Amino acid metal surface corrosion inhibitor material, effect verification method and application

By developing amino acid metal surface corrosion inhibitor materials, a protective film is formed to block the contact between NTO and the metal surface, the problem of NTO corrosion on metal shells is solved, and efficient corrosion protection and industrial application are achieved.

CN119080672APending Publication Date: 2024-12-06BEIJING INST OF TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411032650.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art is difficult to effectively prevent NTO from corrosion on metal shells, and the lack of special corrosion inhibitor materials and verification methods for preventing corrosion of NTO materials, limiting its industrial application.

Method used

Developed amino acid metal surface corrosion inhibitor materials, such as N-[(phenylamino)thiooxymethyl]-tryptophan and N2-[(phenylamino)thiooxymethyl]-arginine corrosion inhibitors , a protective film is formed to block contact between NTO and the metal surface and a verification method is provided to quantify its corrosion inhibitory effect.

Benefits of technology

These corrosion inhibitor materials can effectively reduce the corrosion reaction of NTO to carbon steel, form a stable and dense protective layer, slow down the corrosion rate, and provide efficient corrosion protection without reducing the energy level of NTO to support its industrial application .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080672A_ABST
    Figure CN119080672A_ABST
Patent Text Reader

Abstract

The invention provides an amino acid type metal surface corrosion inhibitor material, an effect verification method and application, and the amino acid type metal surface corrosion inhibitor material is obtained by adding a certain amount of L-tryptophan and phenyl isothiocyanate into a reaction container, adding a solvent, and stirring and reacting at a certain reaction temperature. The amino acid metal surface corrosion inhibitor material provided by the invention can prevent NTO and other corrosion media from being in direct contact with the surface of carbon steel, corrosion reaction is reduced, the metal corrosion inhibition effect is good, and the anti-corrosion requirement of a metal shell for an NTO-based high-energy-density material can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of metal corrosion prevention and control, and relates to amino acid metal surface corrosion inhibitor materials, effect verification methods and applications. Background Art

[0002] NTO is a powerful explosive compound. Due to its excellent stability, it is particularly suitable for use in complex external environments, such as as a supporting equipment material for shipborne and vehicle-borne systems. However, NTO has the characteristics of hygroscopicity and acidity. It easily absorbs moisture from the air to form a local acidic solution, which causes corrosion of the encapsulated metal shell. This poses a challenge to the long-term storage of weapons and equipment containing NTO. Therefore, the practical problem that needs to be solved urgently is how to prevent NTO from corroding the metal shell while maintaining its explosive power.

[0003] However, the prior art tends to produce and prepare different types of corrosion inhibitor materials to solve the problem of metal material corrosion prevention and control. The corresponding corrosion inhibitor materials have been applied to biomedicine, chemical machinery, food containers, petrochemical and other industries, but there are few corrosion inhibitor materials specifically used to prevent NTO materials from corroding metal shells. Considering the dangerousness of NTO materials, the research and development and production needs of metal shell anti-corrosion technology used in conjunction with them are more urgent. At the same time, the technology of using amino acid materials as original reaction materials has not yet been applied, and its preparation conditions often have many restrictions. In addition, the prior art still lacks standardized means to verify the corrosion inhibition effect of related amino acid organic corrosion inhibitors, making it impossible to quantitatively verify the slow-release effect of the product, which also hinders the industrial application of related materials. Summary of the invention

[0004] In view of this, the present invention provides amino acid metal surface corrosion inhibitor materials, effect verification methods and applications, specifically including N-[(phenylamino)sulfurylmethyl]-tryptophan corrosion inhibitor and / or N2-[(phenylamino)sulfurylmethyl]-arginine corrosion inhibitor. This type of corrosion inhibitor material can form a protective film on the metal surface. The formation of this film involves physical or chemical adsorption of functional groups in organic molecules on the metal surface. It has a dense structure and can block direct contact between NTO and other corrosive media and the carbon steel surface, thereby reducing the progress of corrosion reactions. The present invention also provides an effect verification method for the prepared corresponding amino acid metal surface corrosion inhibitor material. The relevant verification method has simple steps and is easy to implement, laying a foundation for the industrial application of relevant corrosion inhibitors.

