Safe-to-operate method for receiving casting residues and returning casting residues to production by using heavy ladle
By adopting the heavy-packed iron-packing method in steel metallurgy, the cast residue is decomposed and the pouring order is controlled, the problems of overflow and splashing in the production of cast residue are solved, and efficient utilization and safe production of cast residue are achieved. .
Patent Information
- Application Number
- CN202310664818.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-06
- Publication Date
- 2024-12-06
AI Technical Summary
During the process of steel metallurgy, the cast residue is highly oxidized during production, and it is easy to condense and react in the molten iron bag, resulting in overflow or splash accidents, limiting the efficient use of cast residue.
Using the heavy-pack molten iron bag method, the cast residue in the ladle is first decomposed into two parts and poured out, namely the narrow cast residue and molten steel. By controlling the pouring amount and pouring order, the contact between the oxidizing components and the molten iron is reduced. , reduce CO generation and reaction intensity, avoid spills and splashes.
It has achieved the reduction of spillage and splash accidents in the production of all types of casting residues, improved the rebate productivity and resource utilization efficiency of casting residues, and has significant economic and environmental benefits.
Smart Images

Figure HDA0004270546220000011 
Figure HDA0004270546220000012
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel smelting, and in particular to a method for safely operating a heavy-duty iron ladle to receive casting slag for return to production. Background Art
[0002] In the steel metallurgical process, in order to ensure the quality of the ingot, the ladle of a 250t converter steelmaking continuous casting unit will usually have 3-5 tons of refined molten steel remaining in the ladle. In addition, there will be 3-5 tons of casting slag remaining in the ladle. The molten steel and slag remaining in the ladle are collectively referred to as casting slag.
[0003] The traditional casting slag treatment process is: pour the casting slag in the ladle into a slag basin with a grid, and transport the slag basin filled with casting slag to a special slag treatment company for unloading. After cooling, the slag lumps separated by the grid are crushed with a drop hammer, followed by iron resource recovery and comprehensive utilization of the slag.
[0004] The mainstream technical direction for the development and utilization of casting slag resources is to directly return hot casting slag to production within the steelmaking unit. Various steel companies have carried out research, development and application along different paths.
[0005] One of the ways to return the casting slag to production is to pour the casting slag in the casting ladle into the molten iron ladle, and then return it to the converter process through the molten iron ladle for treatment. Since a bag of casting slag is usually small in volume, in the practice of returning to production, multiple bags of casting slag are poured into one molten iron ladle and then returned. However, in the return of multiple bags of casting slag, the time interval between bags is about half an hour. The casting slag poured in early is easy to condense in the molten iron ladle, and the casting slag poured in later is not enough to melt it, which causes serious accidents of slagging in the molten iron ladle. Therefore, when multiple bags of casting slag are returned to production, it is usually necessary to pre-load a part of molten iron in the molten iron ladle to form a heavy-bag molten iron ladle.
[0006] In the practice of the casting slag recycling process of pouring multiple bags of casting slag into the heavy bag iron ladle, there is a problem of slag overflow and even splashing in the iron ladle when all the casting slag is poured into the heavy bag iron ladle at once. This is because the hot molten slag in the casting slag has been smelted and / or refined in a converter, so it has a high oxidizing property. After it is injected into the iron ladle, the molten iron is reducing and contains many reducing elements, such as [Si], [Mn], [C], etc., among which [C] has the highest content, which can reach 4 to 4.5%. Therefore, the oxidizing casting slag will react with the [C] in the molten iron to generate CO. When the casting slag is injected into the iron ladle in a short time, the volume of the slag-iron mixture in the iron ladle will expand rapidly due to the generation of a large amount of CO, rushing out of the iron ladle to cause slag overflow, and when the reaction is more intense, splashing will be formed.
[0007] In view of the existence of this problem, the method currently usually adopted is to roughly classify the steel types smelted in the converter. When producing ultra-low carbon automobile sheet steel, the slag is not suitable for return due to its high oxidizability, so the slag is treated by the traditional grid method. Only when producing steel types such as silicon steel, the slag is not highly oxidizable and will not overflow when added to the ladle, and then it is poured into the ladle for return. Although this eliminates the danger of production accidents such as overflow, it cannot achieve a high slag return productivity, and loses a considerable part of the benefits of hot slag return production. Summary of the invention
[0008] The purpose of the present invention is to provide a method for safely operating the heavy-clad iron ladle to receive the casting slag for return to production, so as to solve the problem of slag overflow or splashing caused by the heavy-clad iron ladle to receive the casting slag, and the method is suitable for the utilization of all types of casting slag return production, so as to promote the implementation of the casting slag return production process, and has significant economic and environmental benefits.
