen reduction reaction, oxygen reduction reaction or electrocatalytic organic molecule synthesis, and is particularly suitable for electrocatalytic synthesis of ammonia, with high selectivity and high yield, and has high economic value.
[0090] The present application is specifically described below through examples.
[0091] Example 1
[0092] This embodiment provides a method for preparing a monomer, comprising:
[0093] Weigh 1 mmol of 4,8-dibromo-2,6-dimethyl[1,3]oxazacyclopenta[4',5':4,5]benzo[d][1,3]oxazacyclopenta[4',5':4,5]benzo[d][1,3]oxazacyclopenta[1,3], 3 mmol of 4-formylphenylboronic acid, 4 mmol of potassium carbonate, and 0.1 mmol of tetrakis(triphenylphosphine)palladium into a 100 mL Shrek bottle, then add 4 mL of water and 20 mL of tetrahydrofuran into the Shrek bottle, and react at 75°C for 24 hours under a nitrogen atmosphere. The reaction formula is as follows:
[0094]
[0095] After the reaction is completed, the filter residue is collected by suction filtration, washed with water and tetrahydrofuran respectively, and then placed in a vacuum oven and dried at 75°C for 12 hours to obtain the monomer 4-{2-[(1-nitrogenylideneethyl)oxy]-1-[(4E)-2-methyl-5H,4H-1,3-oxaazacyclopentyl-4-ylidene]ethyl}benzene-1-carboxaldehyde benzaldehyde, recorded as DMOD.
[0096] The results of its nuclear magnetic resonance test are:
[0097] 1 H NMR (400MHz, CDCl3): δ2.77(6H,s),8.10(4H,d),8.41(4H,d),10.13(2H,s).
[0098] Example 2
[0099] This embodiment provides a method for preparing a monomer, comprising:
[0100] Weigh 1 mmol of 4,8-dibromo-2,6-dimethyl[1,3]oxazacyclopenta[4',5':4,5]benzo[d][1,3]oxazacyclopenta[4',5':4,5]benzo[d][1,3]oxazacyclopenta[1,3], 3 mmol of 3-fluoro-4-formylphenylboronic acid, 4 mmol of potassium carbonate, and 0.1 mmol of tetrakis(triphenylphosphine)palladium into a 100 mL Shrek bottle, then add 4 mL of water and 20 mL of tetrahydrofuran into the Shrek bottle, and react at 75° C. for 24 hours under a nitrogen atmosphere. The reaction formula is as follows:
[0101]
[0102] After the reaction is completed, the filter residue is collected by suction filtration, washed with water and tetrahydrofuran respectively, and then placed in a vacuum oven and dried at 75°C for 12 hours to obtain the monomer 2-fluoro-4-[8-(3-fluoro-4-formylphenyl)-2,6-dimethyl[1,3]oxazacyclopentyl[4',5':4,5]benzo[d][1,3]oxazacyclopentyl-4-yl]benzene-1-carboxaldehyde, recorded as DMOD-2F.
[0103] The results of its nuclear magnetic resonance test are:
[0104] 1 H NMR (400MHz, CDCl3): δ2.81(6H,s),8.10(2H,t),8.24(4H,m),10.48(2H,s).
[0105] Example 3
[0106] This embodiment provides a method for preparing a monomer, comprising:
[0107] Weigh 1 mmol of 4,8-dibromo-2,6-dimethyl[1,3]oxazacyclopenta[4',5':4,5]benzo[d][1,3]oxazacyclopenta[4',5':4,5]benzo[d][1,3]oxazacyclopenta[1,3], 3 mmol of 3,5-difluoro-4-formylphenylboronic acid, 4 mmol of potassium carbonate, and 0.1 mmol of tetrakis(triphenylphosphine)palladium into a 100 mL Shrek bottle, then add 4 mL of water and 20 mL of tetrahydrofuran into the Shrek bottle, and react at 75° C. for 24 hours under a nitrogen atmosphere. The reaction formula is as follows:
[0108]
[0109] After the reaction is completed, the residue is collected by filtration, washed with water and tetrahydrofuran respectively, and then placed in a vacuum oven and dried at 75°C for 12 hours to obtain the monomer 4-[8-(3,5-difluoro-4-formylphenyl)-2,6-dimethyl[1,3]oxazacyclopentyl[4',5':4,5]benzo[d][1,3]oxazacyclopentyl-4-yl]-2,6-difluorobenzene-1-carbaldehyde, recorded as DMOD-4F.