[0005] In order to achieve the above effects, the first aspect of the present invention provides an amino acid metal surface corrosion inhibitor material, which is obtained by adding a certain amount of L-tryptophan and phenyl isothiocyanate into a reaction container, adding a solvent, and stirring the reaction at a certain reaction temperature, and its specific structure is as follows:

[0006]

[0007] Optionally, the step of adding a certain amount of L-tryptophan and phenyl isothiocyanate into a reaction container, adding a solvent, and stirring the reaction at a certain reaction temperature specifically includes: the amount of L-tryptophan is 1-5 mmol, the amount of phenyl isothiocyanate is 1-5 mmol; the solvent is 50-100 mL of tetrahydrofuran; the reaction temperature is 80-90° C., and the stirring time is 7-9 h.

[0008] Preferably, the amount of L-tryptophan is 4.9 mmol, the amount of phenyl isothiocyanate is 4.9 mmol; the solvent is 85 mL of tetrahydrofuran; the reaction temperature is 85° C., and the stirring time is 8 h.

[0009] The second aspect of the present invention provides another amino acid metal surface corrosion inhibitor material, which is obtained by adding a certain amount of L-arginine and phenyl isothiocyanate into a reaction container, adding a solvent, and stirring the reaction at a certain reaction temperature, and its specific structure is as follows:

[0010]

[0011] Optionally, the step of adding a certain amount of L-arginine and phenyl isothiocyanate into a reaction container, adding a solvent, and stirring the reaction at a certain reaction temperature specifically includes: the amount of L-arginine is 5.5-8 mmol, the amount of phenyl isothiocyanate is 5.5-8 mmol; the solvent is 50-100 mL of ethanol and 5-15 mL of double distilled water; the reaction temperature is 50-70°C, and the stirring time is 4-6 h.

[0012] Preferably, the amount of L-tryptophan is 5.74 mmol, the amount of phenyl isothiocyanate is 5.74 mmol; the solvent is 75 mL of ethanol and 10 mL of double distilled water; the reaction temperature is 60° C., and the stirring time is 5 h.

[0013] A third aspect of the present invention provides an application of an amino acid metal surface corrosion inhibitor material in the field of metal corrosion prevention and control technology.

[0014] Optionally, the amino acid metal surface corrosion inhibitor material forms a protective film on the metal surface, thereby blocking direct contact between NTO or other corrosive media and the metal surface, thereby achieving corrosion inhibition of the metal material.

[0015] The fourth aspect of the present invention provides a method for verifying the effect of an amino acid-based metal surface corrosion inhibitor material, which is used to verify the corrosion inhibition effect of the amino acid-based metal surface corrosion inhibitor material, and is characterized in that it includes the following specific steps: S1: adding the amino acid-based metal surface corrosion inhibitor material to a saturated NTO solution; S2: soaking carbon steel in the saturated NTO solution to which the amino acid-based metal surface corrosion inhibitor material is added as described in S1, and calculating the corrosion rate of the carbon steel; S3: setting a comparative example, and performing parameter comparison between the corrosion rate calculated in S2 and the comparative example to verify the corrosion inhibition effect of the amino acid-based metal surface corrosion inhibitor material.

[0016] Optionally, S3 specifically includes: the comparative example is set to directly immerse carbon steel in a saturated NTO solution to which the amino acid-based metal surface corrosion inhibitor material is not added, and test the corrosion rate.