[0009] To achieve the above object, the technical solution of the present invention is:
[0010] A safe method for using a heavy-duty iron ladle to receive casting slag for production, comprising the following steps:
[0011] 1) After the molten iron is filled into the ladle for use, the amount of molten iron filled accounts for 10-15% of the molten iron volume. The ladle filled with molten iron is called a heavy ladle;
[0012] 2) After the molten steel is poured, the ladle is hoisted above the casting slag storage device, and the ladle is tilted. When the horizontal spreading surface of the melt in the ladle extends to the edge of the inner wall of the ladle, the tilting is stopped, and the ladle is kept still for 5 to 20 seconds. Then, the ladle is tilted again to make the upper layer of the casting slag in the ladle flow out, and the following control is made: 1 / 6 of the total weight of the casting slag ≤ the weight of the flowing casting slag < 1 / 2 of the total weight of the casting slag; then, the remaining casting slag in the ladle is poured into the heavy-package iron ladle; and the above operation is repeated until the heavy-package iron ladle completes the receiving of the casting slag;
[0013] 3) Return the heavy ladle that receives the casting slag to production.
[0014] Preferably, the temperature of the casting slag in the ladle is ≥1420°C.
[0015] Preferably, the viscosity of the casting slag in the ladle is ≤0.7 Pa·s.
[0016] Preferably, the ladle is equipped with a weight detection device.
[0017] Preferably, during the operation of step 2), the ladle is covered with a notch-shaped ladle cover.
[0018] Preferably, the notch height of the notch-shaped ladle cover satisfies the following condition: 1 / 10 of the ladle radius < notch height ≤ 1 / 4 of the ladle radius.
[0019] Preferably, the casting slag storage device is a basin, a tray or a tank.
[0020] In the method of the present invention:
[0021] After the molten steel is poured, the remaining molten steel and slag in the ladle are collectively called casting slag, of which the molten steel and slag each account for about half of the weight, but the density of the molten steel and slag is quite different, the density of the molten steel is significantly greater than the density of the slag, so the molten steel in the ladle is always below the slag. We call the sum of the molten steel and slag in the ladle the broad casting slag, and the slag in the ladle that does not include the molten steel part is called the narrow casting slag.
[0022] Therefore, the present invention decomposes pouring out the casting slag in the ladle into two steps:
[0023] The first step is to hoist the ladle above the casting slag storage device (basin, plate or tank), slowly tilt the ladle, and pour 1 / 6 to 1 / 2 of the total weight of the casting slag into the casting slag storage device. After pouring, most of the molten steel and a small amount of slag are still retained in the ladle. The trick to this step is: since the density of narrow casting slag is about 1 / 3 of the density of molten steel, the weight of the narrow casting slag in the ladle is basically the same as the weight of the molten steel at the beginning, so the volume of the narrow casting slag is 3 times the volume of the molten steel, so the thickness of the narrow casting slag in the ladle will be 3 times the thickness of the molten steel. In this way, the distribution of molten steel and narrow casting slag in the ladle will be that the molten steel with a relative height of 1 is piled with thick narrow casting slag with a relative height of 3. Since the narrow casting slag in the ladle is always lighter than the molten steel, when the ladle is slowly tipped, the thick narrow casting slag will flow out of the ladle before the molten steel. After (1 / 6 to 1 / 2) of the total weight of the broad casting slag flows out, most of the narrow casting slag will flow out of the ladle. For example, when the outflow of casting slag is 1 / 3 of the total weight of the initial broad casting slag, about 2 / 3 of the original narrow casting slag volume has all flowed out, and the remaining broad casting slag in the ladle is most of the molten steel and a small part of the narrow casting slag.
[0024] In the second step, all the remaining broad casting slag in the ladle is poured into the heavy ladle iron ladle. Since the total amount of oxidizing narrow casting slag poured into the heavy ladle iron ladle is reduced, the amount of substances that react with the oxidizing components in the remaining narrow casting slag and the reducing components in the molten iron is greatly reduced, and the impact momentum and impact time on the molten iron in the ladle are also greatly reduced. Therefore, the reaction intensity of the carbon-oxygen reaction is greatly reduced, and the amount of CO generated by the reaction is greatly reduced. The degree of rise in the slag liquid level in the heavy ladle iron ladle caused by the expansion and overflow of CO is weakened, and the slag liquid level in the heavy ladle iron ladle is only slightly increased.