[0110] The results of its nuclear magnetic resonance test are:
[0111] 1 H NMR (400MHz, CDCl3): δ2.82(6H,s),8.11(4H,d),10.44(2H,s).
[0112] Example 4
[0113] This embodiment provides a method for preparing a monomer, comprising:
[0114] Weigh 1 mmol of 6,7-dibromo-2,3-dimethylquinoxaline, 3 mmol of 4-formylphenylboronic acid, 4 mmol of potassium carbonate, and 0.1 mmol of tetrakis(triphenylphosphine)palladium into a 100 mL Shrek bottle, then add 4 mL of water and 20 mL of tetrahydrofuran into the Shrek bottle, and react at 75° C. for 24 hours under a nitrogen atmosphere. The reaction formula is as follows:
[0115]
[0116] After the reaction is completed, the filter residue is collected by suction filtration, washed with water and tetrahydrofuran respectively, and then placed in a vacuum oven and dried at 75° C. for 12 hours to obtain the monomer 4-[7-(4-formylphenyl)-2,3-dimethylquinoxaline-6-yl]benzene-1-carboxaldehyde.
[0117] The results of its nuclear magnetic resonance test are:
[0118] 1 H NMR (400MHz, CDCl3): δ2.83(6H,s),7.42(4H,d),7.85(4H,d),8.41(2H,s),10.18(2H,s).
[0119] Example 5
[0120] This embodiment provides a method for preparing a monomer, comprising:
[0121] Weigh 1 mmol of 3,6-dibromobenzene-1,2,4,5-tetracarboxylic acid, 3 mmol of N-(4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenyl)benzamide, 4 mmol of potassium carbonate, and 0.1 mmol of tetrakis(triphenylphosphine)palladium into a 100 mL Shrek bottle, then add 4 mL of water and 20 mL of tetrahydrofuran into the Shrek bottle, and react at 75° C. for 24 hours under a nitrogen atmosphere. The reaction formula is as follows:
[0122]
[0123] After the reaction is completed, the filter residue is collected by suction filtration, washed with water and tetrahydrofuran respectively, and then placed in a vacuum oven and dried at 75°C for 12 hours to obtain the monomer 4,4'-bis(benzamido)-[1,1':4',1'-triphenyl]-2',3',5',6'-tetracarboxylic acid, recorded as BZTTA.
[0124] The results of its nuclear magnetic resonance test are:
[0125] 1 H NMR (400MHz, DMSO): δ7.43-7.96(18H,m),10.2(2H,s),11.7(4H,s).
[0126] Example 6
[0127] This embodiment provides a method for preparing a monomer, comprising:
[0128] Weigh 1 mmol of 3,6-dibromobenzene-1,2,4,5-tetracarboxylic acid, 3 mmol of N-(2-fluoro-4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenyl)benzamide, 4 mmol of potassium carbonate, and 0.1 mmol of tetrakis(triphenylphosphine)palladium and add them into a 100 mL Shrek bottle, then add 4 mL of water and 20 mL of tetrahydrofuran into the Shrek bottle, and react at 75° C. for 24 hours under a nitrogen atmosphere. The reaction formula is as follows:
[0129]
[0130] After the reaction is completed, the filter residue is collected by suction filtration, washed with water and tetrahydrofuran respectively, and then placed in a vacuum oven and dried at 75°C for 12 hours to obtain the monomer 4,4'-bis(benzamido)-3,3'-difluoro-[1,1':4',1'-triphenyl]-2',3',5',6'-tetracarboxylic acid, which is recorded as BZTTA-2F.
[0131] The results of its nuclear magnetic resonance test are:
[0132] 1 H NMR (400MHz, DMSO): δ7.54-7.96(16H,m),10.3(2H,s),12.7(4H,s).