[0017] The present invention has at least the following beneficial effects:

[0018] (1) Amino acid-based metal surface corrosion inhibitor materials N2-[(phenylamino)sulfoxymethyl]-arginine molecules contain sulfoxymethyl functional groups, which can chemically adsorb to the metal surface to form a dense protective film. At the same time, the arginine group in the arginine molecule may form coordination bonds or hydrogen bonds with the metal surface, enhancing the adhesion of the film, thereby forming a stable and indestructible protective layer. This film can block the entry of corrosive media such as NTO and water molecules, slowing down the corrosion reaction. N2-[(phenylamino)sulfoxymethyl]-arginine can also synergistically adsorb with NTO molecules on the carbon steel surface, strengthening the adsorption capacity of the main body on the carbon steel surface, while weakening the adsorption and dissociation of NTO molecules on the metal (such as carbon steel) surface, further hindering the corrosion caused by the reaction of NTO molecules on the carbon steel surface. Therefore, N2-[(phenylamino)sulfoxymethyl]-arginine corrosion inhibitor has potential application prospects in the field of NTO corrosion protection.

[0019] (2) Amino acid-based metal surface corrosion inhibitor material N-[(phenylamino)sulfoxymethyl]tryptophan can form a protective film on the metal surface. The formation of this film involves physical or chemical adsorption of functional groups in organic molecules on the metal surface. This film has a dense structure that can block direct contact between NTO and other corrosive media and the carbon steel surface, reducing the progress of corrosion reactions. N-[(phenylamino)sulfoxymethyl]tryptophan may react chemically with NTO to form products with lower corrosiveness. This chemical reaction may include complexation reactions, redox reactions, etc., thereby reducing the corrosiveness of NTO to carbon steel. This reaction can not only slow down the progress of corrosion reactions, but also generate some stable compounds, further improving the corrosion resistance of metals (such as carbon steel). Therefore, N-[(phenylamino)sulfoxymethyl]tryptophan corrosion inhibitor has potential application prospects in the field of NTO corrosion protection.

[0020] In addition, additional advantages, objects, and features of the present invention will be described in part in the following description, and will become apparent to those skilled in the art after studying the following, or may be learned from the practice of the present invention. The objects and other advantages of the present invention may be realized and obtained by the structures and method steps specifically pointed out in the written description and claims and the accompanying drawings.

[0021] Those skilled in the art will appreciate that the objectives and advantages that can be achieved with the present invention are not limited to the above specific description, and the above and other objectives that can be achieved by the present invention will be more clearly understood from the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The drawings described herein are used to provide a further understanding of the present invention, constitute a part of this application, and do not constitute a limitation of the present invention.

[0023] Figure 1 is the H NMR spectrum of N-[(phenylamino)thioxomethyl]tryptophan in Example 3 of the present invention;

[0024] Figure 2 is the infrared spectrum of N-[(phenylamino)thioxomethyl]tryptophan in Example 3 of the present invention;

[0025] Figure 3 is the photoelectron spectrum of N-[(phenylamino)thioxomethyl]tryptophan in Example 3 of the present invention;

[0026] Figure 4 Thermogravimetric analysis of N-[(phenylamino)thioxomethyl]tryptophan in Example 3 of the present invention;

[0027] Figure 5The molecular structure, frontier orbital and electrostatic potential diagram of N-[(phenylamino)sulfoxymethyl]tryptophan in Example 3 of the present invention;

[0028] Figure 6 This is a graph showing the corrosion rate of carbon steel in a saturated NTO solution to which N-[(phenylamino)thioxomethyl]tryptophan is added in Examples 1-4 of the present invention;

[0029] Figure 7 This is the H NMR spectrum of the N2-[(phenylamino)sulfoxymethyl]-arginine corrosion inhibitor in Example 6 of the present invention;

[0030] Figure 8 is the infrared spectrum of the N2-[(phenylamino)sulfoxymethyl]-arginine corrosion inhibitor in Example 6 of the present invention;

[0031] Fig. 9 This is the photoelectron spectrum of the N2-[(phenylamino)sulfoxymethyl]-arginine corrosion inhibitor in Example 6 of the present invention;

[0032] Fig.10 This is the thermogravimetric analysis of the N2-[(phenylamino)sulfoxymethyl]-arginine corrosion inhibitor in Example 6 of the present invention;

[0033] Fig.11 The molecular structure, frontier orbital and electrostatic potential diagram of the N2-[(phenylamino)sulfoxymethyl]-arginine corrosion inhibitor in Example 6 of the present invention;

