High-performance waterborne epoxy zinc-rich primer and preparation method thereof
By using modified zinc powder, aluminum powder and organic anticorrosion pigments in aqueous epoxy zinc-rich primer, combined with modified amine-based curing agents, the problem of insufficient adhesion and corrosion resistance of water-based epoxy zinc-rich primer is solved. It achieves high performance and low VOC emissions, meeting the requirements of environmental protection regulations.
Patent Information
- Application Number
- CN202411419792.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-12-03
AI Technical Summary
The existing water-based epoxy zinc-rich primer with low VOC emissions has shortcomings in adhesion and corrosion resistance, and it is difficult to meet increasingly stringent environmental regulations and performance requirements.
Using a high proportion of modified zinc powder and aluminum powder, the zinc powder is modified by silane coupling agent and combined with aqueous epoxy resin, combined with organic anticorrosion pigments and modified amine curing agents to form a high-performance aqueous epoxy zinc-rich bottom Paint, enhances the corrosion resistance and adhesion of the coating, uses water as a dispersion medium to reduce VOC emissions.
It significantly improves the corrosion resistance and corrosion resistance of water-based epoxy zinc-rich primer, provides dual corrosion protection mechanisms and conductivity, reduces environmental pollution, and meets the requirements of environmental protection regulations.
Smart Images

Figure CN119060612A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of paints, in particular to a high-performance water-based epoxy zinc-rich primer and a preparation method thereof. Background Art
[0002] While traditional solvent-based epoxy zinc-rich primers offer excellent corrosion resistance, they contain large amounts of organic solvents, which can cause significant environmental pollution. With growing environmental awareness, the development of non-toxic, low-VOC water-based epoxy zinc-rich primers is urgently needed. Existing low-VOC water-based epoxy zinc-rich primers often suffer from reduced energy consumption, resulting in poor adhesion and weak corrosion resistance. Summary of the Invention
[0003] The purpose of the present invention is to provide a high-performance water-based epoxy zinc-rich primer and a preparation method thereof, which solves the problems raised in the above-mentioned background technology.
[0004] To achieve the above-mentioned object, the present invention provides the following technical solution: a high-performance water-based epoxy zinc-rich primer, comprising component A and component B, wherein component A comprises the following raw materials in parts by weight: 30-50 parts of water-based epoxy resin, 40-70 parts of modified zinc powder, 0-10 parts of aluminum powder, 0-5 parts of organic anticorrosive pigment, 1-5 parts of dispersant, 0.5-2 parts of leveling agent and 0.1-1 parts of defoaming agent; the addition of aluminum powder can enhance the conductivity and ultraviolet reflection ability of the coating, while also providing an additional shielding effect; component B is 10-20 parts of modified amine curing agent, and the usage ratio of component A to component B is 3-5:1.
[0005] Preferably, the water-based epoxy resin is a 40% aqueous solution, where 40% water-based epoxy resin means that every 100 grams of resin contains 60 grams of water.
[0006] Preferably, the processing method of the modified zinc powder is as follows: dissolving 3% by weight of a silane coupling agent in isopropyl alcohol, adding zinc powder to the silane coupling agent solution, and dispersing it evenly using a high-speed disperser to ensure that the silane coupling agent is evenly coated on the surface of the zinc powder, and drying the treated zinc powder in an oven to remove the solvent and ensure the formation of a silane film. Modifying the zinc powder with a silane coupling agent can significantly improve the anti-corrosion performance of the zinc powder in a water-based epoxy zinc-rich primer, thereby improving the anti-corrosion effect and service life of the entire coating.
[0007] Preferably, the silane coupling agent is selected from one of aminosilane and epoxysilane, and the drying temperature is controlled at 80-120°C.
[0008] Preferably, the particle size of the zinc powder is 5-10 microns. Finer zinc powder particles are easier to disperse evenly in the coating, while coarser particles may require more powerful dispersing equipment to ensure their uniform distribution. Zinc powder with a narrower particle size distribution is selected to ensure the consistency and uniformity of the coating.
[0009] Preferably, the modified amine curing agent is specifically processed as follows: dissolving an appropriate amount of polyol in a solvent, slowly adding a certain amount of polyetheramine, and uniformly dispersing it under stirring conditions, adding an appropriate amount of catalyst to the mixture to promote the reaction between the amine and the polyol, heating the mixture at 60-80°C and maintaining it under stirring conditions for 3-5 hours until the reaction is complete. After the reaction is completed, the mixture is cooled to room temperature, and unreacted impurities are removed by filtration, and the pH value of the curing agent is adjusted.