[0133] Example 7
[0134] This embodiment provides a method for preparing a monomer, comprising:
[0135] Weigh 1 mmol of 3,6-dibromobenzene-1,2,4,5-tetracarboxylic acid, 3 mmol of N-(2,6-difluoro-4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenyl)benzamide, 4 mmol of potassium carbonate, and 0.1 mmol of tetrakis(triphenylphosphine)palladium into a 100 mL Shrek bottle, then add 4 mL of water and 20 mL of tetrahydrofuran into the Shrek bottle, and react at 75° C. for 24 hours under a nitrogen atmosphere. The reaction formula is as follows:
[0136]
[0137] After the reaction is completed, the filter residue is collected by suction filtration, washed with water and tetrahydrofuran respectively, and then placed in a vacuum oven and dried at 75°C for 12 hours to obtain the monomer 4,4"-bis(benzamido)-3,3",5,5"-tetrafluoro-[1,1':4',1"-triphenyl]-2',3',5',6'-tetracarboxylic acid, recorded as BZTTA-4F.
[0138] The results of its nuclear magnetic resonance test are:
[0139] 1 H NMR (400MHz, DMSO): δ7.39-7.96(14H,m),10.4(2H,s),12.8(4H,s).
[0140] Example 8
[0141] This embodiment provides a method for preparing a monomer, comprising:
[0142] Weigh 1 mmol of 3,6-dibromobenzene-1,2,4,5-tetracarboxylic acid, 3 mmol of N-(4'-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)-[1,1'-biphenyl]-4-yl)benzamide, 4 mmol of potassium carbonate, and 0.1 mmol of tetrakis(triphenylphosphine)palladium into a 100 mL Shrek bottle, then add 4 mL of water and 20 mL of tetrahydrofuran into the Shrek bottle, and react at 75°C for 24 hours under a nitrogen atmosphere. The reaction formula is as follows:
[0143]
[0144] After the reaction is completed, the residue is collected by filtration, washed with water and tetrahydrofuran respectively, and then placed in a vacuum oven and dried at 75°C for 12 hours to obtain the monomer 4,4"-bis(benzamide)-[1,1",1":4",1""-quinolyl]-2",3",5',6"-tetracarboxylic acid, recorded as BZTTA-2Ph.
[0145] The results of its nuclear magnetic resonance test are:
[0146] 1 H NMR (400MHz, DMSO): δ7.25(8H,m)7.44-7.96(18H,m),10.2(2H,s),12.5(4H,s).
[0147] Example 9
[0148] This embodiment provides a method for preparing a self-polymerizing covalent organic framework material with irreversible bond connection under an aerobic environment, comprising:
[0149] Take 0.1mmol of the monomer DMOD prepared in Example 1 and 0.6mmol of benzoic acid, put them into a thick-walled glass tube resistant to high temperature and high pressure, and seal the glass tube with a hydrogen generator to form a sealed system. Put the sealed glass tube into a 250°C oven and react for 24 hours to obtain an orange block solid. After soaking it in DMF, extract it in methanol by Soxhlet for 4h to obtain an orange block of irreversibly bonded self-polymerized covalent organic framework material, recorded as DMOD-COF, with a yield of 96%.
[0150] The reaction formula is as follows:
[0151]
[0152] Example 10
[0153] This embodiment provides a method for preparing a self-polymerizing covalent organic framework material with irreversible bond connection in an oxygen-free environment. The difference between Example 10 and Example 9 is that after the raw materials are added to the thick-walled glass tube, the glass tube is evacuated to a pressure of ≤0.15 mmHg, and then the glass tube is sealed by a hydrogen generator to form a sealed system. The rest is the same as Example 9.
[0154] The yield of Example 10 was 98%.
[0155] Embodiment 11
[0156] This embodiment provides a method for preparing a self-polymerizing covalent organic framework material with irreversible bond connection in an oxygen-free environment. The difference between Example 11 and Example 10 is that the amount of the two raw materials is increased by 30 times, and the rest is the same as Example 10.
[0157] The yield of Example 11 was 98%.