[0034] Fig.12 This is a graph showing the corrosion rate of carbon steel in a saturated NTO solution to which N2-[(phenylamino)sulfoxymethyl]-arginine corrosion inhibitor is added in Examples 5-8 of the present invention;

[0035] Fig.13 It is a schematic flow chart of a method for verifying the effect of an amino acid-based metal surface corrosion inhibitor material according to an embodiment of the present invention. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments and the accompanying drawings. The schematic embodiments of the present invention and their descriptions are used to explain the present invention, but are not intended to limit the present invention. It should also be noted that, in order to avoid blurring the present invention due to unnecessary details, only structures and / or processing steps closely related to the solutions according to the present invention are shown in the accompanying drawings, while other details that are not closely related to the present invention are omitted.

[0037] It should be emphasized that the term “include / comprises” when used herein refers to the presence of features, elements, steps or components, but does not exclude the presence or addition of one or more other features, elements, steps or components.

[0038] The first aspect of the embodiment of the present invention provides an amino acid metal surface corrosion inhibitor material, which is obtained by adding a certain amount of L-tryptophan and phenyl isothiocyanate into a reaction container, adding a solvent, and stirring the reaction at a certain reaction temperature, and the specific structure thereof is as follows:

[0039]

[0040] Optionally, a certain amount of L-tryptophan and phenyl isothiocyanate are added to a reaction vessel, and a solvent is added, and the reaction is stirred at a certain reaction temperature. Specifically, the amount of L-tryptophan is 1-5mmol, the amount of phenyl isothiocyanate is 1-5mmol; the solvent is 50-100mL of tetrahydrofuran; the reaction temperature is 80-90°C, and the stirring time is 7-9h. Further, in the process of achieving the corrosion inhibition effect, the product can form a protective film on the metal surface, and the formation of this film involves physical or chemical adsorption of functional groups in organic molecules on the metal surface. At the same time, the product may also react chemically with NTO to form a product with lower corrosiveness. Specifically, the chemical reaction may include complexation reaction, redox reaction, etc., thereby reducing the corrosiveness of NTO to carbon steel, and the additional generated compounds are stable in nature, which can further improve the corrosion resistance of metal surfaces such as carbon steel.

[0041] Preferably, the amount of L-tryptophan is 4.9 mmol, the amount of phenyl isothiocyanate is 4.9 mmol; the solvent is 85 mL of tetrahydrofuran; the reaction temperature is 85° C., and the stirring time is 8 h.

[0042] The second aspect of the embodiment of the present invention provides another amino acid metal surface corrosion inhibitor material, which is obtained by adding a certain amount of L-arginine and phenyl isothiocyanate into a reaction container, adding a solvent, and stirring the reaction at a certain reaction temperature, and the specific structure is as follows:

[0043]

[0044] Optionally, a certain amount of L-arginine and phenyl isothiocyanate are added to a reaction vessel, and a solvent is added, and the reaction is stirred at a certain reaction temperature. Specifically, the amount of L-arginine is 5.5-8mmol, and the amount of phenyl isothiocyanate is 5.5-8mmol; the solvent is 50-100mL ethanol and 5-15mL double distilled water; the reaction temperature is 50-70°C, and the stirring time is 4-6h. In the process of achieving the corrosion inhibition effect, the arginine group in the product may form a coordination bond or hydrogen bond with the metal surface, enhancing the adhesion of the film, thereby forming a stable and non-destructive protective layer, which has potential application prospects in the field of NTO corrosion protection. Further, the raw materials L-tryptophan and L-arginine used in the present invention can be one or more finished materials used for industrial mass production and addition. The special functional groups in the molecular structure of phenyl isothiocyanate (PITC) give it a variety of reaction capabilities. For example, it can specifically undergo a nucleophilic substitution reaction with a nucleophilic reagent, and then various target organic compounds with characteristic functions can be obtained by adjusting specific reactants and reaction conditions. At the same time, the materials in the present invention are all selected from conventional industrial product materials, which is conducive to the batch preparation of the final product of the present invention and maintains the balanced and stable quality of the final product.