[0025] During operation, the ladle is covered with a round ladle cover to avoid heat loss, keep the molten steel and narrow casting slag in the ladle in a high-temperature molten state, ensure that the casting slag temperature is greater than 1420°C, has sufficient fluidity, and the viscosity is no more than 0.7 Pa·s.
[0026] A weight detection device is installed on the ladle to record the initial weight of the casting slag each time it comes off the line and the weight of the casting slag stored in the ladle during the dumping process. When the amount of casting slag dumped reaches the set value, the slag dumping operation is ended.
[0027] The differences and improvements of the present invention over the prior art are as follows:
[0028] Chinese patent CN202111249196.4 discloses "a method for pouring excess steel into a tank", which mainly solves the technical problem of slag overflow and even splashing during the pouring process of excess steel into a tank. The technical solution includes: 1) turning over the bottom molten iron; 2) transporting the ladle containing the bottom molten iron to the ladle slag turning area under the ladle turntable of the continuous casting machine; 3) pouring out the excess steel in the ladle; 4) deoxidizing the slag in the ladle; 5) pouring the molten iron into a tank; 6) desulfurizing the molten iron; 7) adding metal materials to the converter; 8) blowing in the converter; 9) tapping the converter. This patent requires pouring 40-60% of the total mass of molten steel and hot slag into the ladle containing molten iron as a bottom layer. That is, pouring about half of the broad-sense casting slag into the ladle. Directly dumping the broad-sense casting slag only reduces the amount of dumping, but does not change the ratio of the narrow-sense casting slag to molten steel poured into the ladle. Moreover, this method cannot realize the return of molten steel to production as much as possible.
[0029] Chinese patent CN202110407673.9 discloses "a method for recycling ladle casting residues suitable for super low carbon steel", using a ladle filled with molten iron to repeatedly recover ladle casting residues, adding deoxidizer to the surface of molten iron before recovering ladle casting residues, using slag pressing insulation materials to press slag after each recovery of ladle casting residues, adding deoxidizer to the surface of molten iron after the last recovery, and then adding the recovered casting residues and molten iron in the ladle to the converter, so that the recovery efficiency is high, and the technical solution of the present invention can control the amount of molten iron in the ladle + the amount of molten steel in the recovered ladle casting residues to meet the subsequent converter furnace tapping requirements, and no special expensive equipment is required. After adding to the converter, the converter blowing process is stable, and no splashing, slag overflow, etc. occur. The patent mainly achieves the purpose of the invention by adding an external deoxidizer, and the present invention does not need to add anything extra, and only needs to control the operation in the return process to achieve it.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] 1. The present invention first pours most of the narrow slag in the ladle into the casting slag storage device, and then injects the remaining broad casting slag in the ladle into the heavy ladle iron ladle. Since the remaining broad casting slag in the ladle only includes most of the molten steel and a small part of the narrow casting slag, the amount of narrow casting slag entering the iron ladle is reduced, and the slag overflow or splashing caused by the generation of gases such as CO during the reaction between the narrow casting slag and the molten iron is greatly reduced. The method of the present invention is applicable to the utilization of all types of casting slag recycling production, and promotes the implementation of the casting slag recycling production process.
[0032] 2. By adopting the method of the present invention, the most valuable molten steel in the casting slag can be returned to the steel metallurgical process, while most of the casting slag without iron can be discharged from the steel metallurgical system, which has significant economic and environmental benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 A schematic diagram of a device for pouring the casting slag in a ladle into a casting slag storage device according to an embodiment of the present invention;
[0034] Figure 2 It is a schematic diagram of a device for injecting the remaining casting slag in the steel ladle into the heavy ladle iron ladle according to the embodiment of the present invention. DETAILED DESCRIPTION
[0035] The present invention will be further described below in conjunction with specific embodiments:
[0036] Example 1
[0037] See also Figure 1 , Figure 2 The present invention discloses a safe method for using a heavy-duty iron ladle to receive casting slag for production, which comprises the following steps:
[0038] 1) After the molten iron is filled into the ladle for use, the amount of molten iron filled accounts for 10% of the molten iron volume. The ladle filled with molten iron is called a heavy ladle 2;
[0039] 2) After the molten steel is poured, the ladle 100 is hoisted above the casting slag storage device 1, and the ladle is tilted. When the horizontal spreading surface of the melt in the ladle 100 extends to the edge of the inner wall of the ladle, the tilting is stopped, and the ladle is kept stationary for 10 seconds, and then the ladle 100 is tilted again to make the upper layer of the casting slag in the ladle 100 flow out, and the weight of the outflowing casting slag is controlled to be 1 / 3 of the total weight of the casting slag, and then the remaining casting slag in the ladle 100 is poured into the heavy-clad iron ladle 2; repeat the above operation until the heavy-clad iron ladle 2 takes over the casting slag;
[0040] 3) Return the heavy iron ladle 2 after receiving the casting slag to production and utilization.