[0158] Example 12
[0159] This embodiment provides a method for preparing a self-polymerizing covalent organic framework material with irreversible bond connection under an aerobic environment, comprising:
[0160] Take 0.1mmol of the monomer DMOD-2F prepared in Example 2 and 0.4mmol of benzoic anhydride, put them into a thick-walled glass tube resistant to high temperature and high pressure, and seal the glass tube with a hydrogen generator to form a sealed system. Put the sealed glass tube into a 250°C oven and react for 24 hours to obtain a red block solid. After soaking it in DMF, extract it in methanol by Soxhlet for 4h to obtain a red block of irreversibly bonded self-polymerized covalent organic framework material, recorded as DMOD-2F-COF, with a yield of 97%.
[0161] The reaction formula is as follows:
[0162]
[0163] Embodiment 13
[0164] This embodiment provides a method for preparing a self-polymerizing covalent organic framework material with irreversible bond connection under an aerobic environment, comprising:
[0165] Take 0.1mmol of the monomer DMOD-4F prepared in Example 3 and 0.4mmol of benzoic anhydride, put them into a thick-walled glass tube resistant to high temperature and pressure, and seal the glass tube with a hydrogen generator to form a sealed system. Put the sealed glass tube into a 250°C oven and react for 24 hours to obtain a reddish-brown block solid. After soaking it in DMF, extract it in methanol by Soxhlet for 4h to obtain an orange block of irreversibly bonded self-polymerized covalent organic framework material, recorded as DMOD-4F-COF, with a yield of 98%.
[0166] The reaction formula is as follows:
[0167]
[0168] Embodiment 14
[0169] This embodiment provides a method for preparing a self-polymerizing covalent organic framework material with irreversible bond connection under an aerobic environment, comprising:
[0170] Take 0.1mmol of 4-(4-{8-[4-(4-formylphenyl)phenyl]-2,6-dimethyl[1,3]oxazacyclopentyl[4',5':4,5]benzo[d][1,3]oxazacyclopentyl-4-yl}phenyl)benzene-1-carboxaldehyde and 0.4mmol of benzoic anhydride, put them into a thick-walled glass tube resistant to high temperature and pressure, and seal the glass tube with a hydrogen generator to form a sealed system. Put the sealed glass tube into a 250℃ oven and react for 24 hours to obtain a yellow block solid. After soaking it in DMF, Soxhlet extraction was performed in methanol for 4h to obtain an orange block of irreversibly bonded self-polymerized covalent organic framework material with a yield of 97%.
[0171] The reaction formula is as follows:
[0172]
[0173] Embodiment 15
[0174] This embodiment provides a method for preparing a self-polymerizing covalent organic framework material with irreversible bond connection in an oxygen-free environment, comprising:
[0175] Take 0.1mmol of the monomer BZTTA prepared in Example 5 and 0.4mmol of benzoic anhydride, put them into a thick-walled glass tube resistant to high temperature and high pressure, evacuate until the pressure in the glass tube is ≤0.15mmHg, and then seal the glass tube with a hydrogen generator to form a sealed system. The sealed glass tube is placed in a 250°C oven and reacted for 24 hours to obtain a light yellow block solid. After soaking it in DMF, it is extracted by Soxhlet in methanol for 4h to obtain a yellow block of irreversibly bonded self-polymerized covalent organic framework material, recorded as BZTTA-COF, with a yield of 92%.
[0176] The reaction formula is as follows:
[0177]
[0178] Example 16
[0179] This embodiment provides a method for preparing a self-polymerizing covalent organic framework material with irreversible bond connection in an oxygen-free environment.
[0180] Take 0.1mmol of the monomer BZTTA-2F prepared in Example 6 and 0.4mmol of benzoic anhydride, put them into a thick-walled glass tube resistant to high temperature and high pressure, evacuate until the pressure in the glass tube is ≤0.15mmHg, and then seal the glass tube with a hydrogen generator to form a sealed system. The sealed glass tube is placed in a 250°C oven and reacted for 24 hours to obtain a brown block solid. After soaking it in DMF, it is extracted by Soxhlet in methanol for 4h to obtain a brown block of irreversibly bonded self-polymerized covalent organic framework material, recorded as BZTTA-2F-COF, with a yield of 95%.