[0045] Preferably, the amount of L-tryptophan is 5.74 mmol, the amount of phenyl isothiocyanate is 5.74 mmol; the solvent is 75 mL of ethanol and 10 mL of double distilled water; the reaction temperature is 60° C., and the stirring time is 5 h.

[0046] A third aspect of an embodiment of the present invention provides an application of an amino acid-based metal surface corrosion inhibitor material in the field of metal corrosion prevention and control technology.

[0047] Optionally, the amino acid metal surface corrosion inhibitor material forms a protective film on the metal surface, thereby blocking direct contact between NTO or other corrosive media and the metal surface, thereby achieving corrosion inhibition of the metal material.

[0048] The fourth aspect of the embodiments of the present invention provides a method for verifying the effect of an amino acid metal surface corrosion inhibitor material, which is used to verify the corrosion inhibition effect of the amino acid metal surface corrosion inhibitor material, and is characterized in that it includes the following specific steps: S1: adding the amino acid metal surface corrosion inhibitor material to a saturated NTO solution; S2: soaking carbon steel in the NTO saturated solution of S1 to which the amino acid metal surface corrosion inhibitor material is added, and calculating the corrosion rate of the carbon steel; S3: setting a comparative example, and performing parameter comparison between the corrosion rate calculated in S2 and the comparative example to verify the corrosion inhibition effect of the amino acid metal surface corrosion inhibitor material.

[0049] Optionally, S3 specifically includes: a comparative example is set to directly immerse carbon steel in a saturated NTO solution without adding an amino acid-based metal surface corrosion inhibitor material, and test the corrosion rate.

[0050] The present invention is further described in detail below through specific examples. The following examples are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.

[0051] Example 1

[0052] 1mmol of L-tryptophan and 1mmol of phenyl isothiocyanate were added to a 150mL conical flask. Subsequently, 50mL of tetrahydrofuran was added to the conical flask. Later, the mixture was stirred at 80°C for 7h. After the reaction was monitored by thin layer chromatography, the mother liquor was concentrated by cooling at 12°C / h, and then separated by column chromatography, and purified from PE:EA to EA. The obtained solid was vacuum dried at 60°C for 35h and then collected to obtain a tryptophan organic corrosion inhibitor. Finally, the collected tryptophan organic corrosion inhibitor was added to a saturated solution of NTO, and the mass loss of carbon steel immersed in this solution was taken to calculate the corrosion rate to verify the effect of this tryptophan organic corrosion inhibitor.

[0053] Example 2

[0054] 3mmol of L-tryptophan and 3mmol of phenyl isothiocyanate were added to a 150mL conical flask. Subsequently, 70mL of tetrahydrofuran was added to the conical flask. Later, the mixture was stirred at 82°C for 7.5h. After the reaction was monitored by thin layer chromatography, the mother liquor was concentrated by cooling at 18°C / h, and then separated by column chromatography, and purified from PE:EA to EA. The obtained solid was vacuum dried at 60°C for 38h and then collected to obtain a tryptophan organic corrosion inhibitor. Finally, the collected tryptophan organic corrosion inhibitor was added to a saturated NTO solution, and the mass loss of carbon steel immersed in this solution was taken to calculate the corrosion rate to verify the effect of this tryptophan organic corrosion inhibitor.

[0055] Example 3

[0056] 4.9mmol of L-tryptophan and 4.9mmol of phenyl isothiocyanate were added to a 150mL conical flask. Subsequently, 85mL of tetrahydrofuran was added to the conical flask. Later, the mixture was stirred at 85°C for 8h. After the reaction was monitored by thin layer chromatography, the mother liquor was concentrated by cooling at 15°C / h, and then separated by column chromatography, and purified from PE:EA to EA. The obtained solid was vacuum dried at 60°C for 40h and then collected to obtain a tryptophan organic corrosion inhibitor. Finally, the collected tryptophan organic corrosion inhibitor was added to a saturated solution of NTO, and the mass loss of carbon steel immersed in this solution was taken to calculate the corrosion rate to verify the effect of this tryptophan organic corrosion inhibitor.