[0010] Preferably, the material ratio of the modified amine curing agent is as follows: 50 parts of polyetheramine, 30 parts of polyol, 5 parts of catalyst and an appropriate amount of solvent.
[0011] Preferably, the dispersant is one of sodium polyacrylate and polyvinyl alcohol, which reduces the mutual attraction between particles and prevents particle agglomeration, thereby improving the uniformity and stability of the coating. The leveling agent is polydimethylsiloxane, which has excellent surface activity and can significantly reduce the surface tension of the coating. The defoaming agent is polydimethylsiloxane, which has a good defoaming effect.
[0012] Preferably, the organic anti-corrosion pigment is selected from at least one of zinc phosphate, tricalcium phosphate, thiosulfate, thiourea, benzotriazole and imidazolinone. The organic anti-corrosion pigment can form a thin film on the metal surface to prevent the corrosive medium from contacting the metal surface. The organic anti-corrosion pigment can release active substances such as phosphate ions and sulfides. These active substances can react with corrosion products on the metal surface to form a protective layer. The organic anti-corrosion pigment can promote the passivation of the metal surface to form a stable oxide or hydroxide protective layer.
[0013] Another technical problem to be solved by the present invention is to provide a method for preparing a high-performance waterborne epoxy zinc-rich primer, comprising the following steps:
[0014] Slowly add modified zinc powder and aluminum powder to the water-based epoxy resin, and disperse them evenly with a high-speed disperser. Add organic anti-corrosion pigment and continue to disperse them evenly at high speed. Add dispersant, leveling agent and defoaming agent in turn and continue stirring until completely mixed. Finally, add modified amine curing agent and stir evenly again. Adjust to the appropriate construction viscosity to obtain the finished product.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] The present invention proposes a high-performance water-based epoxy zinc-rich primer and a preparation method. The formula contains a high proportion of modified zinc powder. The modified zinc powder can provide cathodic protection in the coating, effectively preventing corrosion of the metal surface, which makes the primer have excellent anti-corrosion performance. The mixed use of modified aluminum powder and zinc powder provides a dual anti-corrosion mechanism. The modified zinc powder provides cathodic protection, while the aluminum powder enhances the conductivity and ultraviolet reflection ability of the coating. The addition of silane coupling agent and organic anti-corrosion pigment in the modified zinc powder can improve the adhesion and corrosion resistance of the coating. The use of water as a dispersion medium instead of traditional organic solvents greatly reduces VOC emissions and reduces environmental pollution, which is very important for meeting increasingly stringent environmental regulations. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a flow chart of the preparation process of the present invention. DETAILED DESCRIPTION
[0018] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.
[0019] Example 1:
[0020] In order to solve the problem that the existing low VOC emission waterborne epoxy zinc-rich primer often has a decline in new energy, resulting in poor adhesion and weak corrosion resistance of waterborne epoxy zinc-rich primer, please refer to Figure 1 , this embodiment provides the following technical solutions:
[0021] A high-performance waterborne epoxy zinc-rich primer comprises component A and component B. Component A comprises the following raw materials in parts by weight:
[0022] 40 parts of water-based epoxy resin;
[0023] 50 parts of modified zinc powder;
[0024] 5 parts of aluminum powder;
[0025] 3 parts of dispersant;
[0026] 1 part of leveling agent;
[0027] 0.5 parts of defoaming agent;
[0028] Component B is 15 parts of modified amine curing agent.
[0029] Preparation steps:
[0030] Slowly add modified zinc powder and aluminum powder to the water-based epoxy resin. The addition of aluminum powder can enhance the conductivity and ultraviolet reflection ability of the coating, and can also provide additional shielding effect. Disperse evenly with a high-speed disperser, add dispersant, leveling agent, and defoaming agent, continue stirring until completely mixed, add modified amine curing agent, stir evenly again, adjust the viscosity to a suitable construction state, and obtain the finished product.
[0031] Water-based epoxy resin is a 40% aqueous solution. 40% water-based epoxy resin means that every 100 grams of resin contains 60 grams of water. During the processing, no water needs to be added for adjustment. At the same time, the 40% water-based epoxy resin is mixed evenly before processing, which reduces the step of dissolving the water-based epoxy resin.