[0181] The reaction formula is as follows:
[0182]
[0183] Embodiment 17
[0184] This embodiment provides a method for preparing a self-polymerizing covalent organic framework material with irreversible bond connection in an oxygen-free environment.
[0185] Take 0.1mmol of the monomer BZTTA-4F prepared in Example 7 and 0.4mmol of benzoic anhydride, put them into a thick-walled glass tube resistant to high temperature and high pressure, evacuate until the pressure in the glass tube is ≤0.15mmHg, and then seal the glass tube with a hydrogen generator to form a sealed system. The sealed glass tube is placed in a 250°C oven and reacted for 24 hours to obtain an orange block solid. After soaking it in DMF, it is extracted in methanol by Soxhlet for 4h to obtain an orange block of irreversibly bonded self-polymerized covalent organic framework material, recorded as BZTTA-4F-COF, with a yield of 96%.
[0186] The reaction formula is as follows:
[0187]
[0188] Embodiment 18
[0189] This embodiment provides a method for preparing a self-polymerizing covalent organic framework material with irreversible bond connection in an oxygen-free environment.
[0190] Take 0.1mmol of the monomer BZTTA-2Ph prepared in Example 8 and 0.4mmol of benzoic anhydride, put them into a thick-walled glass tube resistant to high temperature and high pressure, evacuate to a pressure of ≤0.15mmHg in the glass tube, and then seal the glass tube with a hydrogen generator to form a sealed system. The sealed glass tube is placed in a 250°C oven and reacted for 24 hours to obtain a dark yellow block solid. After soaking it in DMF, it is extracted by Soxhlet in methanol for 4h to obtain a dark yellow block of irreversibly bonded self-polymerized covalent organic framework material, recorded as BZTTA-2Ph-COF, with a yield of 91%.
[0191] The reaction formula is as follows:
[0192]
[0193] Embodiment 19
[0194] This embodiment provides a method for preparing a composite electrocatalyst, comprising:
[0195] 20 mg of the DMOD-COF powder prepared in Example 9 was weighed and dispersed in 20 mL of ethylene glycol solution, and ultrasonicated for 30 minutes; 0.6 mL of 3.0 mg / mL sodium chloropalladate solution was then added dropwise to the solution, and 1 mL of 0.28 mg / mL sodium citrate solution was added dropwise after stirring for 2 hours, and heated to 120° C. under a nitrogen atmosphere for 1 hour to obtain an orange suspension. The suspension was centrifuged, the solid phase was separated, washed with water and ethanol in turn, and then dried in a vacuum oven at 50° C. to obtain an orange powdery composite electrocatalyst, recorded as Pd / DMOD-COF.
[0196] Embodiment 20
[0197] This embodiment provides a method for preparing a composite electrocatalyst, comprising:
[0198] Weigh 20 mg of the DMOD-4F-COF powder prepared in Example 9, disperse it in 20 mL of ethylene glycol solution, and ultrasonicate for 30 minutes; then add 0.6 mL of 3.0 mg / mL sodium chloropalladate solution to the solution, stir for 2 hours, then add 1 mL of 0.28 mg / mL sodium citrate solution dropwise, heat to 120°C in a nitrogen atmosphere for 1 hour to obtain an orange suspension. Centrifuge the suspension, separate the solid phase, wash with water and ethanol in turn, and then dry in a vacuum oven at 50°C to obtain an orange powdery composite electrocatalyst, recorded as Pd / DMOD-4F-COF.
[0199] Embodiment 21
[0200] This embodiment provides a method for preparing a composite electrocatalyst, comprising:
[0201] Weigh 20 mg of the DMOD-COF powder prepared in Example 9, disperse it in 20 mL of ethylene glycol solution, and ultrasonicate for 30 minutes; then drop 0.6 mL of 2.4 mg / mL chloroauric acid solution into the solution, stir for 2 hours, then dropwise add 1 mL of 0.35 mg / mL sodium citrate solution, heat to 120°C in a nitrogen atmosphere for 1 hour to obtain an orange suspension. Centrifuge the suspension, separate the solid phase, wash with water and ethanol in turn, and then dry in a vacuum oven at 50°C to obtain an orange powdery composite electrocatalyst, recorded as Au / DMOD-COF.