[0057] Example 4

[0058] 5mmol of L-tryptophan and 5mmol of phenyl isothiocyanate were added to a 150mL conical flask. Subsequently, 100mL of tetrahydrofuran was added to the conical flask. Later, the mixture was stirred at 90°C for 9h. After the reaction was monitored by thin layer chromatography, the mother liquor was concentrated by cooling at 20°C / h, and then separated by column chromatography, and purified from PE:EA to EA. The obtained solid was vacuum dried at 60°C for 45h and then collected to obtain a tryptophan organic corrosion inhibitor. Finally, the collected tryptophan organic corrosion inhibitor was added to a saturated solution of NTO, and the mass loss of carbon steel immersed in this solution was taken to calculate the corrosion rate to verify the effect of this tryptophan organic corrosion inhibitor.

[0059] Comparative Example 1

[0060] The corrosion rate of carbon steel was tested by immersing it directly in a saturated NTO solution without adding N-[(phenylamino)sulfoxymethyl]tryptophan corrosion inhibitor.

[0061] Table 1. Corrosion inhibition performance of N-[(phenylamino)thioxomethyl]tryptophan inhibitor on NTO

[0062] Group Corrosion rate (mm / y) Comparative Example 1 9.03 Example 1 7.65 Example 2 5.93 Example 3 5.48 Example 4 5.87

[0063] from Figure 6It can be seen that the corrosion of carbon steel by the saturated solution of NTO after adding the organic matter N-[(phenylamino) sulfoxymethyl] tryptophan is significantly slowed down, and its corrosion rate is 5.48mm / y, which shows that the corrosion of NTO to low carbon steel is effectively controlled by N-[(phenylamino) sulfoxymethyl] tryptophan. This is due to the fact that N-[(phenylamino) sulfoxymethyl] tryptophan can form a protective film on the metal surface. The formation of this film involves the physical or chemical adsorption of functional groups in organic molecules on the metal surface. This film has a dense structure, which can block the direct contact between NTO and other corrosive media and the carbon steel surface, and reduce the progress of corrosion reactions. In addition, N-[(phenylamino) sulfoxymethyl] tryptophan may react chemically with NTO to form products with lower corrosiveness. This chemical reaction may include complexation reaction, redox reaction, etc., thereby reducing the corrosiveness of NTO to carbon steel. This reaction can not only slow down the progress of corrosion reaction, but also generate some stable compounds, further improving the corrosion resistance of carbon steel.

[0064] Example 5

[0065] 5.5 mmol of L-arginine and 5.5 mmol of phenyl isothiocyanate were added to a 250 mL round-bottom flask, and then 50 mL of ethanol and 7 mL of distilled water were added to the flask and placed in an oil bath at 50 ° C for 4 hours. The reaction was monitored by thin layer chromatography and cooled at 2 ° C / min. The obtained solid was filtered and washed with ethanol. Subsequently, the obtained solid was vacuum freeze-dried at 50 ° C for 48 hours and then collected to obtain an arginine organic corrosion inhibitor. Finally, the collected arginine organic corrosion inhibitor was added to a saturated NTO solution, and the mass loss of carbon steel immersed in this solution was taken to calculate the corrosion rate to verify the effect of this arginine organic corrosion inhibitor.

[0066] Example 6

[0067] 5.74mmol of L-arginine and 5.74mmol of phenyl isothiocyanate were added to a 250mL round-bottom flask, and then 75mL of ethanol and 10mL of distilled water were added to the flask and placed in an oil bath at 60°C for 5h. The reaction was monitored by thin layer chromatography and then cooled at 5°C / min. The obtained solid was filtered and washed with ethyl acetate. Subsequently, the obtained solid was collected after vacuum freeze drying at 50°C for 60h to obtain an arginine organic corrosion inhibitor. Finally, the collected arginine organic corrosion inhibitor was added to a saturated NTO solution, and the mass loss of carbon steel immersed in this solution was taken to calculate the corrosion rate to verify the effect of this arginine organic corrosion inhibitor.