[0041] Example 2
[0042] A safe method for using a heavy-duty iron ladle to receive casting slag for production, comprising the following steps:
[0043] 1) After the molten iron is loaded into the molten iron ladle 3 for standby use, the amount of molten iron loaded accounts for 15% of the molten iron ladle capacity, and the molten iron ladle filled with molten iron is called a heavy ladle;
[0044] 2) After the molten steel is poured, the ladle 100 is hoisted above the casting slag storage device 1, and the ladle is tilted. When the horizontal spreading surface of the melt in the ladle 100 extends to the edge of the inner wall of the ladle, the tilting is stopped, and the ladle is kept stationary for 8 seconds, and then the ladle 100 is tilted again to make the upper layer of the casting slag in the ladle 100 flow out, and the weight of the flowing casting slag is controlled to be 2 / 5 of the total weight of the casting slag, and then the remaining casting slag in the ladle 100 is poured into the heavy-clad iron ladle 2; repeat the above operation until the heavy-clad iron ladle 2 completes the receiving of the casting slag; during the operation, the ladle is covered with a round-shaped ladle cover;
[0045] 3) Return the heavy iron ladle 2 after receiving the casting slag to production and utilization.
[0046] Example 3
[0047] A safe method for using a heavy-duty iron ladle to receive casting slag for production, comprising the following steps:
[0048] 1) After the molten iron is loaded into the molten iron ladle 3 for standby use, the amount of molten iron loaded accounts for 12% of the molten iron ladle capacity, and the molten iron ladle filled with molten iron is called a heavy ladle;
[0049] 2) After the molten steel is poured, the ladle 100 is hoisted above the casting slag storage device 1, and the ladle is tilted. When the horizontal spreading surface of the melt in the ladle 100 extends to the edge of the inner wall of the ladle, the tilting is stopped, and the ladle is kept stationary for 15 seconds. Then, the ladle 100 is tilted again to make the upper layer of the casting slag in the ladle 100 flow out, and the weight of the flowing casting slag is controlled to be 9 / 20 of the total weight of the casting slag. Then, the remaining casting slag in the ladle 100 is poured into the heavy-clad iron ladle 2; the above operation is repeated until the heavy-clad iron ladle 2 completes the receiving of the casting slag; during the operation, a round-shaped ladle cover is added to the ladle;
[0050] 3) Return the heavy iron ladle 2 after receiving the casting slag to production and utilization.
Claims
1. A safe method for using a heavy ladle to receive casting slag for production, characterized in that: The steps include: 1) After the molten iron is filled into the ladle for use, the amount of molten iron filled accounts for 10-15% of the molten iron volume. The ladle filled with molten iron is called a heavy ladle; 2) After the molten steel is poured, the ladle is hoisted above the casting slag storage device, and the ladle is tilted. When the horizontal spreading surface of the melt in the ladle extends to the edge of the inner wall of the ladle, the tilting is stopped, and the ladle is kept still for 5 to 20 seconds. Then, the ladle is tilted again to make the upper layer of the casting slag in the ladle flow out, and the following control is made: 1 / 6 of the total weight of the casting slag ≤ the weight of the flowing casting slag < 1 / 2 of the total weight of the casting slag; then, the remaining casting slag in the ladle is poured into the heavy-package iron ladle; and the above operation is repeated until the heavy-package iron ladle completes the receiving of the casting slag; 3) Return the heavy ladle that receives the casting slag to production.
2. The method according to claim 1, characterized in that: The temperature of the casting slag in the ladle is ≥1420°C.
3. The method according to claim 1 or 2, characterized in that: The viscosity of the casting slag in the ladle is ≤0.7 Pa·s.
4. The method according to claim 1, characterized in that: The ladle is equipped with a weight detection device.
5. The method according to claim 1 or 4, characterized in that: During the operation of step 2), the ladle is covered with a circular ladle cover.
6. The method according to claim 5, characterized in that: The notch height of the notch-shaped ladle cover satisfies the following condition: 1 / 10 of the ladle radius < notch height ≤ 1 / 4 of the ladle radius.
7. The method according to claim 1, characterized in that: The casting slag storage device is a basin, a tray or a tank.