[0202] Embodiment 22
[0203] This embodiment provides a method for preparing a composite electrocatalyst, comprising:
[0204] Weigh 20 mg of the DMOD-COF powder prepared in Example 9, disperse it in 20 mL of ethylene glycol solution, and ultrasonicate for 30 minutes; then drop 0.04 mL of 4.8 mg / mL ruthenium trichloride solution into the solution, stir for 2 hours, then dropwise add 1 mL of 5 mg / mL sodium borohydride solution, heat to 50°C in a nitrogen atmosphere and react for 4 hours to obtain an orange suspension. Centrifuge the suspension, separate the solid phase, wash with water and ethanol in turn, and then dry in a vacuum oven at 50°C to obtain an orange powdery composite electrocatalyst, recorded as Ru / DMOD-COF.
[0205] The performance evaluation of the irreversibly bonded self-polymerizing covalent organic framework material (DMOD-COF) prepared in Example 9, the irreversibly bonded self-polymerizing covalent organic framework material prepared in Examples 10-11, and the irreversibly bonded self-polymerizing covalent organic framework material (BZTTA-COF) prepared in Example 15 was performed as follows:
[0206] 1. XRD test, its spectrum is as follows Figure 1 shown.
[0207] Figure 1 In the figure, (a), (b), (c) and (d) are the XRD spectra of the irreversibly bonded self-polymerized covalent organic framework materials prepared in Example 9, Example 10, Example 11 and Example 15, respectively. Figure 1 It can be seen that the above-mentioned self-polymerizing covalent organic framework materials connected by irreversible bonds all have high crystallinity.
[0208] 2. DMOD-COF prepared in Example 9 and BZTTA-COF prepared in Example 15 were subjected to infrared testing, and their spectra were as follows: Figure 2 shown.
[0209] in, Figure 2 (a) is the infrared test spectrum of DMOD-COF, which shows that DMOD-COF is a vinyl-linked COFs material, where 1631.5 cm -1 The peak at corresponds to the stretching vibration of the carbon-carbon double bond.
[0210] Figure 2 (b) is the infrared test spectrum of BZTTA-COF, which shows that BZTTA-COF is a polyimide-based COFs material, where 1375 cm -1 The peak at 40 corresponds to the stretching vibration of imide CNC.
[0211] 3.BET surface area test
[0212] The nitrogen isothermal adsorption-desorption curves of DMOD-COF and BZTTA-COF at 77K were tested respectively. Figure 3 As shown, (a) is the nitrogen isothermal adsorption-desorption curve of DMOD-COF, and (b) is the nitrogen isothermal adsorption-desorption curve of BZTTA-COF. Figure 3 The BET surface area of DMOD-COF can be calculated from the isothermal adsorption curve to be 929 m 2 / g, and the BET surface area of BZTTA-COF is 628m 2 / g, both have large specific surface area.
[0213] The composite catalyst Pd / DMOD-4F-COF prepared in Example 20 was used to electrocatalyze the synthesis of ammonia, and its electrocatalytic performance was evaluated. The electrocatalytic test was carried out on an electrochemical workstation using a three-electrode system, and the specific method was as follows:
[0214] Take 10 mg of powdered Pd / DMOD-4F-COF and put it in a mortar, add 3 mL of ethanol and 20 μL of Nafion ethanol solution, grind it evenly, then drop the slurry on hydrophobic carbon paper, and use it as the working electrode in the three-electrode system after drying. The counter electrode is a platinum electrode, the reference electrode is a silver-silver chloride electrode, and the electrolyte is a 0.1 M sodium sulfate aqueous solution.
[0215] Before the test, nitrogen was introduced into the three-electrode system for at least 1 hour, and then the electrostatic potential test was performed for 2 hours at different working voltages. Ammonia in the solution was detected in a UV-Vis spectrophotometer using a variety of color developers.