[0068] Example 7

[0069] 6.5mmol of L-arginine and 6.5mmol of phenyl isothiocyanate were added to a 250mL round-bottom flask, and then 85mL of ethanol and 12mL of distilled water were added to the flask and placed in an oil bath at 65°C for 5.5h. The reaction was monitored by thin layer chromatography and then cooled at 8°C / min. The obtained solid was filtered and washed with ethyl acetate. Subsequently, the obtained solid was collected after vacuum freeze drying at 50°C for 66h to obtain an arginine organic corrosion inhibitor. Finally, the collected arginine organic corrosion inhibitor was added to a saturated NTO solution, and the mass loss of carbon steel immersed in this solution was taken to calculate the corrosion rate to verify the effect of this arginine organic corrosion inhibitor.

[0070] Example 8

[0071] 8mmol of L-arginine and 8mmol of phenyl isothiocyanate were added to a 250mL round-bottom flask, and then 100mL of ethanol and 15mL of distilled water were added to the flask and placed in an oil bath and stirred at 70°C for 6h. The reaction was monitored by thin layer chromatography and cooled at 10°C / min. The obtained solid was filtered and washed with double distilled water. Subsequently, the obtained solid was vacuum freeze-dried at 50°C for 72h and then collected to obtain an arginine organic corrosion inhibitor. Finally, the collected arginine organic corrosion inhibitor was added to a saturated NTO solution, and the mass loss of carbon steel immersed in this solution was taken to calculate the corrosion rate to verify the effect of this arginine organic corrosion inhibitor.

[0072] Comparative Example 2

[0073] The corrosion rate of carbon steel was tested by immersing it directly in a saturated NTO solution without adding N2-[(phenylamino)sulfoxymethyl]-arginine corrosion inhibitor.

[0074] Table 2. Corrosion inhibition performance of N2-[(phenylamino)sulfoxymethyl]-arginine inhibitor on NTO

[0075]

[0076]

[0077] from Fig.12It can be seen that the corrosion of low carbon steel by NTO saturated solution after adding N2-[(phenylamino) thioxomethyl]-arginine corrosion inhibitor was significantly inhibited, and its corrosion rate was 6.13mm / y. This is due to the presence of thioxomethyl functional groups in N2-[(phenylamino) thioxomethyl]-arginine molecules, which can chemically adsorb with the metal surface to form a dense protective film. At the same time, the arginine group in the arginine molecule may form coordination bonds or hydrogen bonds with the metal surface, enhancing the adhesion of the film, thereby forming a stable and indestructible protective layer. This film can block the entry of corrosive media such as NTO and water molecules, slowing down the corrosion reaction. In addition, N2-[(phenylamino) thioxomethyl]-arginine can also synergistically adsorb with NTO molecules on the carbon steel surface, strengthening the adsorption capacity of the body on the carbon steel surface while weakening the adsorption and dissociation of NTO molecules on the carbon steel surface, further hindering the corrosion caused by the reaction of NTO molecules on the carbon steel surface.

[0078] In addition, the N-[(phenylamino)sulfurylmethyl]tryptophan corrosion inhibitor and N2-[(phenylamino)sulfurylmethyl]-arginine corrosion inhibitor prepared by the present invention can effectively inhibit the corrosion of NTO without reducing its energy level, and the preparation method is simple, easy to operate, and has low production cost. It meets the requirements for long-term storage of NTO-based weapons and equipment and has high industrial application value.