[0032] The processing method of modified zinc powder is as follows: dissolving 3% by weight of aminosilane in isopropyl alcohol, adding zinc powder to the silane coupling agent solution, and evenly dispersing it with a high-speed disperser to ensure that the silane coupling agent is evenly coated on the surface of the zinc powder. The treated zinc powder is dried in an oven at a drying temperature of 80-120°C to remove the solvent and ensure the formation of a silane film. Modifying the zinc powder with a silane coupling agent can significantly improve the anti-corrosion performance of the zinc powder in a water-based epoxy zinc-rich primer, thereby improving the anti-corrosion effect and service life of the entire coating. When the silane coupling agent comes into contact with the surface of the zinc powder, the silanol group forms a chemical bond with the hydroxyl group on the surface of the zinc powder. A silane film is formed on the surface of the zinc powder. The surface activity of the zinc powder treated with the silane coupling agent is enhanced, and it can better combine with organic materials such as epoxy resin. This enhanced binding force can improve the overall performance of the coating, including corrosion resistance and adhesion. The silane coupling agent can improve the dispersibility of the zinc powder in the coating, making it more evenly distributed in the coating and avoiding aggregation. The particle size of the zinc powder is selected to be 5-10 microns. Finer zinc powder particles are easier to disperse evenly in the coating, while coarser particles may require stronger dispersing equipment to ensure their uniform distribution. Select zinc powder with a narrower particle size distribution to ensure the consistency and uniformity of the coating.
[0033] The specific processing method of the modified amine curing agent is as follows: dissolve 30 parts of polyethylene glycol in an appropriate amount of water, slowly add 50 parts of polyetheramine, Jeffamine D-230 is selected as the polyetheramine, and uniformly disperse it under stirring conditions, add 5 parts of potassium acetate to the mixture, heat the mixture to 70°C, and maintain it under stirring conditions for 4 hours. After cooling to room temperature, filter to remove impurities, adjust the pH value to 6-8 as needed, and store in a sealed container.
[0034] The dispersant is sodium polyacrylate, which reduces the mutual attraction between particles and prevents particle agglomeration, thereby improving the uniformity and stability of the coating. The leveling agent is polydimethylsiloxane, which has excellent surface activity and can significantly reduce the surface tension of the coating. The defoaming agent is polydimethylsiloxane, which has a good defoaming effect.
[0035] Example 2:
[0036] A high-performance waterborne epoxy zinc-rich primer comprises component A and component B. Component A comprises the following raw materials in parts by weight:
[0037] 35 parts of water-based epoxy resin;
[0038] 60 parts of modified zinc powder;
[0039] 5 parts of aluminum powder;
[0040] 2 parts of dispersant;
[0041] 0.8 parts of leveling agent;
[0042] 0.2 parts of defoaming agent;
[0043] Component B is 18 parts of modified amine curing agent.
[0044] Preparation steps:
[0045] Slowly add modified zinc powder and aluminum powder to the water-based epoxy resin. The addition of aluminum powder can enhance the conductivity and ultraviolet reflection ability of the coating, and can also provide additional shielding effect. Disperse evenly with a high-speed disperser, add dispersant, leveling agent, and defoaming agent, continue stirring until completely mixed, add modified amine curing agent, stir evenly again, adjust the viscosity to a suitable construction state, and obtain the finished product.
[0046] Other materials and steps are the same as those in Example 1.
[0047] Example 3:
[0048] A high-performance waterborne epoxy zinc-rich primer comprises component A and component B. Component A comprises the following raw materials in parts by weight:
[0049] 45 parts of water-based epoxy resin;
[0050] 45 parts of modified zinc powder;
[0051] 5 parts of aluminum powder;
[0052] 2 parts of organic anticorrosive pigment;
[0053] 4 parts of dispersant;
[0054] 1.5 parts of leveling agent;
[0055] 0.7 parts of defoaming agent;
[0056] Component B is 12 parts of modified amine curing agent.
[0057] Preparation steps:
[0058] Slowly add modified zinc powder and aluminum powder to the water-based epoxy resin, and disperse them evenly with a high-speed disperser, add zinc phosphate anti-corrosion pigment, continue stirring to ensure that the zinc powder and zinc phosphate are fully mixed, add dispersant, leveling agent, and defoaming agent, continue stirring until completely mixed, add modified amine curing agent, stir evenly again, adjust the viscosity to a suitable construction state, and obtain the finished product. Organic anti-corrosion pigments can form a thin film on the metal surface to prevent the corrosive medium from contacting the metal surface. Organic anti-corrosion pigments can release active substances such as phosphate ions and sulfides. These active substances can react with corrosion products on the metal surface to form a protective layer. Organic anti-corrosion pigments can promote the passivation of the metal surface and form a stable oxide or hydroxide protective layer.