[0216] Ammonia yield and Faraday efficiency at different voltages Figure 4 As shown. Figure 4 It can be seen that Pd / DMOD-4F-COF has high ammonia yield and Faradaic efficiency at different voltages. The maximum ammonia yield of Pd / DMOD-4F-COF is 90±2.6 μg h at -0.2 V vs. RHE. -1 mg cat. -1 The maximum Faraday efficiency is 44%, which proves that the composite electrocatalyst of the present application has a high catalytic efficiency. The catalytic product is calibrated using different color developers, and the results obtained are basically consistent, which also proves that the composite electrocatalyst of the present application has a high catalytic efficiency.
[0217] The composite electrocatalyst of the present application was cycled to test its catalytic activity. The results are as follows: Figure 5 As shown. Figure 5 It can be seen that after 15 cycles of operation, the composite electrocatalyst still maintains good catalytic activity.
[0218] Although the present application has been described in detail in general terms and in specific embodiments in this specification, it is obvious to those skilled in the art that some modifications or improvements may be made to the present application. Therefore, these modifications or improvements made without departing from the spirit of the present application are within the scope of protection claimed in the present application.
Claims
1. A self-polymerizing covalent organic framework material connected by irreversible bonds, characterized in that: Prepared by synthesizing monomers having equal amounts of reactive functional groups by Suzuki coupling and then subjecting the monomers to self-polymerization; The monomer has an equal amount of aldehyde group and methyl group, or has an equal amount of phthalic acid group and amide group.
2. The method for preparing the self-polymerizing covalent organic framework material with irreversible bond connection according to claim 1, characterized in that: include: S1, organic matter A, organic matter B, potassium carbonate and catalyst A are subjected to solvent reaction in a reactor under a nitrogen atmosphere to obtain a monomer; S2, the monomer and the catalyst B are subjected to a melt condensation reaction in a reactor, and the product is cleaned and purified to obtain a self-polymerizing covalent organic framework material connected by irreversible bonds.
3. The preparation method according to claim 2, characterized in that: The organic compound A is an aromatic compound having multiple bromine or iodine functional groups; The organic substance B is an aromatic compound having a phenylethynyl group, a phenylboronic acid group or a phenylboronic acid pinacol ester group; The catalyst A is an organic complex of palladium; The solvent includes any one or a combination of water, tetrahydrofuran, 1,4-dioxane, N,N-dimethylformamide and toluene.
4. The preparation method according to claim 3, characterized in that: The organic matter A includes 4,8-dibromo-2,6-dimethyl[1,3]oxazacyclopenta[4',5':4,5]benzo[d][1,3]oxazacyclopenta, 1,3,5-tribromo-2,4,6-triiodobenzene, 6,7-dibromo-2,3-dimethylquinoxaline, 5,8-dibromo-2,3-dimethylquinoxaline, 1,2-dibromo-4,5-diiodobenzene, 1,3-dibromo-4,6-diiodobenzene, 1 , 4-dibromo-2,5-diiodobenzene, 4-bromo-2,6-dimethylpyridine, 4-bromo-6-methylpyridine-2-carboxaldehyde, 1,4-dibromobenzene, 1,3,5-tribromobenzene, 1,3,4,6-tetrabromo-2,5-dimethylbenzene, 2,7-dibromopyrene, 2,6-dibromonaphthalene, 2,6-dibromoanthracene, 3,6-dibromobenzene-1,2,4,5-tetracarboxylic acid or 3,6-diiodobenzene-1,2,4-5-tetracarboxylic acid; and / or: The organic matter B includes 4-formylphenylboronic acid, 3-fluoro-4-formylphenylboronic acid, 3,5-difluoro-4-formylphenylboronic acid, 4-formyl-3,5-dimethoxyphenylboronic acid, 2-methoxy-4-(4,4,5,5-tetramethylethyl-1,3,2-dioxaborolanol-2-yl)benzaldehyde, 4-boric acid pinacol ester-2-hydroxybenzaldehyde, 2-nitro-4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolanol-2-yl)benzaldehyde, 4'- Formylbiphenyl-4-boronic acid pinacol ester; 4-(4-formylphenyl)phenyl-2-boronic acid pinacol ester, 2-methyl-5-(4,4,5,5-tetramethyl-1,3,2-dioxaborol-2-yl)pyridine, 4-ethynylbenzene-1-carboxaldehyde, 5-(4,4,5,5-tetramethyl-1,3,2-dioxaborol-2-yl)benzene-1,3-dicarboxaldehyde, 1,4-phenyldiboronic acid pinacol ester, 4,4'-biphenyldiboronic acid pinacol ester, N-(4-( 4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenyl)benzamide, N-(2-fluoro-4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenyl)benzamide, N-(2,6-difluoro-4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenyl)benzamide, N-(2-hydroxy-4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenyl)benzamide any one of N-(4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenyl)benzamide, N-(4'-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)-[1,1'-biphenyl]-4-yl)benzamide or N-(4-(4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenyl)ethynyl)phenylbenzamide; and / or: The catalyst A includes any one of tetrakis(triphenylphosphine)palladium(0), bis(triphenylphosphine)palladium dichloride, 1,1-bis(diphenylphosphino)ferrocenepalladium dichloride or palladium acetate.