[0079] The specific description above further illustrates the purpose, technical solutions and beneficial effects of the invention in detail. It should be understood that the above is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. An amino acid metal surface corrosion inhibitor material, characterized in that: The amino acid corrosion inhibitor material is obtained by adding a certain amount of L-tryptophan and phenyl isothiocyanate into a reaction container, adding a solvent, and stirring the reaction at a certain reaction temperature. The specific structure of the amino acid corrosion inhibitor material is as follows:

2. The amino acid metal surface corrosion inhibitor material according to claim 1, characterized in that: The step of adding a certain amount of L-tryptophan and phenyl isothiocyanate into a reaction container, adding a solvent, and stirring the reaction at a certain reaction temperature specifically includes: The amount of L-tryptophan is 1-5 mmol, the amount of phenyl isothiocyanate is 1-5 mmol; the solvent is 50-100 mL of tetrahydrofuran; the reaction temperature is 80-90° C., and the stirring time is 7-9 h.

3. The amino acid metal surface corrosion inhibitor material according to claim 2, characterized in that: The step of adding a certain amount of L-tryptophan and phenyl isothiocyanate into a reaction container, adding a solvent, and stirring the reaction at a certain reaction temperature specifically includes: The amount of L-tryptophan is 4.9 mmol, the amount of phenyl isothiocyanate is 4.9 mmol; the solvent is 85 mL of tetrahydrofuran; the reaction temperature is 85° C., and the stirring time is 8 h.

4. An amino acid-based metal surface corrosion inhibitor material, characterized in that: The amino acid corrosion inhibitor material is obtained by adding a certain amount of L-arginine and phenyl isothiocyanate into a reaction container, adding a solvent, and stirring the reaction at a certain reaction temperature. The specific structure of the amino acid corrosion inhibitor material is as follows:

5. The amino acid metal surface corrosion inhibitor material according to claim 4, characterized in that: The step of adding a certain amount of L-arginine and phenyl isothiocyanate into a reaction container, adding a solvent, and stirring the reaction at a certain reaction temperature specifically includes: The amount of L-arginine is 5.5-8 mmol, the amount of phenyl isothiocyanate is 5.5-8 mmol; the solvent is 50-100 mL ethanol and 5-15 mL double distilled water; the reaction temperature is 50-70° C., and the stirring time is 4-6 h.

6. The amino acid metal surface corrosion inhibitor material according to claim 5, characterized in that: The step of adding a certain amount of L-arginine and phenyl isothiocyanate into a reaction container, adding a solvent, and stirring the reaction at a certain reaction temperature specifically includes: The amount of L-tryptophan is 5.74 mmol, and the amount of phenyl isothiocyanate is 5.74 mmol; the solvent is 75 mL of ethanol and 10 mL of double distilled water; the reaction temperature is 60° C., and the stirring time is 5 h.

7. An application of the amino acid metal surface corrosion inhibitor material according to any one of claims 1 to 6 in the field of metal corrosion prevention and control technology.

8. The use according to claim 7, characterized in that: The amino acid metal surface corrosion inhibitor material forms a protective film on the metal surface, thereby blocking direct contact between NTO or other corrosive media and the metal surface, thereby achieving corrosion inhibition of the metal material.

9. A method for verifying the effect of an amino acid-based metal surface corrosion inhibitor material, used for verifying the corrosion inhibition effect of the amino acid-based metal surface corrosion inhibitor material according to any one of claims 1 to 6, characterized in that: The specific steps include: S1: adding the amino acid metal surface corrosion inhibitor material to the NTO saturated solution; S2: taking carbon steel and immersing it in the NTO saturated solution to which the amino acid metal surface corrosion inhibitor material is added as described in S1, and calculating the corrosion rate of the carbon steel; S3: Setting a comparative example, and performing parameter comparison between the corrosion rate calculated in S2 and the comparative example to verify the corrosion inhibition effect of the amino acid-based metal surface corrosion inhibitor material.

10. The method for verifying the effect of the amino acid-based metal surface corrosion inhibitor material according to claim 9, characterized in that: The S3 specifically includes: The comparative example is set to directly immerse carbon steel in a saturated NTO solution without adding the amino acid-based metal surface corrosion inhibitor material, and test the corrosion rate.

Citation Information

Patent Citations

  • Synthesis method of bis(caproylaminomethyl)-thiourea

    CN104151221A