[0059] Other materials and steps are the same as those in Example 1.
[0060] Example 4:
[0061] A high-performance waterborne epoxy zinc-rich primer comprises component A and component B. Component A comprises the following raw materials in parts by weight:
[0062] 48 parts of water-based epoxy resin;
[0063] 50 parts of modified zinc powder;
[0064] 3 parts of organic anticorrosive pigment;
[0065] 4 parts of dispersant;
[0066] 1.5 parts of leveling agent;
[0067] 0.7 parts of defoaming agent;
[0068] Component B is 18 parts of modified amine curing agent.
[0069] Preparation steps:
[0070] Slowly add modified zinc powder to the water-based epoxy resin and disperse it evenly with a high-speed disperser. Add zinc phosphate anti-corrosion pigment and continue stirring to ensure that the zinc powder and zinc phosphate are fully mixed. Add dispersant, leveling agent, and defoaming agent and continue stirring until completely mixed. Add modified amine curing agent and stir evenly again. Adjust the viscosity to a suitable construction state to obtain the finished product.
[0071] Other materials and steps are the same as those in Example 1.
[0072] Example 5:
[0073] A high-performance waterborne epoxy zinc-rich primer comprises component A and component B. Component A comprises the following raw materials in parts by weight:
[0074] 48 parts of water-based epoxy resin;
[0075] 50 parts of modified zinc powder;
[0076] 4 parts of dispersant;
[0077] 1.5 parts of leveling agent;
[0078] 0.7 parts of defoaming agent;
[0079] Component B is 15 parts of modified amine curing agent.
[0080] Preparation steps:
[0081] Slowly add modified zinc powder to the water-based epoxy resin and disperse it evenly with a high-speed disperser. Add dispersant, leveling agent, and defoamer, continue stirring until completely mixed, add modified amine curing agent, stir evenly again, adjust the viscosity to a suitable construction state, and obtain the finished product.
[0082] Other materials and steps are the same as those in Example 1.
[0083] Comparative Example 1:
[0084] The water-based epoxy zinc-rich primer comprises component A and component B. Component A comprises the following raw materials in parts by weight:
[0085] 48 parts of water-based epoxy resin;
[0086] 50 parts of zinc powder;
[0087] 5 parts of aluminum powder;
[0088] 3 parts of organic anticorrosive pigment;
[0089] 4 parts of dispersant;
[0090] 1.5 parts of leveling agent;
[0091] 0.7 parts of defoaming agent;
[0092] Component B is 15 parts of modified amine curing agent.
[0093] Preparation steps:
[0094] Slowly add zinc powder to the water-based epoxy resin and disperse it evenly with a high-speed disperser. Add dispersant, leveling agent, and defoamer, continue stirring until completely mixed, add modified amine curing agent, stir evenly again, adjust the viscosity to a suitable construction state, and obtain the finished product.
[0095] The waterborne epoxy zinc-rich primer prepared by the above-mentioned examples and comparative examples was subjected to performance testing, and the following data were obtained:
[0096]
[0097]
[0098] It can be concluded from the above table that in Examples 1 to 3, the performance parameters obtained are basically the same when organic anti-corrosion pigments are added. However, after the organic anti-corrosion pigments are added in Example 4, the adhesion and corrosion resistance are improved. However, in Example 5, without adding aluminum powder, the adhesion and corrosion resistance are reduced, indicating that the organic anti-corrosion pigments and aluminum powder are added at the same time, which has a synergistic effect. In addition, in Comparative Example 1, ordinary zinc powder is used instead of modified zinc powder to prepare the water-based epoxy zinc-rich primer, but the adhesion and corrosion resistance are not as good as the water-based epoxy zinc-rich primer prepared in the examples, indicating that modified zinc powder can improve the adhesion and corrosion resistance of the water-based epoxy zinc-rich primer.
[0099] It should be noted that, in this document, relational terms such as first and second, etc., are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. Moreover, the terms "comprises," "comprising," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a list of elements includes not only those elements but also other elements not explicitly listed, or elements inherent to such process, method, article, or apparatus.