5. The preparation method according to claim 2, characterized in that: The monomer has equal amounts of aldehyde groups and methyl groups, or has equal amounts of phthalic acid groups and amide groups; The catalyst B is a compound containing anhydride functional groups, a compound containing acyl chloride functional groups or a compound containing carboxylic acid functional groups.
6. The preparation method according to claim 2, characterized in that: The molar ratio of the organic matter A, the organic matter B, potassium carbonate and the catalyst A is 1:(3-4):(3-4):(0.1-0.2); and / or: The molar ratio of the catalyst B to the monomer is 1:1-10:1; The temperature of the solvent reaction is 70-80°C; The temperature of the melt condensation reaction is 160-250°C.
7. Use of the irreversibly bonded self-polymerizing covalent organic framework material according to claim 1 or the irreversibly bonded self-polymerizing covalent organic framework material prepared by the preparation method according to any one of claims 2 to 6 in electrocatalysts.
8. A composite electrocatalyst, characterized in that: It includes an electrocatalyst and a carrier for supporting the electrocatalyst; The carrier is the irreversibly bonded self-polymerizing covalent organic framework material according to claim 1 or the irreversibly bonded self-polymerizing covalent organic framework material prepared by the preparation method according to any one of claims 2 to 6.
9. The method for preparing the composite electrocatalyst according to claim 8, characterized in that: include: The self-polymerizing covalent organic framework material connected by irreversible bonds is dispersed in a solvent, a metal salt solution is added, and the reaction is carried out in a nitrogen atmosphere under the action of a reducing agent, and the solid product is collected, washed and dried to obtain the product; The metal salt includes at least one of sodium chloropalladate, chloroauric acid, sodium chloroplatinate, ruthenium chloride, rhodium chloride, silver nitrate, and copper chloride; The solvent is at least one of water, acetonitrile, ethylene glycol, ethanol, methanol or N-methylpyrrolidone; The reducing agent includes any one of sodium citrate, sodium borohydride or potassium borohydride.
10. Use of the composite electrocatalyst according to claim 8 in electrocatalytic synthesis of ammonia.
Citation Information
Patent Citations
Covalent organic framework material Py-COF and preparation method thereof
CN110003026A
Green solid-phase synthesis method of covalent organic framework material
CN114773556A
Covalent organic framework material based on benzodifuran diketone as well as preparation method and application of covalent organic framework material
CN117384333A
COFs (Covalent Organic Frameworks) material for improving carrier separation efficiency as well as preparation method and application of COFs material
CN118027327A
Green synthesis method suitable for various types of covalent organic frameworks
CN118562081A
Cited By
COF nanosheet for enhancing flame retardant property of PVC (polyvinyl chloride) and PE (polyethylene) pipes as well as preparation method and application of COF nanosheet
CN120647959A
COF nanosheet for enhancing flame retardant performance of PVC and PE pipes, and preparation method and application thereof
CN120647959B