[0100] While the embodiments of the present invention have been shown and described, it will be apparent to those skilled in the art that various changes, modifications, substitutions, and alterations can be made to the embodiments without departing from the principles and spirit of the invention.
Claims
1. A high-performance waterborne epoxy zinc-rich primer, comprising component A and component B, characterized in that: The component A comprises the following raw materials in parts by weight: 30-50 parts of waterborne epoxy resin, 40-70 parts of modified zinc powder, 0-10 parts of aluminum powder, 0-5 parts of organic anticorrosive pigment, 1-5 parts of dispersant, 0.5-2 parts of leveling agent and 0.1-1 parts of defoaming agent; the component B is 10-20 parts of modified amine curing agent; and the usage ratio of component A to component B is 3-5:
1.
2. The high performance waterborne epoxy zinc-rich primer according to claim 1, characterized in that: The water-based epoxy resin is a 40% aqueous solution.
3. The high performance waterborne epoxy zinc-rich primer according to claim 1, characterized in that: The processing method of the modified zinc powder is as follows: dissolving 3% by weight of a silane coupling agent in isopropanol, adding zinc powder to the silane coupling agent solution, and dispersing it evenly with a high-speed disperser to ensure that the silane coupling agent is evenly coated on the surface of the zinc powder, and drying the treated zinc powder in an oven to remove the solvent and ensure the formation of a silane film.
4. The high performance waterborne epoxy zinc-rich primer according to claim 3, characterized in that: The silane coupling agent is selected from one of aminosilane and epoxysilane, and the drying temperature is controlled at 80-120°C.
5. The high performance waterborne epoxy zinc-rich primer according to claim 4, characterized in that: The particle size of the zinc powder is selected to be 5-10 microns.
6. The high performance waterborne epoxy zinc-rich primer according to claim 1, characterized in that: The specific processing method of the modified amine curing agent is as follows: dissolving an appropriate amount of polyol in a solvent, slowly adding a certain amount of polyetheramine, and uniformly dispersing it under stirring conditions, adding an appropriate amount of catalyst to the mixture, heating the mixture to 60-80° C., and maintaining it for 3-5 hours under stirring conditions until the reaction is complete. After the reaction is completed, the mixture is cooled to room temperature, and unreacted impurities are removed by filtering, and the pH value of the curing agent is adjusted.
7. The high performance waterborne epoxy zinc-rich primer according to claim 6, characterized in that: The material ratio of the modified amine curing agent is as follows: 50 parts of polyetheramine, 30 parts of polyol, 5 parts of catalyst and an appropriate amount of solvent.
8. The high performance waterborne epoxy zinc-rich primer according to claim 1, characterized in that: The dispersant is one of sodium polyacrylate and polyvinyl alcohol, the leveling agent is polydimethylsiloxane, and the defoaming agent is polydimethylsiloxane.
9. The high performance waterborne epoxy zinc-rich primer according to claim 8, characterized in that: The organic anticorrosive pigment is selected from at least one of zinc phosphate, tricalcium phosphate, thiosulfate, thiourea, benzotriazole and imidazolinone.
10. A method for preparing a high-performance waterborne epoxy zinc-rich primer as claimed in claim 9, characterized in that: The following steps are involved: Slowly add modified zinc powder and aluminum powder to the water-based epoxy resin, and disperse them evenly with a high-speed disperser. Add organic anti-corrosion pigments and continue to disperse them evenly at high speed. Add dispersant, leveling agent and defoaming agent in turn and continue stirring until completely mixed. Finally, add modified amine curing agent and stir evenly again. Adjust to a suitable construction viscosity to obtain the finished product.
Citation Information
Patent Citations
Double-anticorrosion paint for steel and preparing method thereof
CN101104764A
Bi-component waterborne epoxy zinc-rich primer and preparation method thereof
CN107418369A
Cited By
Corrosion-resistant coating for metal surface and preparation method of corrosion-resistant coating
CN119775814A
Environment-friendly paint and production process thereof
CN120329833A
High-performance formula and preparation method of wax sealing primer for pencils
CN121450214A
Pencil sealing wax primer high-performance formula and preparation method
CN121450214B
Special-shaped zinc powder for waterborne epoxy anticorrosive primer as well as preparation method and application of special-shaped zinc powder
CN121673860A